Preparation method of high-transmittance nano coating for photovoltaic glass
Through high-transmittance nanocoating composed of nanotitanium dioxide, carbon-based mesoporous materials and fluorosilicone polyether, the problem of traditional coatings being susceptible to pollution and acid rain erosion in open air environments is solved, and high transmittance and hydrophobic properties are achieved , suitable for anti-fouling and ultraviolet ray applications on a variety of substrate surfaces, and meets environmental protection requirements.
Patent Information
- Application Number
- CN202411142415.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-26
AI Technical Summary
Traditional physical compartments and chemical coatings are susceptible to pollution and acid rain erosion in open air environments, resulting in reduced performance of devices such as photovoltaic glass, and complex preparation process and potential risks to the environment.
Using a high-transmittance nanocoating composed of nanotitanium dioxide, carbon-based mesoporous materials and fluorosilicone polyether, nanocoating is formed through ultrasonic dispersion, stirring and thermal drying, combining silane coupling agent and modifier to improve adhesiveness. Adhesion and hydrophobic properties.
It achieves high transmittance, good hydrophobic properties and mechanical strength, reduces the risks of pollution and corrosion, is suitable for anti-fouling, dust-proof and UV-resistant applications on a variety of substrate surfaces, and meets environmental protection requirements.
Smart Images

Figure CN119019899A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of nano coating materials, and in particular relates to a method for preparing a high-transmittance nano coating that can be used for photovoltaic glass. Background Art
[0002] Modern society is developing rapidly, and traditional physical barriers can no longer meet the requirements of modern industry. Photovoltaic glass, outdoor display cabinets, outdoor display equipment and other devices are in open air environments and are easily affected by harsh environments, such as being covered by sand, dust and sludge and eroded by acid rain, which will not only damage the appearance of the device, but also cause expensive repair costs. Even if it is not eroded by acid rain, it will inevitably come into contact with pollutants. These pollutants will not only be adsorbed on the surface of the coating, but also enter the coating through the pores, reducing the porosity of the coating, thereby hindering the transmission of light. In severe cases, it will contact with the substrate and corrode it, reducing the performance of the equipment.
[0003] There are two measures currently in place. The first is to physically cover the display devices in an open-air environment when wind and rain come, but this method is inefficient and requires a large number of partitions, which takes up space. The second is to apply chemical coatings on the surface of the device, but some of the current chemical coatings have potential risks to the human body and the environment, and the preparation process is complicated, which invisibly increases the cost again. Summary of the invention
[0004] In view of this, an object of the present invention is to provide a method for preparing a high-transmittance nano-coating that can be used for photovoltaic glass to solve the above-mentioned problems.
[0005] To achieve the above object, the present invention provides the following technical solution: a method for preparing a high-transmittance nano-coating that can be used for photovoltaic glass, comprising the following steps:
[0006] S1, adding nano titanium dioxide, carbon-based mesoporous material, and dispersant into an organic solvent, and forming a particle dispersion by ultrasonic dispersion;
[0007] S2, mixing a film-forming substance composed of acrylic resin, silicone resin and polyurethane with an adhesive solvent, and then stirring evenly to obtain a prepolymer solution;
[0008] S3, adding fluorinated silicone polyether, siloxane compound and additive to the microparticle dispersion, adding a catalyst under stirring to continue the reaction, and obtaining a mixed solution A;
[0009] S4, adding the mixed solution A to the prepolymer solution, and then adding a cross-linking agent and a modifier and stirring to obtain a mixed solution B, wherein the cross-linking agent is a silane coupling agent;
[0010] S5, uniformly coating the mixed solution B on the surface of the substrate, and thermally drying and curing at a low temperature, so that the mixed solution B fully reacts and solidifies into a film;
[0011] S6. After the film is completely cured, rinse the substrate surface with deionized water to remove unreacted residues, and finally dry naturally to form a nano coating.
[0012] Furthermore, in parts by weight, the nano titanium dioxide is 17-24 parts, the carbon-based mesoporous material is 10-18 parts, the dispersant is 3-8 parts, the organic solvent is 45-55 parts, the film-forming substance is 10-14 parts, and the adhesive solvent is 2-6 parts; the fluorine-containing silicone polyether is 0.12-1.2 parts, the siloxane compound is 0.52-2.5 parts; the additive is 5-12 parts; the catalyst is 3-5 parts; the silane coupling agent is 8-13 parts, the cross-linking agent is 4-7 parts; and the modifier is 1-1.5 parts.
[0013] Furthermore, in the step S1, the ultrasonic dispersion rate is first stirred at 90 rpm / min for 5 minutes; then increased to 150 rpm / min for 8 minutes, and then reduced to 60 rpm / min for 3 minutes; in the step S2, when the film-forming material and the adhesive solvent are mixed, stirred at 120 rpm / min for 30 minutes; in the step S3, the stirring rate is 180 rpm / min for 20 minutes.
[0014] Furthermore, the carbon-based mesoporous material is any one or more combinations of carbon fiber, silicon carbide fiber, carbon black, carbon nanotube, and graphene; the dispersant is composed of polyvinyl alcohol, a colloid protective agent, dimethyl sulfoxide, sodium dodecylbenzene sulfonate, and ethanol; and the organic solvent is composed of a mixture of styrene, perchloroethylene, trichloroethylene, and ethylene glycol ether.
[0015] Furthermore, the adhesive solvent is composed of a mixture of chloroform, methyl methacrylate, vinyl acetate, N-methylpyrrolidone, ethyl acetate and butanol.
[0016] Furthermore, the siloxane compound is composed of heptadecafluorodecyltrimethoxysilane, hydroxypolydimethylsiloxane and triethoxysilane; and the catalyst is one of acetic acid and ammonia water.
[0017] Furthermore, the additive is composed of a mixture of a drying agent, a heat stabilizer, an antioxidant, a flame retardant and a light stabilizer.
[0018] Furthermore, the modifier is heptadecafluorodecyltriethoxysilane, and the silane coupling agent is composed of trimethoxysilane and triethoxysilane.
[0019] Furthermore, the step S4 is specifically as follows: firstly, solution A is slowly added to the prepolymer solution and stirred evenly, and then refluxed for 5-6 hours; then, a crosslinking agent and a modifier are added, and then cooled to room temperature, and then dried and washed to obtain a mixed solution B.
[0020] The beneficial effects of the present invention are:
[0021] 1. The nano titanium dioxide used in the present invention has a small particle size, a large specific surface area, a strong surface adsorption force and a high chemical purity. It also has high chemical stability, thermal stability, super hydrophilicity, and non-migration. It can sterilize for a long time under the action of ultraviolet rays in the light. Nano titanium dioxide can absorb ultraviolet rays, reflect and scatter ultraviolet rays, and can also transmit visible light. It is a protective agent with superior performance and great development prospects. The nano coating of the present application has a high transmittance, and the application of nano titanium dioxide can play an anti-ultraviolet effect. In addition, nano titanium dioxide can also be used to improve the self-cleaning ability and anti-pollution performance of the coating. As the main material for constructing the nanostructure, a rough surface is provided to achieve the effect of improving the self-cleaning ability and anti-pollution performance of the coating. Carbon-based mesoporous molecular sieves have the characteristics of high specific surface area, high pore volume and high adsorption performance, and can effectively adsorb tiny particles including dust. It can be used to prepare nano coatings for effective self-cleaning effects, and can also selectively adsorb gases and purify the environment when attached to the surface of the substrate.
[0022] 2. The fluorosilane compound used in the present invention can form a stable silicon-oxygen bond, enhance the adhesion and mechanical strength of the coating, and act as a hydrophobic modifier to reduce the surface energy of the nanofilm. The organic solvent used can dissolve and disperse the medium of other raw materials, making the solution more uniform, and can be used to disperse nanoparticles and dissolve fluorosilane. The catalyst used can promote the hydrolysis and condensation reactions of fluorosilane, catalyze the reaction, and improve production efficiency. The deionized water used is used to adjust the reaction system and improve the uniformity and stability of the coating. The film-forming material used can provide the necessary mechanical properties and weather resistance as the matrix of the nanocoating. The dispersant used can be used to improve the dispersibility of nanoparticles in the solvent. And the modifier used is used to further reduce the surface properties of the nanocoating and improve the hydrophobicity. The silane coupling agent has a hydrolyzable Si-OCH3 bond and an active Si-H bond. After reacting with a variety of raw materials, it can improve the performance of the material, increase the bonding strength, and obtain a composite material with excellent performance and reliability.
[0023] 3. The preparation method of the present invention can effectively disperse and mix the raw materials evenly through multiple dispersions and ultrasound. Each raw material is prepared through different preparation steps, which can effectively stimulate the performance of the raw materials and enable each raw material to exert the maximum efficiency in the subsequent finished product. The preparation method of the present invention is simple, and the time consumption is significantly shortened compared with the prior art, and can be effectively applied to industrial applications.
[0024] 4. The high transmittance nano coating of the present invention has high transmittance and excellent hydrophobic properties, as well as good mechanical strength and durability. The good adhesion of the formed silicon-oxygen bonds ensures the mechanical strength and durability of the coating. It has a wide range of applications, including but not limited to anti-oxidation, waterproofing, and anti-fouling treatment of metal surfaces, hydrophobic, anti-fouling, and anti-ultraviolet coatings on glass surfaces, waterproofing, anti-fouling, and anti-corrosion treatments on ceramic and stone surfaces, and anti-fouling and weather-resistant coatings for solar cells, and other hydrophobic, anti-fouling, and dust-proof uses on the surfaces of various substrates.
[0025] 5. The high-transmittance nano-coating of the present invention is easily degraded, does not cause environmental accumulation, and meets environmental protection requirements. By making the surface rough by corrosion etching and reducing the surface energy by fluorination treatment, a contact angle greater than 150 degrees can be obtained, thereby becoming a super-hydrophobic material.
[0026] 6. After the high transmittance nano coating of the present invention is prepared, performance tests including transmittance, contact angle, rolling angle, etc. are carried out, which verify its high transmittance and high hydrophobicity characteristics.
[0027] Other advantages, objectives and features of the present invention will be described in the following description and will be apparent to those skilled in the art to some extent, or those skilled in the art may be taught from the practice of the present invention. The objectives and other advantages of the present invention may be realized and obtained through the following description. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] In order to make the purpose, technical solution and beneficial effects of the invention clearer, the present invention provides the following drawings for illustration:
[0029] Figure 1 is a process flow chart of the present invention;
[0030] Figure 2 This is a comparison chart of the transmittance of Example 1 of the present invention and ordinary glass;
[0031] Figure 3 This is a schematic diagram of the microscopic results of the nanocoating in Example 1 of the present invention. DETAILED DESCRIPTION
[0032] A method for preparing a high-transmittance nano coating that can be used for photovoltaic glass.
[0033] Example 1
[0034] S1. Add 17 parts of nano-titanium dioxide, 8 parts of carbon-based mesoporous material composed of silicon carbide fiber and carbon black, and 3 parts of dispersant to 45 parts of organic solvent, and stir at 90 rpm / min for 5 min for ultrasonic dispersion, then increase the speed to 150 rpm / min for 8 min, and then reduce the speed to 60 rpm / min for 3 min, until the solution is evenly dispersed to form a microparticle dispersion;
[0035] S2, 10 parts of the film-forming material and 2 parts of the adhesive solvent were mixed, and then stirred at 120 rpm / min for 30 min to uniformly stir the solution to obtain a prepolymer solution;
[0036] S3, adding 0.12 parts of fluorinated silicone polyether, 0.52 parts of siloxane compound and 5 parts of additive to the microparticle dispersion, stirring at 180 rpm / min for 20 min, and adding 3 parts of catalyst under stirring to continue the reaction, to obtain a mixed solution A;
[0037] S4, adding the mixed solution A to the prepolymer solution and stirring evenly, and then reflux for 5 hours; then adding 8 parts of silane coupling agent as a cross-linking agent and 1 part of a modifier and stirring evenly, cooling to room temperature, and then drying and washing to obtain a mixed solution B;
[0038] S5, coating the mixed solution B evenly on the surface of the substrate, and drying and curing it at 25° C. to allow the mixed solution B to fully react and cure into a film;
[0039] S6. After the film is completely cured, rinse the surface with deionized water to remove unreacted residues, and finally dry naturally to form a nano coating with high transmittance.
[0040] Example 2
[0041] S1. Add 24 parts of nano-titanium dioxide, 15 parts of carbon-based mesoporous materials composed of carbon black and graphene, and 8 parts of dispersant to 55 parts of organic solvent, and stir at 90 rpm / min for 5 minutes for ultrasonic dispersion, then increase the speed to 150 rpm / min for 8 minutes, and then reduce the speed to 60 rpm / min for 3 minutes, until the solution is evenly dispersed to form a particle dispersion;
[0042] S2, 14 parts of the film-forming material and 6 parts of the adhesive solvent were mixed, and then stirred at 120 rpm / min for 30 min to uniformly stir the solution to obtain a prepolymer solution;
[0043] S3, adding 1.2 parts of fluorinated silicone polyether, 2.5 parts of siloxane compound and 12 parts of additive to the microparticle dispersion, stirring at 180 rpm / min for 20 min, and adding 3 parts of catalyst under stirring to continue the reaction, to obtain a mixed solution A;
[0044] S4, adding the mixed solution A to the prepolymer solution and stirring evenly, and then reflux for 5 hours; then adding 13 parts of silane coupling agent as a cross-linking agent and 1.5 parts of a modifier and stirring evenly, cooling to room temperature, and then drying and washing to obtain a mixed solution B;
[0045] S5, coating the mixed solution B evenly on the surface of the substrate, and drying and curing it at 25° C. to allow the mixed solution B to fully react and cure into a film;
[0046] S6. After the film is completely cured, rinse the surface with deionized water to remove unreacted residues, and finally dry naturally to form a nano coating with high transmittance.
[0047] Example 3
[0048] S1. Add 18 parts of nano-titanium dioxide, 12 parts of carbon-based mesoporous material composed of silicon carbide fiber and silicon carbide fiber, and 5 parts of dispersant to 55 parts of organic solvent, and stir at 90 rpm / min for 5 minutes for ultrasonic dispersion, then increase the speed to 150 rpm / min for 8 minutes, and then reduce the speed to 60 rpm / min for 3 minutes, until the solution is evenly dispersed to form a microparticle dispersion;
[0049] S2, 10 parts of the film-forming material and 6 parts of the adhesive solvent were mixed, and then stirred at 120 rpm / min for 30 min to uniformly stir the solution to obtain a prepolymer solution;
[0050] S3, adding 0.5 parts of fluorinated silicone polyether, 1 part of siloxane compound and 5 parts of additive to the microparticle dispersion, stirring at 180 rpm / min for 20 min, and adding 3 parts of catalyst under stirring to continue the reaction, to obtain a mixed solution A;
[0051] S4, adding the mixed solution A to the prepolymer solution and stirring evenly, and then reflux for 5 hours; at the same time, adding 10 parts of silane coupling agent as a cross-linking agent and 1 part of a modifier and stirring evenly, cooling to room temperature, and then drying and washing to obtain a mixed solution B;
[0052] S5, coating the mixed solution B evenly on the surface of the substrate, and drying and curing it at 25° C. to allow the mixed solution B to fully react and cure into a film;
[0053] S6. After the film is completely cured, rinse the surface with deionized water to remove unreacted residues, and finally dry naturally to form a nano coating with high transmittance.
[0054] The preparation methods of Examples 1 to 3 are the same, except that the components are different in the protection scope. In order to verify the superiority of the ratio and method of the present invention, based on Example 1, Comparative Examples 1-4 are set here.
[0055] Comparative Example 1
[0056] S1. Add 23 parts of carbon-based mesoporous materials consisting of 10 parts of nano-titanium dioxide, carbon fiber, silicon carbide fiber, and carbon black, and 10 parts of dispersant to 35 parts of organic solvent, and stir at 90 rpm / min for 5 minutes for ultrasonic dispersion, then increase the speed to 150 rpm / min for 8 minutes, and then reduce the speed to 60 rpm / min for 3 minutes, until the solution is evenly dispersed to form a particle dispersion;
[0057] S2, 15 parts of the film-forming material and 1 part of the adhesive solvent were mixed, and then stirred at 120 rpm / min for 30 minutes to uniformly stir the solution to obtain a prepolymer solution;
[0058] S3, adding 3 parts of fluorinated silicone polyether, 3 parts of siloxane compound and 3 parts of additive to the microparticle dispersion, stirring at 180 rpm / min for 20 min, and adding 3 parts of catalyst under stirring to continue the reaction, to obtain a mixed solution A;
[0059] S4, adding the mixed solution A to the prepolymer solution and stirring evenly, and then reflux for 5 hours; at the same time, adding 15 parts of silane coupling agent as a cross-linking agent and 2 parts of a modifier and stirring evenly, cooling to room temperature, and then drying and washing to obtain a mixed solution B;
[0060] S5, coating the mixed solution B evenly on the surface of the substrate, and drying and curing it at 25° C. to allow the mixed solution B to fully react and cure into a film;
[0061] S6. After the film is completely cured, rinse the surface with deionized water to remove unreacted residues, and finally dry naturally to form a coating.
[0062] The difference between Comparative Example 1 and Example 1 is that the raw material range used in Comparative Example 1 is not within the scope of the present application. Since the ratio of each raw material exceeds the protection scope of the present application, the finished product has low film-forming property and insufficient bonding ability during preparation. In addition, due to excessive or insufficient raw materials, the prepared finished coating is thick, the high transmittance is insufficient, and the hydrophobic performance is general, and it cannot be effectively applied to the surface of the product substrate.
[0063] Comparative Example 2
[0064] S1. Add 17 parts of nano-titanium dioxide, 8 parts of carbon-based mesoporous material composed of silicon carbide fiber and carbon black, and 3 parts of dispersant to 45 parts of organic solvent, and stir at 90 rpm / min for 5 min for ultrasonic dispersion, then increase the speed to 150 rpm / min for 8 min, and then reduce the speed to 60 rpm / min for 3 min, until the solution is evenly dispersed to form a microparticle dispersion;
[0065] S2, 10 parts of the film-forming material and 2 parts of the adhesive solvent were mixed, and then stirred at 120 rpm / min for 30 min to uniformly stir the solution to obtain a prepolymer solution;
[0066] S3, adding 8 parts of silane coupling agent as a cross-linking agent and 1 part of a modifier to the prepolymer solution and stirring evenly to obtain a mixed solution B;
[0067] S4, uniformly coating the mixed solution B on the surface of the substrate, and heat drying and curing at 25° C. to allow the mixed solution B to fully react and solidify into a film;
[0068] S5. After the film is completely cured, rinse the surface with deionized water to remove unreacted residues, and finally dry naturally to form a coating.
[0069] The difference between Comparative Example 2 and Example 1 is that no mixed solution A is prepared in Comparative Example 2, and the obtained coating has low mechanical strength, insufficient weather resistance, cannot effectively adhere to the surface of the substrate, and cannot play an effective hydrophobic role.
[0070] Comparative Example 3
[0071] S1, add 3 parts of dispersant to 45 parts of organic solvent, and stir at 90 rpm / min for 5 minutes for ultrasonic dispersion, then increase the speed to 150 rpm / min for 8 minutes, and then reduce the speed to 60 rpm / min for 3 minutes, until the solution is evenly dispersed to form a microparticle dispersion;
[0072] S2, adding 0.12 parts of fluorinated silicone polyether, 0.52 parts of siloxane compound and 5 parts of additive to the microparticle dispersion, stirring at 180 rpm / min for 20 min, and adding 3 parts of catalyst under stirring to continue the reaction, to obtain a mixed solution A;
[0073] S3, mixing the mixed solution A with 8 parts of silane coupling agent as a cross-linking agent and 1 part of a modifier to obtain a mixed solution B;
[0074] S4, uniformly coating the mixed solution B on the surface of the substrate, and heat drying and curing at 25° C. to allow the mixed solution B to fully react and solidify into a film;
[0075] S5. After the film is completely cured, rinse the surface with deionized water to remove unreacted residues, and finally dry naturally to form a coating.
[0076] The difference between Comparative Example 3 and Example 1 is that in Comparative Example 3, nano titanium dioxide, carbon-based mesoporous material, and prepolymer solution are not added, and the obtained coating has poor self-cleaning recovery, cannot effectively resist pollution, cannot effectively form a film, and has poor adhesion performance.
[0077] Comparative Example 4
[0078] S1. Add 17 parts of nano titanium dioxide, 8 parts of carbon-based mesoporous material composed of silicon carbide fiber and carbon black, and 3 parts of dispersant to 45 parts of organic solvent, and then add 10 parts of film-forming material and 2 parts of adhesive solvent to mix; continue to add 0.12 parts of fluorinated silicone polyether, 0.52 parts of siloxane compound and 5 parts of additive, and continue to add 8 parts of silane coupling agent after stirring to obtain a mixed solution;
[0079] S2, coating the mixed solution evenly on the surface of the substrate, and drying and curing it at 25°C to allow the mixed solution B to fully react and cure into a film;
[0080] S3. After the film is completely cured, rinse the surface with deionized water to remove unreacted residues, and finally dry it naturally to form a coating.
[0081] The difference between Comparative Example 4 and Example 1 is that all the raw materials are directly mixed without going through the time, rate, temperature and other parameter conditions of the present invention. The resulting nano coating has poor adhesion, insufficient mechanical strength, poor weather resistance, poor transmittance, and almost no self-cleaning performance when attached to the surface of the substrate.
[0082] The nano coatings prepared in Examples 1 to 3 and Comparative Examples 1 to 4 were tested for performance, as shown in Table 1 below:
[0083]
[0084]
[0085] By testing the nanocoatings prepared in various embodiments and comparative examples, it can be found that the nanocoatings prepared in the present invention have high transmittance and can be applied to the surface of a glass substrate without affecting the user's line of sight; at the same time, they have good hydrophobic properties, good anti-fouling properties, and self-cleaning capabilities, providing effective support for modern industries.
[0086] However, the coating that is not prepared using the raw materials, proportions, and methods of the present invention has poor transmittance, which will affect the user's vision and cannot be effectively used in scenes requiring high transmittance. In addition, the coating has poor hydrophobicity, and water stains cannot be effectively evacuated on the coating surface, resulting in serious residue and penetration.
[0087] The nano coatings prepared in Examples 1 to 3 and the coatings prepared in Comparative Examples 1 to 4 were coated on the surface of the substrate, and then the substrate was placed in the same open air environment, exposed to the sun and washed by rain, and tested after 7 days. The results are shown in Table 2 below:
[0088]
[0089]
[0090] It can be found from Table 2 that after the nano coating prepared by the present invention was exposed to sunlight, washed by rain, and placed in an open-air environment for one week, the surface was still flat without warping or cracking, and it was effectively bonded to the substrate without falling off. At the same time, no water stains remained on the surface of the nano coating, and no water stains penetrated the surface of the substrate.
[0091] However, the coatings prepared in Comparative Examples 1 to 4 have different raw materials, proportions, and methods from the nanocoating of the present invention. After being coated on the surface of the substrate, the obtained coatings have greatly reduced performance in all aspects, with obvious dust and poor self-cleaning performance; they also penetrate into the surface of the substrate, have poor hydrophobic performance, poor adhesion, insufficient mechanical strength, and serious breakage; and the surface flatness is poor, and bubbles, particles, etc. appear after being coated on the surface of the substrate.
[0092] In summary, the nano coating obtained by the raw materials, proportions and methods within the scope of protection of the present invention has high transmittance, good hydrophobicity, strong adhesion, certain mechanical strength, and plays a certain protective role on the substrate. However, due to differences in raw materials, proportions and methods, the performance of the coating is insufficient and cannot be effectively applied to modern industry.
[0093] Finally, it should be noted that the above preferred embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail through the above preferred embodiments, those skilled in the art should understand that various changes can be made in form and details without departing from the scope defined by the claims of the present invention.
Claims
1. A method for preparing a high-transmittance nano-coating that can be used for photovoltaic glass, characterized in that: The following steps are included: S1, adding nano titanium dioxide, carbon-based mesoporous material, and dispersant into an organic solvent, and forming a particle dispersion by ultrasonic dispersion; S2, mixing a film-forming substance composed of acrylic resin, silicone resin and polyurethane with an adhesive solvent, and then stirring evenly to obtain a prepolymer solution; S3, adding fluorinated silicone polyether, siloxane compound and additive to the microparticle dispersion, adding a catalyst under stirring to continue the reaction, and obtaining a mixed solution A; S4, adding the mixed solution A to the prepolymer solution, and then adding a cross-linking agent and a modifier and stirring to obtain a mixed solution B, wherein the cross-linking agent is a silane coupling agent; S5, uniformly coating the mixed solution B on the surface of the substrate, and thermally drying and curing at a low temperature, so that the mixed solution B fully reacts and solidifies into a film; S6. After the film is completely cured, rinse the substrate surface with deionized water to remove unreacted residues, and finally dry naturally to form a nano coating.
2. The method for preparing a high-transmittance nano-coating for photovoltaic glass according to claim 1, characterized in that: In parts by weight, the nano titanium dioxide is 17-24 parts, the carbon-based mesoporous material is 8-15 parts, the dispersant is 3-8 parts, the organic solvent is 45-55 parts, the film-forming substance is 10-14 parts, the adhesive solvent is 2-6 parts; the fluorine-containing silicone polyether is 0.12-1.2 parts, the siloxane compound is 0.52-2.5 parts; the additive is 5-12 parts; the catalyst is 3-5 parts; the silane coupling agent is 8-13 parts, the cross-linking agent is 4-7 parts; and the modifier is 1-1.5 parts.
3. The method for preparing a high-transmittance nano-coating for photovoltaic glass according to claim 1, characterized in that: In the step S1, the ultrasonic dispersion rate is first stirred at 90 rpm / min for 5 minutes; then increased to 150 rpm / min for 8 minutes, and then reduced to 60 rpm / min for 3 minutes; in the step S2, when the film-forming material and the adhesive solvent are mixed, stirred at 120 rpm / min for 30 minutes; in the step S3, the stirring rate is 180 rpm / min for 20 minutes.
4. The method for preparing a high-transmittance nano-coating for photovoltaic glass according to claim 2, characterized in that: The carbon-based mesoporous material is any one or more combinations of carbon fiber, silicon carbide fiber, carbon black, carbon nanotube, and graphene; the dispersant is composed of polyvinyl alcohol, a colloid protective agent, dimethyl sulfoxide, sodium dodecylbenzene sulfonate, and ethanol; and the organic solvent is a mixture of styrene, perchloroethylene, trichloroethylene, and ethylene glycol ether.
5. The method for preparing a high-transmittance nano-coating for photovoltaic glass according to claim 4, characterized in that: The adhesive solvent is composed of a mixture of chloroform, methyl methacrylate, vinyl acetate, N-methyl pyrrolidone, ethyl acetate and butanol.
6. The method for preparing a high-transmittance nano-coating for photovoltaic glass according to claim 5, characterized in that: The siloxane compound consists of heptadecafluorodecyltrimethoxysilane, hydroxypolydimethylsiloxane and triethoxysilane; and the catalyst is acetic acid or ammonia water.
7. The method for preparing a high-transmittance nano-coating for photovoltaic glass according to claim 6, characterized in that: The additive is composed of a mixture of a drying agent, a heat stabilizer, an antioxidant, a flame retardant and a light stabilizer.
8. The method for preparing a high-transmittance nano-coating for photovoltaic glass according to claim 7, characterized in that: The modifying agent is heptadecafluorodecyltriethoxysilane, and the silane coupling agent is composed of trimethoxysilane and triethoxysilane.
9. The method for preparing a high-transmittance nano-coating for photovoltaic glass according to claim 1, characterized in that: The step S4 is specifically as follows: firstly, adding solution A into the prepolymer solution and stirring for 2 hours, and then refluxing for 5-6 hours; then adding a crosslinking agent and a modifier, cooling to room temperature, and then drying and washing to obtain a mixed solution B.
Citation Information
Patent Citations
High-transmissivity hydrophobic and dustproof nanometer coating composition, preparation method and applications thereof
CN108300303A
Transparent super-hydrophobic coating and preparation method thereof
CN112300648A
Photovoltaic glass self-cleaning dustproof anti-reflection nanometer material and preparation method thereof
CN116891645A
Conductive and superhydrophobic coatings, and its fabrication method
KR1020090044220A