Photochromic coating liquid and preparation method thereof

By adding polyurethane and organosiloxane to the photochromic coating liquid and cross-linking modification during high-temperature curing, the problems of insufficient color depth, fading rate and adhesion of existing photochromic coatings are solved. It achieves the effects of dark color change, fast fading, strong adhesion and excellent mechanical properties, and is suitable for industrial applications of photochromic lenses.

CN119019925AActive Publication Date: 2024-11-26JIANGSU KELUOMING NEW MATERIAL TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411172326.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-26
Estimated Expiration
2044-08-26

AI Technical Summary

Technical Problem

The existing photochromic coatings have problems such as difficulty in darkening the color depth, slow fading rate, poor adhesion and insufficient mechanical properties.

Method used

Using a photochromic coating liquid composed of photochromic dye, organic prepolymer, isocyanate curing agent, polymethylsiloxane, organic solvent, coupling agent and additive, by adding organic to the main component polyurethane The silicone is cross-linked and modified during high-temperature curing to enhance the discoloration and adhesion of the coating.

Benefits of technology

It significantly improves the discoloration depth and fading rate, and imparts excellent adhesion and mechanical strength to the coating. It is suitable for spin coating, spray coating and dip coating methods, realizing the industrial application of photochromic lenses.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019925A_ABST
    Figure CN119019925A_ABST
Patent Text Reader

Abstract

The invention discloses a photochromic coating liquid and a coating preparation method thereof, and belongs to the technical field of high polymer materials. The photochromic coating liquid comprises the following components: a photochromic dye, polyacrylic polyol, polycarbonate polyol, polyether polyol, an isocyanate curing agent, polymethylsiloxane, an organic solvent, an antioxidant and a light stabilizer. The photochromic dye comprises one or more of spiropyrane, spirooxazine, naphthopyran and fulgide compounds. The polymethylsiloxane is selected from polymethylsiloxane of which the molecular weight is 1000-3000g / mol and the two ends are hydroxyl / amino functionalized. Compared with an existing photochromic coating liquid formula, polymethylsiloxane is introduced into the coating liquid, a good microenvironment is provided for photochromic dye, the photochromic dye has good color changing depth and high color fading rate in a coating, and in addition, the lens coating is endowed with firm adhesive force and good surface hardness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer materials, and in particular relates to a photochromic coating liquid and a preparation method thereof. Background Art

[0002] Photochromism refers to the phenomenon that the optical properties of a material undergo a reversible change under the irradiation of ultraviolet light. Photochromism can change the color and transmittance, and this change is reversible. Organic photochromic dyes are popular because of their diverse structures and rich colors. They are widely used in information storage, optical lenses, textiles and clothing, printing and anti-counterfeiting, etc. At present, the most widely used organic photochromic dyes are spiropyran, spirooxazine, naphthopyran, naphthoxazine, fulgide, etc.

[0003] Smart photochromic lenses are a typical example of photochromic dye applications. They can filter out ultraviolet light from sunlight, reduce the intensity of light hitting the eyes outdoors, and make it more comfortable for the wearer to see objects outdoors. At the same time, reducing ultraviolet light also protects the wearer's eye health. Early photochromic lenses were glass lenses that used silver halide as a color-changing material. With the continuous advancement of science and technology, most photochromic lenses now use organic photochromic dyes. Photochromic dyes are added to the polymerized monomers of the lens substrate, and after curing and molding, smart photochromic lenses can be formed. This method is also called substrate color change. However, due to the influence of polymer molecules and polymerization environment, the color change / fading performance of the color-changing dye is limited when it is excited by ultraviolet rays. There are also disadvantages such as poor photostability, low photochromic response value, and insufficient thermal stability. In addition, due to the different thicknesses in the middle and around the lens, there is chromatic aberration after the lens changes color. In recent years, people have begun to develop new processes for preparing photochromic lenses. By coating a color-changing layer on the surface of the lens, not only can the uneven color change of the substrate and the large impact of the polymerization environment be solved, but it is also expected to achieve an ideal photochromic effect. However, existing photochromic coatings have certain shortcomings: (1) The color depth of the coating is difficult to deepen, the fading rate after the color change is slow, and a little base color remains for a long time; (2) The coating has poor adhesion and is easy to fall off the lens; (3) The coating is thick and soft, and it is easy to be scratched. Therefore, it is key to develop a photochromic coating liquid with deep color change, fast fading, strong adhesion and excellent mechanical properties. Summary of the invention

[0004] In order to overcome the problems existing in the existing photochromic coating, the present invention provides a photochromic coating liquid and a preparation method thereof.

[0005] The present invention provides a photochromic coating liquid, which is composed of a photochromic dye, an organic prepolymer, an isocyanate curing agent, polymethylsiloxane, an organic solvent, a coupling agent and an auxiliary agent. The content of each component is as follows by mass fraction:

[0006] Photochromic dye: 3-8%;

[0007] Organic prepolymer: 25-45%;

[0008] Isocyanate curing agent: 20-40%;

[0009] Polymethylsiloxane: 3-10%;

[0010] Organic solvent: 20-40%

[0011] Coupling agent: 2-6%;

[0012] Additives: 0.3~2%.

[0013] Furthermore, the photochromic dye includes one or more of spiropyran, spirooxazine, naphthopyran, and fulgide compounds.

[0014] Furthermore, the organic prepolymer includes one or more of polymethacrylic acid polyol, polyether polyol and polycarbonate polyol.

[0015] Further, the isocyanate curing agent includes one or more of toluene diisocyanate curing agent, diphenylmethane-4,4'-diisocyanate curing agent, 1,6-hexane diisocyanate curing agent, meta-xylylene diisocyanate curing agent, methylcyclohexyl diisocyanate curing agent, and isophorone diisocyanate curing agent.

[0016] Furthermore, the structural formula of the polymethylsiloxane is shown in Formula I below:

[0017]

[0018] Wherein R and R' are independently selected from H or CH 3 , and each structural unit is independent of each other;

[0019] R 1 and R 2 Independently selected from (CH 2 ) x OH or (CH 2 ) x NH 2 , where x=2~5.

[0020] Furthermore, the term "independent of each other" means that R and R' in each structural unit may be the same or different.

[0021] Furthermore, the molecular weight of the polymethylsiloxane is 1000 to 3000 g / mol.

[0022] Furthermore, the organic solvent includes one or more of toluene, xylene, N-methylpyrrolidone, N-ethylpyrrolidone, propylene glycol methyl ether, diethylene glycol dimethyl ether, ethylene glycol ethyl ether acetate, propylene glycol methyl ether acetate, ethyl acetate, and butyl acetate.

[0023] Furthermore, the coupling agent includes one or more of γ-aminopropyltriethoxysilane (APTES), γ-methacryloxypropyltrimethoxysilane (MPTS), γ-glycidyloxypropyltrimethoxysilane (GPTMS), and vinyltrimethoxysilane (VTMS).

[0024] Furthermore, the auxiliary agent includes an antioxidant, a light stabilizer or a leveling agent.

[0025] Further, the antioxidant includes hindered phenols, aromatic amines, nitrites, phosphates or mercaptans.

[0026] Further, the light stabilizer includes hindered amines, benzotriazoles, benzofuranones, benzophenones or triazines.

[0027] Furthermore, the leveling agent includes polysiloxanes, acrylates, fluorocarbons, polyethers or nonionic surfactants.

[0028] The present invention also provides a method for preparing the photochromic coating liquid, which comprises the following steps:

[0029] The photochromic dye and the auxiliary agent are added to the organic solvent and fully dissolved to form a solution A, and then the organic prepolymer, the isocyanate curing agent, the methylsiloxane and the coupling agent are fully mixed to form a solution B. Finally, the solution A is added to the solution B and stirred, and then filtered to obtain a photochromic coating liquid.

[0030] Furthermore, the stirring temperature in the preparation method is 10 to 40° C., and the stirring time is 1 to 24 hours.

[0031] The photochromic coating liquid provided by the present invention and the photochromic coating liquid prepared according to the preparation method are used in the fields of coatings, information storage, optical lenses, textiles and clothing, and printing anti-counterfeiting.

[0032] Furthermore, the photochromic coating liquid is applied by coating the surface of an article with the photochromic coating liquid by means of spin coating, spray gun coating, or immersion coating. After thermal curing, the coating thickness is controlled to be 5 to 20 μm, and a product with a reversible photochromic effect can be obtained by ultraviolet irradiation.

[0033] Compared with the prior art, the present invention has the following beneficial effects:

[0034] The present invention prepares a photochromic coating by adding a certain amount of organic siloxane into the main component polyurethane, and then cross-linking and modifying the polyurethane network during high-temperature curing, thereby enhancing the color-changing performance of the photochromic compound, greatly increasing the color-changing depth, accelerating the fading rate, and giving the coating excellent adhesion and mechanical strength.

[0035] The preparation method of the photochromic coating liquid of the present invention is simple and can be used in spin coating, spray coating and dip coating, and is easy to realize industrial application on photochromic lenses. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 This is a comparison picture of the color change of the photochromic coating prepared in Example 1 of the present invention on the lens before and after ultraviolet irradiation, and there are also traces of a hundred-grid adhesion test on it.

[0037] Figure 2 This is a hundred-grid adhesion test of the photochromic lens prepared in Example 1. DETAILED DESCRIPTION

[0038] The present invention is further described below in conjunction with examples, but the embodiments of the present invention are not limited thereto.

[0039] The raw materials in the embodiments and comparative examples are all commercially available products.

[0040] Example 1

[0041] The photochromic dye and the auxiliary agent (antioxidant and light stabilizer) are added to the organic solvent to fully dissolve to form a solution A, the organic prepolymer, the isocyanate curing agent, the methylsiloxane and the coupling agent are fully mixed to form a solution B, the solution A is added to the solution B and stirred at room temperature for 3 hours, and the photochromic coating liquid is obtained by filtration. The components and their contents are shown in Table 1 below:

[0042] Table 1

[0043]

[0044]

[0045] Wherein, the structural formula of spiropyran is as follows:

[0046]

[0047] The structural formula of polymethylsiloxane is as follows:

[0048]

[0049] The preparation method of the photochromic coating lens is as follows:

[0050] First, the lens blank was washed and dried. After the lens surface was moistened with N-methylpyrrolidone, the lens was fixed on a spin coater, 400 μL of photochromic coating liquid was added to the center of the lens, and the lens was rotated at 500 rpm for 20 seconds, and then at 1500 rpm for 30 seconds. Finally, the lens was dried and cured at 110°C for 2.5 hours to obtain a photochromic coated lens.

[0051] Example 2

[0052] The operation steps are the same as those in Example 1, and the material composition is shown in Table 2 below, and finally a photochromic coating and a photochromic coating lens are prepared.

[0053] Table 2

[0054] A solution Solution B Spiropyran: 4g Polymethacrylate polyol KN3210P: 16g N-Methylpyrrolidone: 20g Polycarbonate polyol PC-1122: 15g Antioxidant Zrganox-245: 0.5g Polyether polyol PTMEG2000: 5g Light stabilizer Tinuvin-144: 0.5g Isocyanate curing agent SBN70D: 30g Polymethylsiloxane M≈2000g / mol: 3g Coupling agent A-187: 3g

[0055] Example 3

[0056] The operation steps are the same as those in Example 1, and the material composition is shown in Table 3 below, and finally a photochromic coating and a photochromic coating lens are prepared.

[0057] Table 3

[0058] A solution Solution B Spiropyran: 4g Polymethacrylate polyol KN3210P: 16g N-Methylpyrrolidone: 20g Polycarbonate polyol PC-1122: 16g Antioxidant Zrganox-245: 0.5g Polyether polyol PTMEG2000: 5g Light stabilizer Tinuvin-144: 0.5g Isocyanate curing agent SBN70D: 30g Polymethylsiloxane M≈2000g / mol: 8g Coupling agent A-187: 3g

[0059] Example 4

[0060] The operation steps and the composition of each component are the same as those in Example 1, wherein the structural formula of polymethylsiloxane is adjusted to the following formula IV, and finally a photochromic coating and a photochromic coating lens are prepared.

[0061]

[0062] Example 5

[0063] The operation steps and the composition of each component are the same as those in Example 1, wherein the structural formula of polymethylsiloxane is adjusted to the following formula V, and finally a photochromic coating and a photochromic coating lens are prepared.

[0064]

[0065] Example 6

[0066] The operation steps and the composition of each component are the same as those in Example 1, wherein the molecular weight of polymethylsiloxane is adjusted to 1000 g / mol, and finally a photochromic coating and a photochromic coating lens are prepared.

[0067] Comparative Example 1

[0068] The preparation method of the photochromic coating is referred to in Example 1, except that polymethylsiloxane is not added.

[0069] Comparative Example 2

[0070] The preparation method of the photochromic coating is referred to in Example 1, except that the polymethylsiloxane is replaced by a small molecule tetraethoxysilane.

[0071] Comparative Example 3

[0072] The preparation method of the photochromic coating is described in Example 1, except that the molecular weight of the polymethylsiloxane is 4000 g / mol.

[0073] Comparative Example 4

[0074] Referring to the preparation method of the photochromic coating of Example 1, the only difference is that the polymethylsiloxane is replaced by an amino polymer, and the molecular formula is shown in the following formula VI:

[0075]

[0076] Performance Testing:

[0077] (1) Color change depth: The transmittance of the lens after being exposed to ultraviolet light for 2 minutes is measured by an instrument and expressed in %. The smaller the value, the deeper the color change.

[0078] (2) Fading rate: the time it takes for the lens to fade from its darkest color to half of its transmittance after being tinted, expressed in seconds;

[0079] (3) Adhesion: tested using the GB / T 9286-1998 100-grid cross-cut method;

[0080] (4) Surface hardness: Tested using the pencil hardness method of GB 6739-86;

[0081] The test results are shown in Table 4 below:

[0082] Table 4 Performance comparison of the photochromic coatings prepared in each embodiment and comparative example

[0083] Color change depth / % Fading rate / s Adhesion Surface hardness Example 1 17.2 52 5B 3H Example 2 18.5 55 5B 3H Example 3 18.8 48 5B 2H Example 4 16.6 57 5B 2H Example 5 19.0 60 4B 2H Example 6 18.3 54 5B 2H Comparative Example 1 20.1 127 4B H Comparative Example 2 28.6 115 3B HB Comparative Example 3 24.5 99 3B 2H Comparative Example 4 34.8 146 2B HB

[0084] It can be seen from Table 4 that the color change depth of Examples 1 to 6 is less than 20%, the fading rate is less than 60s, the adhesion exceeds level 4B, and the surface hardness is greater than 2H; while the other comparative examples are inferior to the embodiments.

[0085] The present invention uses the above-mentioned embodiments to illustrate a photochromic coating liquid and a preparation method thereof, but the present invention is not limited to the above-mentioned process steps, that is, it does not mean that the present invention must rely on the above-mentioned process steps to be implemented. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.

Claims

1. A photochromic coating liquid, characterized in that: The coating liquid is composed of a photochromic dye, an organic prepolymer, an isocyanate curing agent, polymethylsiloxane, an organic solvent, a coupling agent and an auxiliary agent. The content of each component is as follows by mass fraction: Photochromic dye: 3-8%; Organic prepolymer: 25-45%; Isocyanate curing agent: 20-40%; Polymethylsiloxane: 3-10%; Organic solvent: 20-40% Coupling agent: 2-6%; Additives: 0.3-2%; The structural formula of the polymethylsiloxane is shown in the following formula I: Wherein, R and R' are independently selected from H or CH3, and each structural unit is independent of each other; R1 and R2 are independently selected from (CH2) x OH or (CH2) x NH2, wherein x = 2 to 5; The molecular weight of the polymethylsiloxane is 1000-3000 g / mol.

2. The photochromic coating liquid according to claim 1, characterized in that: The photochromic dye includes one or more of spiropyran, spirooxazine, naphthopyran and fulgide compounds.

3. The photochromic coating liquid according to claim 1, characterized in that: The organic prepolymer includes at least one of polymethacrylic acid polyol, polyether polyol and polycarbonate polyol.

4. The photochromic coating liquid according to claim 1, characterized in that: The isocyanate curing agent includes at least one of toluene diisocyanate curing agent, diphenylmethane-4,4'-diisocyanate curing agent, 1,6-hexamethylene diisocyanate curing agent, meta-xylylene diisocyanate curing agent, methylcyclohexyl diisocyanate curing agent or isophorone diisocyanate curing agent.

5. The photochromic coating liquid according to claim 1, characterized in that: The organic solvent includes one or more of toluene, xylene, N-methylpyrrolidone, N-ethylpyrrolidone, propylene glycol methyl ether, diethylene glycol dimethyl ether, ethylene glycol ethyl ether acetate, propylene glycol methyl ether acetate, ethyl acetate, and butyl acetate.

6. The photochromic coating liquid according to claim 1, characterized in that: The coupling agent includes one or more of γ-aminopropyltriethoxysilane, γ-methacryloxypropyltrimethoxysilane, γ-glycidyloxypropyltrimethoxysilane or vinyltrimethoxysilane.

7. The photochromic coating liquid according to claim 1, characterized in that: The auxiliary agent includes an antioxidant, a light stabilizer or a leveling agent; the antioxidant includes hindered phenols, aromatic amines, nitrites, phosphates or thiols; the light stabilizer includes hindered amines, benzotriazoles, benzofuranones, benzophenones or triazines; the leveling agent includes polysiloxanes, acrylates, fluorocarbons, polyethers or non-ionic surfactants.

8. A method for preparing the photochromic coating liquid according to any one of claims 1 to 7, characterized in that: The preparation method comprises the following steps: The photochromic dye and the auxiliary agent are added to the organic solvent and fully dissolved to form a solution A, and then the organic prepolymer, the isocyanate curing agent, the methylsiloxane and the coupling agent are fully mixed to form a solution B. Finally, the solution A is added to the solution B and stirred, and then filtered to obtain a photochromic coating liquid.

9. Application of the photochromic coating liquid according to any one of claims 1 to 7 and / or the photochromic coating liquid prepared according to the preparation method according to claim 8 in the fields of coatings, information storage, optical lenses, textiles and clothing, and printing anti-counterfeiting.

10. The use according to claim 9, characterized in that The application is to cover the surface of an object with a photochromic coating liquid by means of spin coating, spray gun coating, and immersion coating. After thermal curing, the coating thickness is controlled at 5 to 20 μm, and a product with a reversible photochromic effect can be obtained by ultraviolet irradiation.

Citation Information

Patent Citations

  • Photochromic composition and optical product thereof

    CN106433608A