Polypropylene interface adhesive and application thereof
By using maleic anhydride graft modified propylene-butene copolymer in polypropylene interface adhesive, the adhesion between polypropylene and metal is enhanced, the problem of poor adhesion between polypropylene and metal is solved, and the poly The high-strength bonding of propylene/metal composite materials avoids modification of the polypropylene surface.
Patent Information
- Application Number
- CN202411284772.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-13
- Publication Date
- 2024-11-26
AI Technical Summary
The poor adhesion between polypropylene and metal limits the development and application of polypropylene and metal laminated composite materials. The existing interface adhesives require surface modification of polypropylene, which damages its structure and machinery. performance.
Develop a polypropylene interface adhesive containing polypropylene and maleic anhydride graft modified propylene-butene copolymer, which increases polarity through maleic anhydride groups, enhances interaction forces with metals, and crystallizes with The mechanical locking force forms an adhesion layer to achieve good adhesion between polypropylene and metal.
The bonding strength of polypropylene/metal composite materials is improved, the bonding strength requirements of polypropylene/metal laminated composite materials are met, the modification of the polypropylene surface is avoided, and its mechanical properties are maintained.
Smart Images

Figure CN119019961A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of adhesives, and in particular to a polypropylene interface adhesive and application thereof. Background Art
[0002] Metal / polymer laminate composites have the corresponding properties of polymers and metals, and have broad application prospects in the fields of electronic products, photovoltaics, energy batteries, automobiles, aerospace, and food / drug packaging. The successful application of metal / polymer laminate composites depends on the adhesive for metal / polymer interface bonding, which must adapt to the two materials with huge differences in surface energy.
[0003] Due to its low cost and easy processing performance, polypropylene has become one of the most widely used thermoplastic materials. In recent years, lightweight aluminum / thermoplastic polypropylene laminated composites have attracted attention from the industry. The interfacial adhesion problem of aluminum / polypropylene is the key to affecting the excellent performance of aluminum / polypropylene laminated composites. Strong adhesion is sufficient to withstand the stress and strain that may occur during the processing and molding process. However, polypropylene is generally hydrophobic and has low surface free energy, resulting in poor adhesion with other materials, especially the extremely low adhesion between polypropylene and metal, which seriously restricts the development and application of polypropylene and metal laminated composites.
[0004] At present, the commonly used interface adhesives in industry all require surface modification of polypropylene, and then laminated composite materials made of adhesives and metals can exert the excellent performance of laminated composite materials. For example, the surface of polypropylene needs to be chemically modified, flame treated, plasma treated, etc. However, these surface modification treatments not only require specific equipment, but also destroy the structure of polypropylene, resulting in a decrease in its own mechanical properties. Moreover, it is not suitable to improve the surface of polypropylene in many industrial applications. Therefore, there is an urgent need to develop an interface adhesive that can directly bond untreated polypropylene to metal. Summary of the invention
[0005] The purpose of the present invention is to provide a polypropylene interface adhesive and application thereof in view of the deficiencies in the prior art.
[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0007] The invention provides a polypropylene interface adhesive, which comprises polypropylene and a maleic anhydride graft-modified propylene-butene copolymer.
[0008] Preferably, the polypropylene comprises metallocene polypropylene or chlorinated polypropylene.
[0009] Preferably, the grafting rate of maleic anhydride in the maleic anhydride graft-modified propylene-butene copolymer is 3.8-7.2%.
[0010] Preferably, the mass fraction of polypropylene in the polypropylene interface adhesive is 10 to 50%.
[0011] The invention also provides application of the polypropylene interface adhesive in polypropylene / metal laminated composite materials.
[0012] Preferably, the metal of the polypropylene / metal laminate composite material comprises aluminum or copper.
[0013] Preferably, the thickness of the polypropylene interface adhesive is 10 to 200 μm.
[0014] Beneficial effects of the present invention:
[0015] The addition of maleic anhydride groups increases the polarity of the propylene-butene copolymer, so that the maleic anhydride grafted modified propylene-butene copolymer and metal aluminum form Al-O=CO better, thereby enhancing the interaction force between the adhesive and the metal aluminum; the crystallization of the polypropylene interface adhesive of the present invention is similar to that of polypropylene, and the crystallization of the adhesive can be diffused into the polypropylene substrate through crystallization force, van der Waals force, mechanical locking force, etc., so that the two polymer molecules in the adhesive and the polypropylene substrate are entangled with each other to form an adhesion layer, thereby generating good bonding ability. The interface adhesive prepared by the maleic anhydride grafted modified propylene-butene copolymer of the present invention and metallocene polypropylene and chlorinated polypropylene can simultaneously improve the interaction force with the polypropylene substrate and the metal substrate, so that the composite material of polypropylene / metal has good bonding strength, thereby meeting the bonding strength requirements of the polypropylene / metal laminated composite material. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 The peel test results of the polypropylene interface adhesive of Examples 1 to 9 and Comparative Examples 1 to 4 are shown;
[0017] Figure 2 The peel test results of the polypropylene interface adhesives of Examples 12 to 20 and Comparative Examples 5 to 8 are shown. DETAILED DESCRIPTION
[0018] The invention provides a polypropylene interface adhesive, which comprises polypropylene and a maleic anhydride graft-modified propylene-butene copolymer.
[0019] In the present invention, the polypropylene preferably comprises metallocene polypropylene or chlorinated polypropylene.
[0020] In the present invention, the grafting rate of maleic anhydride in the maleic anhydride graft-modified propylene-butene copolymer is preferably 3.8 to 7.2%, more preferably 4.5 to 6.5%, and even more preferably 5.2%.
[0021] In the present invention, the mass fraction of polypropylene in the polypropylene interface adhesive is preferably 10 to 50%, more preferably 20 to 40%, and even more preferably 30%.
[0022] The invention also provides application of the polypropylene interface adhesive in polypropylene / metal laminated composite materials.
[0023] In the present invention, the metal of the polypropylene / metal laminate composite material preferably comprises aluminum or copper.
[0024] In the present invention, the thickness of the polypropylene interface adhesive is preferably 10 to 200 μm, more preferably 20 to 50 μm, and even more preferably 30 μm.
[0025] In the present invention, when the polypropylene interface adhesive is used in an amount of not less than 0.1 kg, it is preferred that the polypropylene and the maleic anhydride grafted modified propylene-butene copolymer are directly melt-blended and coated on the surface of the substrate for curing.
[0026] In the present invention, the curing temperature is preferably 65 to 200° C., more preferably 120 to 180° C.; the curing time is preferably 1 to 8 minutes, more preferably 3 to 5 minutes.
[0027] In the present invention, when the polypropylene interface adhesive is used in an amount less than 0.1 kg, it is preferred that polypropylene and maleic anhydride grafted modified propylene-butene copolymer are mixed in xylene to obtain a mixed liquid, and the mixed liquid is dried to form a polypropylene interface adhesive film, and the polypropylene interface adhesive film is used for the interface bonding of polypropylene and metal in polypropylene / metal laminated composite materials.
[0028] In the present invention, the temperature of the mixed liquid is preferably 100-140°C, more preferably 120°C; the mixing is preferably carried out by stirring, the stirring speed is preferably 600-800r / min, more preferably 700r / min, and the stirring time is preferably 1-3h, more preferably 2h.
[0029] In the present invention, the mass fraction of the polypropylene interface adhesive in the mixed solution is preferably 10-30%, more preferably 15-25%, and more preferably 20%; the thickness of the polypropylene interface adhesive film is preferably 10-200 μm, more preferably 20-50 μm, and more preferably 30 μm.
[0030] In the present invention, the drying temperature is preferably 40-60°C, more preferably 45-55°C, and more preferably 50°C; the drying time is preferably 10-40h, more preferably 20-30h, and more preferably 24h.
[0031] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0032] The preparation method of the maleic anhydride grafted modified propylene-butene copolymer in the embodiment of the present invention is:
[0033] ① A method for preparing a maleic anhydride grafted modified propylene-butene copolymer with a maleic anhydride grafting rate of 3.8% is as follows: 10g of maleic anhydride is divided into 6 parts, and 10g of initiator DTBP is divided into 6 parts; the parameters of the RM200C mixing torque rheometer are set to a temperature of 180°C, a rotation speed of 60r / min, and a time of 18min. When the temperature rises to 180°C, the operation is started. At this time, 30g of propylene-butene copolymer (propylene unit content is 76wt%, butene unit content is 24wt%, and weight-average molecular weight is 214,000) and 1 part of maleic anhydride and 1 part of initiator DTBP are added to the RM200C mixing torque rheometer at the same time. After that, 1 part of maleic anhydride and 1 part of initiator DTBP are added to the RM200C mixing torque rheometer every 3min until the reaction is completed, thereby obtaining a maleic anhydride grafted modified propylene-butene copolymer with a maleic anhydride grafting rate of 3.8%.
[0034] ② A method for preparing a maleic anhydride grafted modified propylene-butene copolymer with a maleic anhydride grafting rate of 5.2% as follows: 20g of maleic anhydride is divided into 10 parts, and 10g of initiator DTBP is divided into 10 parts; the parameters of the RM200C mixing torque rheometer are set to a temperature of 180°C, a rotation speed of 60r / min, and a time of 50min. When the temperature rises to 180°C, the operation is started. At this time, 30g of propylene-butene copolymer (propylene unit content is 76wt%, butene unit content is 24wt%, and weight-average molecular weight is 214,000) and 1 part of maleic anhydride and 1 part of initiator DTBP are added to the RM200C mixing torque rheometer at the same time. After that, 1 part of maleic anhydride and 1 part of initiator DTBP are added to the RM200C mixing torque rheometer every 5min until the reaction is completed, thereby obtaining a maleic anhydride grafted modified propylene-butene copolymer with a maleic anhydride grafting rate of 5.2%.
[0035] ③ A method for preparing a maleic anhydride grafted modified propylene-butene copolymer having a maleic anhydride grafting rate of 7.2% as follows: 30g of maleic anhydride is divided into 10 parts, and 14g of initiator DTBP is divided into 10 parts; the parameters of the RM200C mixing torque rheometer are set to a temperature of 180°C, a rotation speed of 60r / min, and a time of 50min. When the temperature rises to 180°C, the operation is started. At this time, 30g of propylene-butene copolymer (propylene unit content is 76wt%, butene unit content is 24wt%, and weight-average molecular weight is 214,000) and 1 part of maleic anhydride and 1 part of initiator DTBP are added to the RM200C mixing torque rheometer at the same time. After that, 1 part of maleic anhydride and 1 part of initiator DTBP are added to the RM200C mixing torque rheometer every 5min until the reaction is completed, thereby obtaining a maleic anhydride grafted modified propylene-butene copolymer having a maleic anhydride grafting rate of 7.2%.
[0036] In the embodiments of the present invention, the polypropylene interface adhesive is mixed with xylene and then used for the interface bonding between polypropylene and metal in the polypropylene / metal laminated composite material.
[0037] Example 1
[0038] Metallocene polypropylene (mPP) with a mass ratio of 1:9 and maleic anhydride grafted modified propylene-butene copolymer with a maleic anhydride grafting rate of 3.8% are added into a three-necked flask, and xylene is added to make a mixed solution with a mass fraction of 20%. The mixed solution is heated to 120°C and stirred at a speed of 700r / min for 2h; the obtained mixed solution is dripped into a 60mm×15mm×150μm polytetrafluoroethylene mold until the mold is filled, and the mold is placed in a 50°C oven and dried for 24h to obtain a polypropylene interface adhesive film.
[0039] Example 2
[0040] The mass ratio of the metallocene polypropylene and the maleic anhydride grafted modified propylene-butene copolymer in Example 1 was changed to 3:7, and the other parts were the same as in Example 1.
[0041] Example 3
[0042] The mass ratio of the metallocene polypropylene and the maleic anhydride grafted modified propylene-butene copolymer in Example 1 was changed to 1:1, and the other parts were the same as in Example 1.
[0043] Example 4
[0044] The maleic anhydride grafted modified propylene-butene copolymer with a maleic anhydride grafting rate of 3.8% in Example 1 is replaced with a maleic anhydride grafted modified propylene-butene copolymer with a maleic anhydride grafting rate of 5.2%, and the rest is the same as Example 1.
[0045] Example 5
[0046] The maleic anhydride grafted modified propylene-butene copolymer with a maleic anhydride grafting rate of 3.8% in Example 1 was changed to a maleic anhydride grafted modified propylene-butene copolymer with a maleic anhydride grafting rate of 5.2%, and the mass ratio of metallocene polypropylene to maleic anhydride grafted modified propylene-butene copolymer was changed to 3:7. Others were the same as in Example 1.
[0047] Example 6
[0048] The maleic anhydride grafted modified propylene-butene copolymer with a maleic anhydride grafting rate of 3.8% in Example 1 was changed to a maleic anhydride grafted modified propylene-butene copolymer with a maleic anhydride grafting rate of 5.2%, and the mass ratio of metallocene polypropylene and maleic anhydride grafted modified propylene-butene copolymer was changed to 1:1. The rest was the same as Example 1.
[0049] Example 7
[0050] The maleic anhydride grafted modified propylene-butene copolymer with a maleic anhydride grafting rate of 3.8% in Example 1 is replaced with a maleic anhydride grafted modified propylene-butene copolymer with a maleic anhydride grafting rate of 7.2%, and the rest is the same as Example 1.
[0051] Example 8
[0052] The maleic anhydride grafted modified propylene-butene copolymer with a maleic anhydride grafting rate of 3.8% in Example 1 was changed to a maleic anhydride grafted modified propylene-butene copolymer with a maleic anhydride grafting rate of 7.2%, and the mass ratio of metallocene polypropylene to maleic anhydride grafted modified propylene-butene copolymer was changed to 3:7. The rest was the same as Example 1.
[0053] Example 9
[0054] The maleic anhydride grafted modified propylene-butene copolymer with a maleic anhydride grafting rate of 3.8% in Example 1 was changed to a maleic anhydride grafted modified propylene-butene copolymer with a maleic anhydride grafting rate of 7.2%, and the mass ratio of metallocene polypropylene and maleic anhydride grafted modified propylene-butene copolymer was changed to 1:1. The rest was the same as Example 1.
[0055] Example 10
[0056] The mass fraction of the mixed liquid in Example 1 was changed to 10%, the oven temperature was modified to 40° C., the drying time was changed to 20 h, and the rest was the same as in Example 1.
[0057] Embodiment 11
[0058] The mass fraction of the mixed liquid in Example 1 was changed to 30%, the oven temperature was modified to 60° C., the drying time was changed to 30 h, and the rest was the same as in Example 1.
[0059] Example 12
[0060] Chlorinated polypropylene (CPP) with a mass ratio of 1:9 and maleic anhydride grafted modified propylene-butene copolymer with a maleic anhydride grafting rate of 3.8% are added into a three-necked flask, and xylene is added to make a mixed solution with a mass fraction of 20%. The mixed solution is heated to 120°C and stirred at a speed of 800r / min for 2h; the obtained mixed solution is dripped into a 60mm×15mm×150μm polytetrafluoroethylene mold until the mold is filled, and the mold is placed in a 50°C oven and dried for 24h to obtain a polypropylene interface adhesive film.
[0061] Embodiment 13
[0062] The mass ratio of chlorinated polypropylene and maleic anhydride grafted modified propylene-butene copolymer in Example 12 was changed to 3:7, and the rest was the same as Example 12.
[0063] Embodiment 14
[0064] The mass ratio of chlorinated polypropylene and maleic anhydride grafted modified propylene-butene copolymer in Example 12 was changed to 1:1, and the rest was the same as Example 12.
[0065] Embodiment 15
[0066] The maleic anhydride grafted modified propylene-butene copolymer with a maleic anhydride grafting rate of 3.8% in Example 12 is replaced with a maleic anhydride grafted modified propylene-butene copolymer with a maleic anhydride grafting rate of 5.2%, and the rest is the same as Example 12.
[0067] Example 16
[0068] The maleic anhydride grafted modified propylene-butene copolymer with a maleic anhydride grafting rate of 3.8% in Example 12 is changed to a maleic anhydride grafted modified propylene-butene copolymer with a maleic anhydride grafting rate of 5.2%, and the mass ratio of chlorinated polypropylene and maleic anhydride grafted modified propylene-butene copolymer is changed to 3:7. The rest is the same as Example 12.
[0069] Embodiment 17
[0070] The maleic anhydride grafted modified propylene-butene copolymer with a maleic anhydride grafting rate of 3.8% in Example 12 is replaced with a maleic anhydride grafted modified propylene-butene copolymer with a maleic anhydride grafting rate of 5.2%, and the mass ratio of chlorinated polypropylene and maleic anhydride grafted modified propylene-butene copolymer is changed to 1:1. The rest is the same as Example 12.
[0071] Embodiment 18
[0072] The maleic anhydride grafted modified propylene-butene copolymer with a maleic anhydride grafting rate of 3.8% in Example 12 is replaced with a maleic anhydride grafted modified propylene-butene copolymer with a maleic anhydride grafting rate of 7.2%, and the rest is the same as Example 12.
[0073] Embodiment 19
[0074] The maleic anhydride grafted modified propylene-butene copolymer with a maleic anhydride grafting rate of 3.8% in Example 12 is changed to a maleic anhydride grafted modified propylene-butene copolymer with a maleic anhydride grafting rate of 7.2%, and the mass ratio of chlorinated polypropylene and maleic anhydride grafted modified propylene-butene copolymer is changed to 3:7. The rest is the same as Example 12.
[0075] Embodiment 20
[0076] The maleic anhydride grafted modified propylene-butene copolymer with a maleic anhydride grafting rate of 3.8% in Example 12 is replaced with a maleic anhydride grafted modified propylene-butene copolymer with a maleic anhydride grafting rate of 7.2%, and the mass ratio of chlorinated polypropylene and maleic anhydride grafted modified propylene-butene copolymer is changed to 1:1. The rest is the same as Example 12.
[0077] Comparative Example 1
[0078] The metallocene polypropylene in Example 1 is omitted, and the rest is the same as in Example 1.
[0079] Comparative Example 2
[0080] The maleic anhydride graft-modified propylene-butene copolymer in Example 1 is omitted, and the rest is the same as in Example 1.
[0081] Comparative Example 3
[0082] The metallocene polypropylene in Example 4 is omitted, and the rest is the same as in Example 4.
[0083] Comparative Example 4
[0084] The metallocene polypropylene in Example 7 is omitted, and the rest is the same as Example 7.
[0085] Comparative Example 5
[0086] Omit the chlorinated polypropylene in Example 12, and the rest is the same as Example 12.
[0087] Comparative Example 6
[0088] The maleic anhydride graft-modified propylene-butene copolymer in Example 12 is omitted, and the rest is the same as Example 12.
[0089] Comparative Example 7
[0090] Omit the chlorinated polypropylene in Example 15, and the rest is the same as Example 15.
[0091] Comparative Example 8
[0092] Omit the chlorinated polypropylene in Example 18, and the rest is the same as Example 18.
[0093] The polypropylene interface adhesive films prepared in Examples 1 to 20 and Comparative Examples 1 to 8 were respectively placed between a polypropylene laminate and an aluminum foil, and the polypropylene / aluminum foil laminate was placed in a GT-7014-P flat-plate hot press and hot-pressed at 10 MPa and 155° C. for 3 min. After being taken out, a peeling test was performed at a speed of 100 mm / s at room temperature using an Instron 3400 tensile testing machine in accordance with GB / T 2791-1995.
[0094] The peel test results of the polypropylene interface adhesives of Examples 1 to 9 and Comparative Examples 1 to 4 are shown in Table 1. Figure 1 .
[0095] Table 1 Peel test results of polypropylene interface adhesive
[0096]
[0097]
[0098] As shown in Table 1, as the proportion of metallocene polypropylene increases, the bonding performance shows a trend of first increasing and then decreasing. This is because the crystallization of metallocene polypropylene is similar to that of polypropylene. Metallocene polypropylene can diffuse into the polypropylene substrate through crystallization force, van der Waals force, mechanical locking force, etc., so that the two polymer molecules are entangled with each other to form an adhesion layer, resulting in good bonding ability, so that the polypropylene / aluminum foil composite laminate material achieves good bonding strength.
[0099] The peel test results of the polypropylene interface adhesives of Examples 12 to 20 and Comparative Examples 5 to 8 are shown in Table 2. Figure 2 .
[0100] Table 2 Peel test results of polypropylene interface adhesive
[0101]
[0102]
[0103] As shown in Table 2, by adding chlorinated polypropylene to the maleic anhydride grafted modified propylene-butene copolymer, the bonding performance of the adhesive is improved. As the proportion of chlorinated polypropylene increases, the bonding strength shows a trend of first increasing and then decreasing. This is because chlorinated polypropylene also has polarity, which increases the compatibility of the adhesive with the polypropylene substrate.
[0104] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A polypropylene interface adhesive, characterized in that: It contains polypropylene and maleic anhydride grafted modified propylene-butene copolymer.
2. The polypropylene interface adhesive according to claim 1, characterized in that: The polypropylene comprises metallocene polypropylene or chlorinated polypropylene.
3. The polypropylene interface adhesive according to claim 1 or 2, characterized in that: The grafting rate of maleic anhydride in the maleic anhydride graft-modified propylene-butene copolymer is 3.8-7.2%.
4. The polypropylene interface adhesive according to claim 3, characterized in that: In the polypropylene interface adhesive, the mass fraction of polypropylene is 10-50%.
5. Use of the polypropylene interface adhesive according to any one of claims 1 to 4 in polypropylene / metal laminated composite materials.
6. Use of the polypropylene interface adhesive according to claim 5 in polypropylene / metal laminate composite materials, characterized in that: The metal of the polypropylene / metal laminate composite material comprises aluminum or copper.
7. Use of the polypropylene interface adhesive according to claim 5 or 6 in polypropylene / metal laminate composite materials, characterized in that: The thickness of the polypropylene interface adhesive is 10 to 200 μm.