Copper oxide / indium oxide nanoparticle electro-catalytic material as well as preparation method and application thereof

Through the synergistic action of copper oxide/indium oxide nanoparticle electrocatalytic materials, the carbon-carbon coupling reaction is inhibited, and the selectivity of carbon dioxide reduction to carbon monoxide is improved, and the problem of insufficient carbon dioxide reduction selectivity in the prior art is solved, thus achieving efficient Carbon dioxide reduction efficiency.

CN119020808APending Publication Date: 2024-11-26CHINA UNIV OF GEOSCIENCES (WUHAN)
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411112553.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Existing electrocatalytic materials have poor selectivity in the carbon dioxide reduction process, mainly due to the competitive hydrogen precipitation reaction (HER), resulting in insufficient selectivity for specific products.

Method used

Copper oxide/indium oxide nanoparticle electrocatalytic material is used to synergistically inhibit the carbon-carbon coupling reaction through the recombination of copper oxide and indium oxide, thereby improving the desorption of carbon dioxide intermediates and enhancing the selectivity to carbon monoxide. The material is synthesized by wet chemical method, reacted with sodium hydroxide solution with indium copper metal precursor solution, and calcined at high temperature to form hydrophobic nanoparticles.

Benefits of technology

The selectivity of carbon dioxide reduction to carbon monoxide is significantly improved, and the carbon dioxide reduction efficiency of electrocatalytic materials reaches 97%, and the process is simple and easy to operate, making it suitable for large-scale industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119020808A_ABST
    Figure CN119020808A_ABST
Patent Text Reader

Abstract

The invention discloses a copper oxide / indium oxide nanoparticle electro-catalytic material as well as a preparation method and application thereof. The invention relates to the technical field of electro-catalysis. The preparation method comprises the following steps: dropwise adding a sodium hydroxide solution into an indium-copper metal precursor solution with indium ions and copper ions, sufficiently stirring the obtained solution, then putting the solution into a water bath, sufficiently stirring, centrifugally washing, drying in vacuum, and calcining at high temperature to obtain the indium oxide / copper oxide nano-particle electro-catalytic material. According to the invention, indium-doped copper oxide nanoparticles are synthesized by a wet chemical method, and the indium-doped copper oxide nanoparticles are further calcined in an air atmosphere to synthesize the hydrophobic copper oxide / indium oxide nanoparticle electro-catalytic material. The carbon-carbon coupling reaction on the copper oxide catalyst can be inhibited through the synergistic effect between indium oxide and copper oxide, desorption of a carbon dioxide intermediate is greatly promoted, the yield of carbon monoxide is increased due to existence of copper oxide, and the selectivity of reduction of carbon dioxide into carbon monoxide of the electro-catalytic material is greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of electrocatalysis technology, and in particular to a copper oxide / indium oxide nanoparticle electrocatalytic material and a preparation method and application thereof. Background Art

[0002] Carbon dioxide emissions have increased due to the consumption of fossil fuels, so the neutralization and utilization of carbon dioxide has become a pressing issue. As a clean and efficient energy conversion process, electrocatalytic reduction can convert carbon dioxide into a series of alcohol and organic acid molecules, effectively realizing the utilization and conversion of carbon dioxide. Among the different products of electrocatalytic carbon dioxide reduction, the conversion of carbon dioxide to carbon monoxide is considered to be one of the most promising reactions in the chemical industry due to its technical and economic feasibility. The reduced product carbon monoxide is the main component of syngas and various gases and fuels. The regulation of the selectivity of the electrocatalytic carbon dioxide reduction products is crucial, and the performance of carbon dioxide reduction mainly depends on the catalytic material. However, the thermodynamic redox potentials of different products of electrocatalytic carbon dioxide reduction are close, resulting in poor selectivity for specific products, mainly due to the competing hydrogen evolution reaction (HER). Therefore, in electrochemical carbon dioxide reduction, it is crucial to adjust the selectivity of the electrocatalyst to obtain the desired product. Summary of the invention

[0003] The purpose of the present invention is to address the above-mentioned deficiencies in the prior art and to provide a copper oxide / indium oxide nanoparticle electrocatalytic material and a preparation method and application thereof. The synthesized electrocatalytic material has good hydrophobicity. Through the composite of copper oxide and indium oxide, the synergistic effect between indium oxide and copper oxide inhibits the carbon-carbon coupling process, greatly promotes the desorption of carbon dioxide intermediates, and greatly improves the selectivity of the copper oxide / indium oxide nanoparticle electrocatalytic material for reducing carbon dioxide to carbon monoxide.

[0004] The invention discloses a method for preparing a copper oxide / indium oxide nanoparticle electrocatalytic material. The method comprises the following steps: dripping a sodium hydroxide solution into an indium copper metal precursor solution containing indium ions and copper ions, fully stirring the obtained solution, placing the solution in a water bath for full stirring, centrifugation washing, vacuum drying, and high-temperature calcination to obtain the indium oxide / copper oxide nanoparticle electrocatalytic material.

[0005] Furthermore, the molar ratio of copper ions to indium ions is 100:1-10.

[0006] Furthermore, the amount of sodium hydroxide added is such that the indium ions and the copper ions completely generate hydroxides.

[0007] Furthermore, the high temperature calcination temperature is 550-850°C, and the calcination time is 3-5h.

[0008] Furthermore, the water bath temperature is 55-70° C., and the water bath stirring time is 2-4 h.

[0009] Furthermore, the obtained solution is fully stirred for 5-10 minutes.

[0010] Furthermore, the preparation method of the precursor solution having indium ions and copper ions is as follows: a certain amount of copper acetate monohydrate and deionized water are stirred and mixed, a certain amount of indium chloride tetrahydrate and deionized water are stirred and mixed, and after stirring, the indium chloride tetrahydrate solution is dropped into the copper acetate monohydrate solution to obtain a composite solution, and the above composite solution is fully stirred to form an indium copper metal precursor solution.

[0011] Furthermore, the preparation method of the precursor solution containing indium ions and copper ions is as follows: the stirring time of copper acetate monohydrate and deionized water is 5-10 minutes, the stirring time of indium chloride tetrahydrate and deionized water is 5-10 minutes, and the stirring time of the composite solution is 10-20 minutes.

[0012] A copper oxide / indium oxide nanoparticle electrocatalytic material prepared by the above-mentioned preparation method.

[0013] An application of the copper oxide / indium oxide nanoparticle electrocatalytic material as described above in electrocatalyzing carbon dioxide to produce carbon monoxide.

[0014] Copper oxide is a carbon dioxide reduction catalyst with excellent performance. The intermediates adsorbed and activated on the surface of copper oxide tend to undergo carbon-carbon coupling reactions, thereby generating multi-carbon products such as (ethylene, ethanol, ethane, etc.). Indium oxide is a new N-type transparent semiconductor functional material with a wide band gap, a small resistivity and a high catalytic activity. The present invention synthesizes indium-doped copper oxide nanoparticles by a wet chemical method, and further calcines and synthesizes copper oxide / indium oxide nanoparticle electrocatalytic materials with good hydrophobicity in an air atmosphere. Hydrophobicity can increase the carbon dioxide concentration at the solid-liquid interface of the catalyst, thereby improving the selectivity of carbon dioxide reduction. The synergistic effect between indium oxide and copper oxide can inhibit the carbon-carbon coupling reaction on the copper oxide catalyst, greatly promoting the desorption of carbon dioxide intermediates, and the presence of copper oxide increases the yield of carbon monoxide, greatly improving the selectivity of carbon dioxide reduction to carbon monoxide in the copper oxide / indium oxide nanoparticle electrocatalytic material.

[0015] In addition, the synthesis process of copper oxide / indium oxide nanoparticle electrocatalytic materials is simple and easy to operate, does not require expensive high-precision equipment, has reliable repeatability, and has low production costs, making it very suitable for large-scale industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1This is a scanning electron microscope image of the copper oxide / indium oxide nanoparticles prepared in Example 1;

[0017] Figure 2 This is a contact angle diagram of the copper oxide / indium oxide nanoparticles prepared in Example 1;

[0018] Figure 3 This is a scanning electron microscope image of the copper oxide nanoparticles prepared in Comparative Example 1;

[0019] Figure 4 This is a diagram of the electrocatalytic Faraday efficiency of the copper oxide / indium oxide nanoparticle electrocatalytic material prepared in Example 1;

[0020] Figure 5 The X-ray diffraction patterns of Example 1, Comparative Example 1 and Comparative Example 2 are shown in FIG.

[0021] Figure 6 The Raman spectra of Examples 1-3 and Comparative Example 1 are shown below;

[0022] Figure 7 This is a comparison chart of the Faraday efficiencies of the electrocatalytic reduction of carbon dioxide to produce carbon monoxide in Example 1 and Comparative Examples 1-3;

[0023] Figure 8 A comparison chart of the Faraday efficiencies of the electrocatalytic reduction of carbon dioxide to produce carbon monoxide in Examples 1-5 and Comparative Examples 1-3;

[0024] Fig. 9 This is a scanning electron microscope image of the copper oxide / indium oxide nanoparticles prepared in Example 2;

[0025] Fig.10 This is a scanning electron microscope image of the copper oxide / indium oxide nanoparticles prepared in Example 3;

[0026] Fig.11 This is a scanning electron microscope image of the copper oxide / indium oxide nanoparticles prepared in Example 4;

[0027] Fig.12 This is a scanning electron microscope image of the copper oxide / indium oxide nanoparticles prepared in Example 5. DETAILED DESCRIPTION

[0028] The following are specific embodiments of the present invention and the accompanying drawings to further describe the technical solution of the present invention, but the present invention is not limited to these embodiments.

[0029] Example 1

[0030] A method for preparing a copper oxide / indium oxide nanoparticle electrocatalyst comprises the following steps:

[0031] (1) preparing an indium copper metal precursor solution: stirring and mixing 1.99 g of copper acetate monohydrate and 25 mL of deionized water, stirring and mixing 0.147 g of indium chloride tetrahydrate and 25 mL of deionized water, and after stirring, dropping the indium chloride tetrahydrate solution into the copper acetate monohydrate solution to obtain a composite solution, and fully stirring the composite solution to form an indium copper metal precursor solution;

[0032] (2) Preparation of indium-doped copper oxide nanoparticles: 100 ml of 2 mol / L sodium hydroxide solution was dripped dropwise into the indium copper metal precursor solution obtained in step S1, the obtained solution was fully stirred, and placed in a 60° C. water bath for 3 h, and indium-doped copper oxide nanoparticles were obtained after centrifugal washing and vacuum drying;

[0033] (3) Preparation of copper oxide / indium oxide nanoparticle electrocatalytic material: The indium-doped copper oxide nanoparticles obtained in S2 were placed in a porcelain boat, and the porcelain boat was placed in a muffle furnace. The copper oxide / indium oxide nanoparticle electrocatalytic material was obtained after calcining at 700°C for 4 hours in an air atmosphere.

[0034] Example 2

[0035] A method for preparing a copper oxide / indium oxide nanoparticle electrocatalyst comprises the following steps:

[0036] (1) preparing an indium copper metal precursor solution: stirring and mixing 1.99 g of copper acetate monohydrate and 25 mL of deionized water, stirring and mixing 0.03 g of indium chloride tetrahydrate and 25 mL of deionized water, and after stirring, dropping the indium chloride tetrahydrate solution into the copper acetate monohydrate solution to obtain a composite solution, and fully stirring the composite solution to form an indium copper metal precursor solution;

[0037] (2) Preparation of indium-doped copper oxide nanoparticles: 100 ml of 2 mol / L sodium hydroxide solution was dripped dropwise into the indium copper metal precursor solution obtained in step S1, the obtained solution was fully stirred, and placed in a 60° C. water bath for 3 h, and indium-doped copper oxide nanoparticles were obtained after centrifugal washing and vacuum drying;

[0038] (3) Preparation of copper oxide / indium oxide nanoparticle electrocatalytic material: The indium-doped copper oxide nanoparticles obtained in S2 were placed in a porcelain boat, and the porcelain boat was placed in a muffle furnace. The copper oxide / indium oxide nanoparticle electrocatalytic material was obtained after calcining at 700°C for 4 hours in an air atmosphere.

[0039] Example 3

[0040] A method for preparing a copper oxide / indium oxide nanoparticle electrocatalyst comprises the following steps:

[0041] (1) preparing an indium copper metal precursor solution: stirring and mixing 1.99 g of copper acetate monohydrate and 25 mL of deionized water, stirring and mixing 0.3 g of indium chloride tetrahydrate and 25 mL of deionized water, and after stirring, dropping the indium chloride tetrahydrate solution into the copper acetate monohydrate solution to obtain a composite solution, and fully stirring the composite solution to form an indium copper metal precursor solution;

[0042] (2) Preparation of indium-doped copper oxide nanoparticles: 100 ml of 2 mol / L sodium hydroxide solution was dripped dropwise into the indium copper metal precursor solution obtained in step S1, the obtained solution was fully stirred, and placed in a 60° C. water bath for 3 h, and indium-doped copper oxide nanoparticles were obtained after centrifugal washing and vacuum drying;

[0043] (3) Preparation of copper oxide / indium oxide nanoparticle electrocatalytic material: The indium-doped copper oxide nanoparticles obtained in S2 were placed in a porcelain boat, and the porcelain boat was placed in a muffle furnace. The copper oxide / indium oxide nanoparticle electrocatalytic material was obtained after calcining at 700°C for 4 hours in an air atmosphere.

[0044] Example 4

[0045] A method for preparing a copper oxide / indium oxide nanoparticle electrocatalyst comprises the following steps:

[0046] (1) preparing an indium copper metal precursor solution: stirring and mixing 1.99 g of copper acetate monohydrate and 25 mL of deionized water, stirring and mixing 0.147 g of indium chloride tetrahydrate and 25 mL of deionized water, and after stirring, dropping the indium chloride tetrahydrate solution into the copper acetate monohydrate solution to obtain a composite solution, and fully stirring the composite solution to form an indium copper metal precursor solution;

[0047] (2) Preparation of indium-doped copper oxide nanoparticles: 100 ml of 2 mol / L sodium hydroxide solution was dripped dropwise into the indium copper metal precursor solution obtained in step S1, the obtained solution was fully stirred, and placed in a 60° C. water bath for 3 h, and indium-doped copper oxide nanoparticles were obtained after centrifugal washing and vacuum drying;

[0048] (3) Preparation of copper oxide / indium oxide nanoparticle electrocatalytic material: The indium-doped copper oxide nanoparticles obtained in S2 were placed in a porcelain boat, and the porcelain boat was placed in a muffle furnace. The copper oxide / indium oxide nanoparticle electrocatalytic material was obtained after calcining at 550°C for 4 hours in an air atmosphere.

[0049] Example 5

[0050] A method for preparing a copper oxide / indium oxide nanoparticle electrocatalyst comprises the following steps:

[0051] (1) preparing an indium copper metal precursor solution: stirring and mixing 1.99 g of copper acetate monohydrate and 25 mL of deionized water, stirring and mixing 0.147 g of indium chloride tetrahydrate and 25 mL of deionized water, and after stirring, dropping the indium chloride tetrahydrate solution into the copper acetate monohydrate solution to obtain a composite solution, and fully stirring the composite solution to form an indium copper metal precursor solution;

[0052] (2) Preparation of indium-doped copper oxide nanoparticles: 100 ml of 2 mol / L sodium hydroxide solution was dripped dropwise into the indium copper metal precursor solution obtained in step S1, the obtained solution was fully stirred, and placed in a 60° C. water bath for 3 h, and indium-doped copper oxide nanoparticles were obtained after centrifugal washing and vacuum drying;

[0053] (3) Preparation of copper oxide / indium oxide nanoparticle electrocatalytic material: The indium-doped copper oxide nanoparticles obtained in S2 were placed in a porcelain boat, the porcelain boat was placed in a muffle furnace, and the copper oxide / indium oxide nanoparticle electrocatalytic material was obtained after calcination at 850°C for 4 hours in an air atmosphere.

[0054] Comparative Example 1

[0055] A method for preparing a copper oxide nanoparticle electrocatalyst comprises the following steps:

[0056] (1) Preparation of copper hydroxide precursor solution: 2.09 g (CH 3 COO 2 Cu·H 2 O was dispersed in 25 ml of deionized water and stirred for 10 min, and then 100 ml of 2 mol / L sodium hydroxide solution was added dropwise into the copper salt solution to prepare a copper hydroxide precursor solution;

[0057] (2) Preparation of copper oxide catalyst: The copper hydroxide precursor solution was transferred to a 60°C water bath and stirred for 3 h. The obtained precipitate was dispersed, centrifuged, washed, and vacuum dried to obtain a black powder. The black powder was calcined at 700°C for 4 h in an air atmosphere to obtain a copper oxide nanoparticle electrocatalyst.

[0058] Comparative Example 2

[0059] A method for preparing an indium oxide electrocatalytic material comprises the following steps:

[0060] (1) Preparation of indium salt precursor solution: 3.08 g InCl·4H 2 O was dispersed in 25 ml of deionized water and stirred for 10 min, and then 100 ml of 2 mol / L sodium hydroxide solution was dripped into the indium salt solution drop by drop to prepare an indium salt precursor solution;

[0061] (2) Preparation of indium oxide catalyst: The indium salt precursor solution was transferred to a 60°C water bath and stirred for 3 h. The obtained precipitate was dispersed, centrifuged, washed and vacuum dried to obtain a light yellow powder. The light yellow powder was calcined at 700°C for 4 h in an air atmosphere to obtain an indium oxide nanoparticle electrocatalyst.

[0062] Comparative Example 3

[0063] A cuprous oxide electrocatalytic material comprising the following steps:

[0064] (1) Preparation of copper hydroxide precursor solution: 0.75 g (CH 3 COO 2 Cu·H 2 O, 0.37g of sodium citrate dihydrate was dispersed in 200ml of deionized water and stirred for 15min, and then 50ml of 1.25mol / L sodium hydroxide solution was dripped into the solution drop by drop to prepare a copper hydroxide precursor solution;

[0065] (2) Preparation of cuprous oxide catalyst: 125 ml of 0.03 mol / L ascorbic acid solution was added dropwise to the copper hydroxide precursor solution, stirred for 3 min and allowed to settle for 1 h. The brick-red precipitate obtained was dispersed, centrifuged, washed, and vacuum dried to obtain the cuprous oxide electrocatalytic material.

[0066] The scanning electron microscope image of the copper oxide / indium oxide nanoparticles (prepared by S3) prepared in Example 1 is obtained, and the result is as follows: Figure 1 As shown in the figure, it can be seen that the preparation method of Example 1 can obtain irregularly shaped copper oxide / indium oxide nanoparticles;

[0067] Figure 2 This is a contact angle diagram of the copper oxide / indium oxide nanoparticles prepared in Example 1. The prepared copper oxide / indium oxide nanoparticles have good hydrophobicity, which can increase the carbon dioxide concentration at the solid-liquid interface of the catalyst, thereby improving the selectivity of carbon dioxide reduction.

[0068] Figure 3 This is a scanning electron microscope image of the copper oxide nanoparticles prepared in Comparative Example 1. The copper oxide nanoparticles are more likely to undergo carbon-carbon coupling reactions, generating multi-carbon products such as ethanol and ethane.

[0069] Figure 4 This is the electrocatalytic Faraday efficiency diagram of the copper oxide / indium oxide nanoparticle electrocatalytic material prepared in Example 1. As can be seen from the figure, the copper oxide / indium oxide nanoparticle electrocatalytic material prepared in Example 1 has an extremely high efficiency of electrocatalytic carbon dioxide reduction to produce carbon monoxide, and a high selectivity for electrocatalytic carbon dioxide reduction, up to 97%.

[0070] Figure 5 2 are X-ray diffraction patterns of the electrocatalytic materials of Example 1 and Comparative Examples 1 and 2. It can be seen from the figure that the copper oxide / indium oxide nanoparticle electrocatalytic material prepared in Example 1 shows obvious characteristic peaks of copper oxide and indium oxide, proving the successful preparation of the indium oxide / copper oxide nanoparticle electrocatalytic material.

[0071] Figure 6 The Raman spectra of the electrocatalytic materials of Examples 1-3 and Comparative Example 1 show that the characteristic peak of copper oxide and the characteristic peak of In—O appear at the same time, proving the successful preparation of the copper oxide / indium oxide nanoparticle electrocatalytic material.

[0072] Figure 7 The Faraday efficiency of the electrocatalytic reduction of carbon dioxide to produce carbon monoxide was tested for the electrocatalytic materials of Example 1 and Comparative Examples 1-3 at different voltages. It can be seen from the figure that the efficiency of the electrocatalytic reduction of carbon dioxide to produce carbon monoxide in Example 1 is the highest, reaching 97%.

[0073] The copper oxide / indium oxide nanoparticle electrocatalysts prepared in Examples 1-5 were tested for their activity in electrocatalytic reduction of carbon dioxide, wherein the molar ratio of copper salt to indium salt and the high-temperature calcination temperature were different.

[0074] Figure 8 The Faraday efficiency of the electrocatalytic reduction of carbon dioxide to produce carbon monoxide was tested for the electrocatalytic materials of Examples 1-5 and Comparative Examples 1-3 at a voltage of -0.6V. It can be seen from the figure that under this method, the electrocatalytic materials obtained have better performance at different molar ratios of copper salt to indium salt in the metal precursor solution and at different high-temperature calcination temperatures, which are better than the performance of Comparative Examples 1-3, proving that the introduction of indium oxide can greatly improve the selectivity of carbon monoxide. Among them, the copper oxide / indium oxide nanoparticle electrocatalytic material prepared in Example 1 has the highest carbon dioxide reduction reaction activity, and the efficiency of electrocatalytic carbon dioxide reduction to produce carbon monoxide reaches 97%.

[0075] Among them, the scanning electron microscope image of the copper oxide / indium oxide nanoparticle electrocatalyst prepared from Examples 1-3 ( Figure 1 , Fig. 9 and Fig.10 ) It can be seen that when the indium oxide doping amount is small, the synergistic effect between indium oxide and copper oxide is weak and insufficient to promote the desorption of carbon dioxide intermediates. When the doping amount is too large, the synergistic effect between copper oxide and indium oxide is too strong, resulting in a decrease in carbon monoxide selectivity, so the reaction activity of Examples 2 and 3 is lower than that of Example 1.

[0076] Scanning electron microscope images of the copper oxide / indium oxide nanoparticle electrocatalysts prepared from Examples 1, 4, and 5 ( Figure 1 , Fig.11 and Fig.12 ) It can be seen that when the calcination temperature is 550°C, the degree of crystallization of the oxide is poor. When the calcination temperature is increased to 850°C, the boiling point of indium oxide is reached, and the structure of the copper oxide / indium oxide nanoparticles is destroyed, so the reaction activity of Examples 4 and 5 is lower than that of Example 1.

[0077] For matters not mentioned above, the prior art applies.

[0078] Although some specific embodiments of the present invention have been described in detail through examples, those skilled in the art should understand that the above examples are for illustration only and are not intended to limit the scope of the present invention. Those skilled in the art to which the present invention belongs may make various modifications or supplements to the specific embodiments described or replace them in a similar manner, but they will not deviate from the direction of the present invention or exceed the scope defined by the attached claims. Those skilled in the art should understand that any modifications, equivalent substitutions, improvements, etc. made to the above embodiments based on the technical essence of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a copper oxide / indium oxide nanoparticle electrocatalytic material, characterized by: A sodium hydroxide solution is dropped into an indium-copper metal precursor solution containing indium ions and copper ions, and the resulting solution is fully stirred. The solution is then placed in a water bath and fully stirred. After centrifugal washing, vacuum drying, and high-temperature calcination, an indium oxide / copper oxide nanoparticle electrocatalytic material is obtained.

2. The preparation method according to claim 1, wherein: The molar ratio of copper ions to indium ions is 100:1-10.

3. The preparation method according to claim 1, wherein: The amount of sodium hydroxide added is such that the indium ions and the copper ions completely generate hydroxides.

4. The preparation method according to claim 1, wherein: The high temperature calcination temperature is 550-850°C, and the calcination time is 3-5h.

5. The preparation method according to claim 1, wherein: The water bath temperature is 55-70°C, and the water bath stirring time is 2-4h.

6. The preparation method according to claim 1, wherein: The obtained solution was stirred thoroughly for 5-10 minutes.

7. The preparation method according to claim 1, wherein: The preparation method of the precursor solution containing indium ions and copper ions is as follows: a certain amount of copper acetate monohydrate and deionized water are stirred and mixed, a certain amount of indium chloride tetrahydrate and deionized water are stirred and mixed, and after stirring, the indium chloride tetrahydrate solution is dropped into the copper acetate monohydrate solution to obtain a composite solution, and the composite solution is fully stirred to form an indium copper metal precursor solution.

8. The preparation method according to claim 7, wherein: The preparation method of the precursor solution containing indium ions and copper ions is as follows: copper acetate monohydrate and deionized water are stirred for 5-10 minutes, indium chloride tetrahydrate and deionized water are stirred for 5-10 minutes, and the composite solution is stirred for 10-20 minutes.

9. A copper oxide / indium oxide nanoparticle electrocatalytic material prepared by the preparation method according to any one of claims 1 to 8.

10. Use of the copper oxide / indium oxide nanoparticle electrocatalytic material according to claim 9 in electrocatalytic production of carbon monoxide from carbon dioxide.

Citation Information

Cited By

  • Indium-doped copper oxide electrode for electrocatalytic reduction of CO2 and preparation method of indium-doped copper oxide electrode