Refining slag system as well as preparation method and application thereof
Through the adjustment of the components and particle size of the refining slag system, the oxygen, nitrogen and sulfur inclusions in the return material of the high-temperature alloy are successfully removed, the cleanliness and quality of the alloy is improved, and the problem of difficulty in removing impurities in the prior art is solved. Cost reduction and process simplification are achieved.
Patent Information
- Application Number
- CN202411152041.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-08-21
AI Technical Summary
The prior art is difficult to effectively remove impurities in the return material of high-temperature alloys, resulting in low alloy quality and high production costs.
A refining residue system is provided, and the components include 40% to 55% Al2O3, 20% to 30% SiO2, 16% to 22% K2O, 3% to 10% Na2O, 2% to 4% CaO, and the components are adjusted. Content and particle size distribution are used for vacuum refining to remove oxygen, nitrogen and sulfur inclusions in the return material of FGH97 alloy and reduce impurity content.
It significantly improves the cleanliness and quality of the recovered alloy, reduces the alloy production cost, simplifies the refining process, and reduces dust pollution.
Smart Images

Figure CN119020631A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of vacuum refining technology, and in particular to a refined slag system and a preparation method and application thereof. Background Art
[0002] With the rapid development of my country's aerospace, gas turbine, nuclear power and other industries, the use of high-temperature alloy materials is increasing. However, the cleanliness requirements of high-temperature alloy finished products are high, the processing steps are many, the manufacturing process is long, and the effective utilization rate of materials is low. For example, the weight of high-temperature alloy finished products is usually only 30% of the total weight of the original input metal materials, and some are even only about 10%. The rest are in the form of unqualified powder, turnings, cuttings, tails, risers, runners, and forging wastes. The above wastes are all called high-temperature alloy return materials. The content of strategic alloying elements (Ni, Co, Cr, W, Mo, etc.) in high-temperature alloys exceeds 40%, and there are more than 40 main alloying elements and trace elements, including rare and precious elements such as Nb, Ta, Hf, Re, etc. Therefore, the return materials of high-temperature alloys generally need to be melted again for reuse.
[0003] Taking FGH97 alloy as an example, it has excellent heat resistance, corrosion resistance and mechanical properties. However, during the smelting process, there are a lot of impurities and oxides in the FGH97 alloy return material, and it is difficult to remove these impurities by the current refining method. Therefore, developing a FGH97 alloy return material purification technology is of great significance for improving alloy quality and reducing production costs. Summary of the invention
[0004] The present application provides a refining slag system and a preparation method and application thereof. The refining slag system of the present application can remove most of the impurities in the FGH97 alloy return material, thereby improving the quality of the recovered alloy and reducing the production cost of the alloy.
[0005] In a first aspect, the present application provides a refined slag system, whose components, by mass fraction, include 40% to 55% Al2O3, 20% to 30% SiO2, 16% to 22% K2O, 3% to 10% Na2O, and 2% to 4% CaO.
[0006] Based on the refining slag system of the present application, by adjusting the content between each component, the content of oxygen, nitrogen and sulfur inclusions in the alloy return material can be effectively reduced, and the technical effect of purifying the alloy return material can be achieved. Among them, 40% to 55% Al2O3 and 20% to 30% SiO2 are combined to play the role of adsorbing impurities such as oxygen, nitrogen and sulfur inclusions. The specific content of K2O, Na2O and CaO can not only reduce the melting point of the refining slag system, but also adjust the fluidity of the refining slag system to ensure that Al2O3 and SiO2 can better adsorb oxygen, nitrogen and sulfur inclusions. The refining slag system of the present application can remove most of the impurities in the FGH97 alloy return material, which is beneficial to improve the quality of the recovered alloy and reduce the production cost of the alloy.
[0007] In some of the embodiments, the components of the refined slag system may specifically include 40% to 50% Al2O3, 20% to 30% SiO2, 16% to 19% K2O, 8% to 10% Na2O, and 2% to 4% CaO, by mass fraction.
[0008] In some of the embodiments, based on the total mass of the refined slag system, it satisfies at least one of the following conditions: (1) the total content of MgO and TiO2 is not more than 0.5%; (2) the carbon content is not more than 0.03%; (3) the phosphorus content is not more than 0.01%; (4) the sulfur content is not more than 0.005%.
[0009] Based on the above embodiments, the above refined slag system introduces fewer impurities when used, which is more conducive to improving the cleanliness of the recovered alloy.
[0010] In some of the embodiments, the refined slag is in granular form, and the average particle size of the granular refined slag is not greater than 10 mm.
[0011] Based on the above embodiments, the granular refined slag with an average particle size of no more than 10 mm can be better fused with the alloy when used, and can further increase the cleanliness of the recovered alloy.
[0012] In some of the embodiments, in the refined slag system, based on the total mass of the refined slag system, the particle size is between 5 mm and 10 mm, accounting for 25% to 35%, the particle size is greater than 0.5 mm and less than 5 mm, accounting for 60% to 74%, and the particle size is not greater than 0.5 mm, accounting for 1% to 5%.
[0013] Based on the above embodiments, the particle size of the refined slag system is relatively uniform, which is conducive to smelting and has good fluidity, and can reduce dust pollution.
[0014] In the second aspect, the present application provides a method for preparing a refined slag system, which comprises the following steps: ball milling the mixture, and then smelting, cooling and crushing in sequence; the mixture comprises, by mass fraction, 40% to 55% Al2O3, 20% to 30% SiO2, 16% to 22% K2O, 3% to 10% Na2O, and 2% to 4% CaO.
[0015] Based on the above preparation method, the obtained refined slag system can remove most of the impurities in the FGH97 alloy return material, which is beneficial to improve the quality of the recovered alloy and reduce the production cost of the alloy.
[0016] In some of the embodiments, the mixture satisfies at least one of the following conditions: (1) the average particle size of Al2O3 is not greater than 3 mm; (2) the average particle size of TiO2 is not greater than 3 mm; (3) the average particle size of Na2O is not greater than 4 mm; (4) the average particle size of CaO is not greater than 3 mm.
[0017] Based on the above embodiments, the preparation time of the refined slag system is shorter, and the components of the prepared refined slag system are more uniform and the purification effect is better.
[0018] In a third aspect, the present application provides the use of the above-mentioned refined slag system in the return material of vacuum refined FGH97 alloy.
[0019] Based on the above applications, the refining process of FGH97 alloy return material is simpler, with lower consumption and better purification effect.
[0020] In some of the embodiments, the mass ratio of the refining slag system to the FGH97 alloy return material during refining is 0.5:1 to 2:1.
[0021] Based on the above embodiments, controlling the mass ratio within a reasonable range can accelerate the removal of inclusions in the FGH97 alloy return material and ensure the refining effect.
[0022] In some embodiments, the vacuum refining time is 60 to 120 min; and / or the vacuum degree during refining is 20 to 100 Pa.
[0023] Based on the above embodiments, controlling the vacuum refining time and vacuum degree within an appropriate range is more conducive to removing dissolved oxygen and nitrogen in the FGH97 alloy return material. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For those skilled in the art, other drawings can be obtained based on these drawings without paying any creative work.
[0025] Figure 1 This is the EDS element distribution diagram of the refined slag system in Example 1 of the present application. DETAILED DESCRIPTION
[0026] In order to make the purpose, technical solution and advantages of the present application more clearly understood, the present application is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.
[0027] In the prior art, when the FGH97 alloy return material is vacuum refined, the impurities in its components are not easy to be purified, and the recovery quality is not high. In order to solve the above technical problems, the present application proposes a refining slag system, which can effectively remove most of the impurities in the FGH97 alloy return material and improve the recovery quality by using the refining slag system in the present application to vacuum refine the FGH97 alloy return material.
[0028] In the first aspect, the present application provides a refined slag system, the components of which are calculated by mass fraction, including 40% to 55% Al2O3, 20% to 30% SiO2, 16% to 22% K2O, 3% to 10% Na2O, and 2% to 4% CaO. Preferably, the preferred range of each component in the refined slag system can be 40% to 50% Al2O3, 20% to 30% SiO2, 16% to 19% K2O, 8% to 10% Na2O, and 2% to 4% CaO. The synergistic effect of each component in the present application within a specific range can effectively reduce the content of oxygen, nitrogen, and sulfur inclusions in the FGH97 alloy return material, improve the cleanliness of the high-temperature alloy, and thus improve the quality of the recovered alloy. In the refined slag system of the present application, the combination of Al2O3 and SiO2 within the above content range can play a role in absorbing impurities such as oxygen, nitrogen, and sulfur inclusions. K2O, Na2O, and CaO can reduce the melting point of the refined slag system and adjust the fluidity of the refined slag system, so that Al2O3 and SiO2 can better absorb oxygen, nitrogen, and sulfur inclusions. Therefore, the refined slag system in the present application can remove most of the impurities in the FGH97 alloy return material, improve the quality of the recovered alloy, and reduce the production cost of the alloy.
[0029] Of course, in some other embodiments, in order to further improve the flow properties of the refined slag system, the refined slag system may also include Fe3O4 and the like, as long as the purpose of the present application can be achieved, and no further details will be given here.
[0030] In some embodiments of the present application, in order to ensure that the refined slag system introduces fewer impurities during use and further improve the cleanliness of the recovered alloy, the refined slag system generally meets at least one of the following conditions: (1) the total content of MgO and TiO2 is not more than 0.5%; (2) the carbon content is not more than 0.03%; (3) the phosphorus content is not more than 0.01%; (4) the sulfur content is not more than 0.005%. It should be noted that the above-mentioned MgO, TiO2, C, P, S and the like are not components that must be contained, but are inevitable impurities in the process of preparing the refined slag system. These impurities are usually derived from raw materials. Due to the low content of impurities, they are usually ignored.
[0031] In some embodiments of the present application, the refined slag system is usually in a granular form, and the average particle size is not greater than 10 mm, so that the refined slag system can be better fused with the alloy when used, and can further increase the cleanliness of the recovered alloy. It should also be noted that the same components of the refined slag system in the present application are not aggregated together, but are evenly mixed. Therefore, when the refined slag system is granular, the components of each particle are similar or even the same, and will contain Al2O3, SiO2, K2O, Na2O, CaO, Fe3O4, etc.
[0032] In the present application, the equivalent volume particle size is used to characterize the particle size of the particle, that is, the particle size of the particle to be measured is equal to the diameter of a spherical particle with the same volume as the particle to be measured.
[0033] In addition, in some embodiments of the present application, based on the total mass of the refined slag system, in the granular refined slag system, the particle size is 5mm-10mm, accounting for 25%-35%, the particle size is greater than 0.5mm and less than 5mm, accounting for 60%-74%, and the particle size is not greater than 0.5mm, accounting for 1%-5%, so that the particle size of the refined slag system is more uniform, which is conducive to smelting and has good fluidity, and can reduce dust pollution. As an example, in the embodiment of the present application, the particle size is 5mm-10mm, accounting for 25%, the particle size is greater than 0.5mm and less than 5mm, accounting for 70%, and the particle size is not greater than 0.5mm, accounting for 5%.
[0034] In a second aspect, the present application also provides a method for preparing the above-mentioned refined slag system, which specifically comprises the following steps:
[0035] S100, ball milling the mixed material.
[0036] In this step, the mixed material includes 40% to 55% Al2O3, 20% to 30% SiO2, 16% to 22% K2O, 3% to 10% Na2O, and 2% to 4% CaO. Ball milling is generally performed in a ball mill, and the ball milling time is generally 2 to 4 hours, which is conducive to quickly melting the mixed material in the next step.
[0037] In addition, in order to shorten the preparation time and make the components of the refined slag system more uniform and the purification effect better, each component in the mixture should meet at least one of the following conditions: (1) the average particle size of Al2O3 is not greater than 3 mm; (2) the average particle size of TiO2 is not greater than 3 mm; (3) the average particle size of Na2O is not greater than 4 mm; (4) the average particle size of CaO is not greater than 3 mm.
[0038] In practical production, the smaller the particle size of each raw material, the better, because in this way the raw materials are mixed more evenly and the components of the refined slag system are more uniform. However, based on the need to control costs, in the examples of this application, the average particle size of Al2O3, TiO2, Na2O, and CaO is 2 mm, and the ball milling time is 3 hours.
[0039] In addition, this step does not have any special requirements for the purity and water content of the raw materials. However, in the actual preparation process, in order to ensure that the refined slag system has fewer impurities, raw materials with high purity are generally selected as much as possible based on cost considerations. For raw materials that are easy to absorb water and deliquesce, their water content is generally reduced as much as possible; for example: Al2O3 purity ≥99.5%; SiO2 purity ≥98%; K2O purity ≥99%, water content ≤0.5%; Na2O purity ≥99.5%, water content ≤0.5%; CaO purity ≥99%, water content ≤0.1%.
[0040] S200, melting the mixed material.
[0041] This step is generally carried out by placing the ball-milled mixture into an electric arc furnace, supplying power to the electric arc furnace, heating the mixture with a graphite electrode, and then evenly mixing the completely melted mixture to form a mixed system. This step generally also involves component testing of the mixed system to ensure that each component in the mixture is within a preset range, which is conducive to the subsequent formation of a refined slag system that meets the preset conditions.
[0042] S300, cooling and crushing.
[0043] In this step, the mixed system is poured into a copper mold for cooling, and then the cooled mixed system is put into a crusher for crushing to obtain a refined slag system. In addition, in this step, the average particle size of the refined slag system obtained after crushing is generally not greater than 10 mm, so that the refined slag system can be better fused with the alloy when used, and the cleanliness of the recovered alloy can be further increased.
[0044] S400, screening and refining slag system.
[0045] This step usually uses screening equipment to screen the particle size of the refined slag system. After screening, based on the total mass of the refined slag system, the particle size is 5mm-10mm, accounting for 25%-35%, the particle size is greater than 0.5mm and less than 5mm, accounting for 60%-74%, and the particle size is not greater than 0.5mm, accounting for 1%-5%.
[0046] In addition, in the actual production process, the refined slag system may not be used immediately. In this case, the refined slag system can be dried and then stored. Specifically, the refined slag system can be placed in an alumina crucible and then baked in a resistance furnace to reduce moisture. The maximum baking temperature is 950℃±20℃, and the insulation time is 2 to 3 hours. After the insulation is completed, it is cooled, and then the cooled refined slag system is placed in a moisture-proof aluminum foil bag, and after the air is evacuated, high-purity argon gas (purity>99.9%) is filled in and sealed for use.
[0047] In the third aspect, the present application also provides the application of the refining slag system in the vacuum refining of the FGH97 alloy return material. The refining slag system of the present application is used for the vacuum refining of the FGH97 alloy return material, which can simplify the refining process of the FGH97 alloy return material, not only reduce the energy consumption of vacuum refining, but also have better purification effect. Specifically, in some embodiments of the present application, the mass ratio of the refining slag system and the FGH97 alloy return material during refining is 0.5:1-2:1, which can accelerate the removal of inclusions in the FGH97 alloy return material and ensure the refining effect; the vacuum refining time is generally 60-120min; the vacuum degree during refining is 20-100Pa. In addition, when vacuum refining the FGH97 alloy return material, the FGH97 alloy return material can be added to the crucible, and then the above-mentioned refining slag system is added and placed in a vacuum reactor for refining; or the FGH97 alloy return material can be added to the crucible and placed in an argon atmosphere reactor to heat up to melting, and then the above-mentioned refining slag system is added for vacuum refining.
[0048] Example
[0049] The following examples and comparative examples are given to more specifically describe the embodiments of the present application. Various tests and evaluations were performed according to the following methods. In addition, unless otherwise specified, "parts" and "%" are based on mass.
[0050] Test methods and equipment:
[0051] Determination of uniformity of refined slag system:
[0052] Take 500 mg of refined slag and analyze its particle cross-section components using an energy dispersive spectrometer (EDS). Figure 1 This is the EDS element distribution diagram of the refined slag system in Example 1. Figure 1It can be seen that the composition of the refined slag system is relatively uniform.
[0053] Purification effect test:
[0054] 5000g or 10000g of FGH97 alloy return material is added to a crucible, and then the refined slag is added and placed in a vacuum reactor for refining. A cubic sample of about 5mm in the center of the refined alloy ingot is taken and the oxygen content, nitrogen content and sulfur content of the recovered alloy are tested using an oxygen, nitrogen and sulfur analyzer.
[0055] The mass ratio of the refined slag system to the FGH97 alloy return material is 1:1, 1:2 or 2:1, the vacuum refining time is 60 min or 120 min, and the vacuum degree during refining is 60 Pa. The specific purification conditions and purification effects can be seen in Table 1.
[0056] Example 1
[0057] This embodiment provides a refined slag system, and the preparation method thereof is as follows:
[0058] (1) 45% Al2O3, 25% SiO2, 18% K2O, 10% Na2O, and 2% CaO were mixed to form a mixture, and the mixture was ball-milled in a ball mill for 3 h.
[0059] (2) The ball-milled mixture is placed in an electric arc furnace and then smelted until the completely melted mixture is mixed evenly to form a mixed system.
[0060] (3) The mixed system is poured into a copper mold for cooling, and then the cooled mixed system is placed in a crusher for crushing to obtain a refined slag system.
[0061] Detected by an element analyzer, the impurities in the refined slag system include, by mass content, 0.02% C, 0.008% P, 0.003% S, and the sum of the mass content of MgO and TiO2 is 0.42%.
[0062] Example 2
[0063] This embodiment provides a refined slag system, and its preparation method is different from that of Example 1 in that: in step (1), 40% Al2O3, 30% SiO2, 16% K2O, 10% Na2O, and 4% CaO are mixed to form a mixture, which is then ball-milled in a ball mill for 3 hours.
[0064] Detected by an element analyzer, the impurities in the refined slag system include, by mass content, 0.01% C, 0.006% P, 0.005% S, and the sum of the mass content of MgO and TiO2 is 0.48%.
[0065] Example 3
[0066] This embodiment provides a refined slag system, and its preparation method is different from that of Example 1 in that: in step (1), 50% Al2O3, 20% SiO2, 19% K2O, 8% Na2O, and 3% CaO are mixed to form a mixture, which is then ball-milled in a ball mill for 3 hours.
[0067] Detected by an element analyzer, the impurities in the refined slag system include, by mass content, 0.03% C, 0.005% P, 0.004% S, and the sum of the mass content of MgO and TiO2 is 0.40%.
[0068] Example 4
[0069] This embodiment provides a refined slag system, and its preparation method is different from that of Example 1 in that: in step (1), 52% Al2O3, 25% SiO2, 22% K2O, 3% Na2O, and 2% CaO are mixed to form a mixture, which is then ball-milled in a ball mill for 3 hours.
[0070] Detected by an element analyzer, the impurities in the refined slag system include, by mass content, 0.05% C, 0.008% P, 0.009% S, and the sum of the mass content of MgO and TiO2 is 0.44%.
[0071] Comparative Example 1
[0072] This embodiment provides a refined slag system, and its preparation method is different from that of Example 1 in that: in step (1), 38% Al2O3, 32% SiO2, 18% K2O, 10% Na2O, and 2% CaO are mixed to form a mixture, which is then ball-milled in a ball mill for 3 hours.
[0073] Detected by an element analyzer, the impurities in the refined slag system include, by mass content, 0.03% C, 0.006% P, 0.006% S, and the sum of the mass content of MgO and TiO2 is 0.45%.
[0074] Comparative Example 2
[0075] This embodiment provides a refined slag system, and its preparation method is different from that of Example 1 in that: in step (1), 56% Al2O3, 14% SiO2, 18% K2O, 10% Na2O, and 2% CaO are mixed to form a mixture, which is then ball-milled in a ball mill for 3 hours.
[0076] Detected by an element analyzer, the impurities in the refined slag system include, by mass content, 0.02% C, 0.008% P, 0.008% S, and the sum of the mass content of MgO and TiO2 is 0.44%.
[0077] Table 1 Purification conditions and purification effects of the refined slag system of each embodiment and comparative example
[0078]
[0079]
[0080] It can be seen from Table 1 that the refined slag system in the present application can remove most of the impurities in the FGH97 alloy return material, which can improve the quality of the recovered alloy and reduce the production cost of the alloy.
[0081] The above are only preferred embodiments of the present application and are not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application should be included in the protection scope of the present application.
Claims
1. A refined slag system, characterized in that: Its components, by mass fraction, include 40% to 55% Al2O3, 20% to 30% SiO2, 16% to 22% K2O, 3% to 10% Na2O, and 2% to 4% CaO.
2. The refined slag system according to claim 1, characterized in that: Its components, by mass fraction, include 40% to 50% Al2O3, 20% to 30% SiO2, 16% to 19% K2O, 8% to 10% Na2O, and 2% to 4% CaO.
3. The refined slag system according to claim 1, characterized in that: Based on the total mass of the refined slag system, it satisfies at least one of the following conditions: (1) The total content of MgO and TiO2 is not more than 0.5%; (2) The carbon content is not more than 0.03%; (3) The phosphorus content is not more than 0.01%; (4) The sulfur content is not more than 0.005%.
4. The refined slag system according to claim 1, characterized in that: The refined slag is in granular form, and the average particle size of the refined slag is not greater than 10 mm.
5. The refined slag system according to claim 4, characterized in that: In the refined slag system, based on the total mass of the refined slag system, the particle size is 5mm-10mm accounting for 25%-35%, the particle size is greater than 0.5mm and less than 5mm accounting for 60%-74%, and the particle size is not greater than 0.5mm accounting for 1%-5%.
6. A method for preparing the refined slag system according to claim 1, characterized in that: It includes the following steps: The mixed material is ball-milled, and then melted, cooled and crushed in sequence; the mixed material includes 40% to 55% Al2O3, 20% to 30% SiO2, 16% to 22% K2O, 3% to 10% Na2O, and 2% to 4% CaO by mass fraction.
7. The method for preparing a refined slag system according to claim 6, characterized in that: The mixture satisfies at least one of the following conditions: (1) The average particle size of Al2O3 is not greater than 3 mm; (2) The average particle size of the TiO2 is not greater than 3 mm; (3) the average particle size of the Na2O is not greater than 4 mm; (4) The average particle size of the CaO is not greater than 3 mm.
8. Use of the refined slag system according to any one of claims 1 to 5 in the return material of vacuum refining FGH97 alloy.
9. The use according to claim 8, characterized in that: During refining, the mass ratio of the Li refining slag system to the FGH97 alloy return material is 0.5:1 to 2:
1.
10. The use according to claim 8, characterized in that: The vacuum refining time is 60 to 120 minutes; and / or, The vacuum degree during refining is 20~100Pa.
Citation Information
Patent Citations
Novel casting powder and application thereof
CN104439133A
Refining slag for reducing aluminum loss in VD refining process as well as preparation method and application of refining slag
CN118006867A
Method for desulfurizing steel
JP2012001779A
The additive made of al-dross for desulfurizing
KR1020060002117A