Anti-reflection device, and preparation method and application of anti-reflection device

By introducing porous metal-based organic hybrid films and metal oxide films alternately stacked in the antireflection film layer, the problem of complex structure of traditional antireflection films is solved, and a simplified process and wide application of low reflectivity are realized.

CN119024467APending Publication Date: 2024-11-26JIANGSU MICROVIA NANO EQUIP TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411234192.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Traditional antireflective coatings have complex structures, requiring multiple layers of thin films to achieve low reflectivity, resulting in high manufacturing complexity.

Method used

A metal-based organic hybrid film with a porous structure is used as an antireflection enhancement layer. It is prepared by molecular layer deposition and combined with alternating layers of metal oxide films to simplify the film structure.

Benefits of technology

While maintaining low reflectivity, it reduces the number of film layers required for antireflective substrates, simplifies the process, and achieves adjustable refractive index by controlling porosity and pore size, thus broadening the application range.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119024467A_ABST
    Figure CN119024467A_ABST
Patent Text Reader

Abstract

The invention provides an antireflection device, and a preparation method and application of the antireflection device. The anti-reflection device comprises a substrate and an anti-reflection film layer structure arranged on the substrate in a stacked mode, the anti-reflection film layer structure comprises an anti-reflection base layer and an anti-reflection enhancement layer arranged on the anti-reflection base layer in a stacked mode, and the anti-reflection enhancement layer comprises a metal-based organic hybrid film of a porous structure. The metal-based organic hybrid film can enhance the anti-reflection effect of the anti-reflection base layer, so that the number of film layers required in the anti-reflection base layer is reduced while the low reflectivity of the device is maintained, and the structure of the anti-reflection base layer is simplified.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of anti-reflection films, and in particular to an anti-reflection device, a preparation method of the anti-reflection device and an application thereof. Background Art

[0002] Anti-reflection film is also called anti-reflection film. Its main function is to eliminate reflected light from the surface of devices such as lenses, prisms and plane mirrors, increase the light transmittance of the device, and reduce or eliminate the stray light of the system.

[0003] Anti-reflection film mainly uses the principle of interference and destructiveness of light, and matches the refractive index of different materials, thickness design, and the selection of special materials to achieve the reduction of reflected light and the increase of transmitted light. A major feature of this optical anti-reflection film is that if you want to obtain a lower reflectivity, you often need a large number of thin films to form a stacked structure. For example, in some traditional technologies, if you want to reduce the reflectivity of the lens to below 0.5%, you need to use a stacked structure consisting of more than 9 layers of thin films. Therefore, the structure of the anti-reflection film in traditional technology is usually more complicated. Summary of the invention

[0004] Based on this, it is necessary to provide an anti-reflection device in which the anti-reflection film layer structure can be simplified in order to solve the problems in the above-mentioned background technology.

[0005] According to some embodiments of the present disclosure, an anti-reflection device is provided, comprising a substrate and an anti-reflection film layer structure stacked on the substrate, the anti-reflection film layer structure comprising an anti-reflection base layer and an anti-reflection enhancement layer stacked on the anti-reflection base layer, the anti-reflection enhancement layer comprising a metal-based organic hybrid film with a porous structure.

[0006] In some embodiments of the present disclosure, the anti-reflection enhancement layer is the metal-based organic hybrid film; or,

[0007] The anti-reflection enhancement layer comprises at least one layer of the metal-based organic hybrid film and at least one layer of metal oxide film, the material of the metal oxide film comprises metal oxide, and the metal-based organic hybrid film and the metal oxide film are alternately stacked.

[0008] In some embodiments of the present disclosure, the material of the metal oxide film includes one or more of aluminum oxide, zinc oxide and titanium oxide.

[0009] In some embodiments of the present disclosure, the overall equivalent refractive index of the anti-reflection enhancement layer is 1.2-1.5.

[0010] In some embodiments of the present disclosure, the anti-reflection enhancement layer satisfies at least one of the following features:

[0011] (1) The thickness of the anti-reflection enhancement layer is 10nm~200nm;

[0012] (2) The pore size of the pores in the anti-reflection enhancement layer is 1 nm to 30 nm;

[0013] (3) The porosity of the anti-reflection enhancement layer is 10% to 70%.

[0014] In some embodiments of the present disclosure, the material of the metal-based organic hybrid film includes one or more of an aluminum-based hydroquinone hybrid material, a zinc-based hydroquinone hybrid material, and a titanium-based hydroquinone hybrid material.

[0015] In some embodiments of the present disclosure, the metal-based organic hybrid film is prepared by molecular layer deposition.

[0016] In some embodiments of the present disclosure, the raw materials for preparing the metal-based organic hybrid film include a first metal precursor and an organic precursor; wherein,

[0017] The first metal precursor is selected from one or more of trimethylaluminum, ethylene dizinc and titanium tetrachloride, and the organic precursor is selected from hydroquinone.

[0018] In some embodiments of the present disclosure, the anti-reflection base layer includes a high refractive index film and a low refractive index film, and the refractive index of the high refractive index film is higher than the refractive index of the low refractive index film;

[0019] The high refractive index film and the low refractive index film each have at least one layer, and the high refractive index film and the low refractive index film are alternately stacked.

[0020] In some embodiments of the present disclosure, the total number of film layers of the high refractive index film and the low refractive index film is 2 to 4 layers.

[0021] In some embodiments of the present disclosure, the average reflectivity of the anti-reflection film layer structure for light in the 400nm~800nm ​​band is less than 0.2%.

[0022] In a second aspect, the present disclosure also provides a method for preparing the above anti-reflection device, which provides a substrate;

[0023] Preparing an anti-reflection base layer on the substrate;

[0024] The substrate is placed in a deposition chamber, and an anti-reflection enhancement layer is prepared on the substrate, wherein the step of preparing the anti-reflection enhancement layer includes: depositing the metal-based organic hybrid film having a porous structure.

[0025] In some embodiments of the present disclosure, the material of the metal-based organic hybrid film includes one or more of an aluminum-based hydroquinone hybrid material, a zinc-based hydroquinone hybrid material, and a titanium-based hydroquinone hybrid material.

[0026] In some embodiments of the present disclosure, the metal-based organic hybrid material is deposited by molecular layer deposition.

[0027] In some embodiments of the present disclosure, the step of preparing the anti-reflection enhancement layer further includes depositing to form a metal oxide film, and the step of depositing to form a metal-based organic hybrid film and the step of depositing to form a metal oxide film are performed alternately.

[0028] In some embodiments of the present disclosure, the step of depositing a metal-based organic hybrid film includes: introducing a first metal precursor into a deposition chamber and attaching it to the substrate to form a first monolayer, introducing an organic precursor into the deposition chamber and attaching it to the substrate to form a second monolayer;

[0029] The step of depositing the metal oxide material includes: introducing a second metal precursor into the deposition chamber and attaching it to the substrate to form a third monolayer, introducing an oxidant into the deposition chamber and attaching it to the substrate to form a fourth monolayer;

[0030] The steps of forming the first monolayer and the steps of forming the second monolayer are taken as a first deposition cycle, and the steps of forming the third monolayer and the steps of forming the fourth monolayer are taken as a second deposition cycle;

[0031] At least one first deposition cycle is continuously performed to form a metal-based organic hybrid film, and at least one second deposition cycle is continuously performed to form a metal oxide film, and at least one metal-based organic hybrid film and at least one metal oxide film are alternately formed.

[0032] In some embodiments of the present disclosure, the first metal precursor is selected from one or more of trimethylaluminum, ethylene dizinc and titanium tetrachloride, and the organic precursor is selected from hydroquinone; and / or,

[0033] The second metal precursor is selected from one or more of trimethylaluminum, ethylene dizinc and titanium tetrachloride, and the oxidant is selected from one or more of water and oxygen.

[0034] In some embodiments of the present disclosure, a ratio of the number of times the first deposition cycle is performed to the number of times the second deposition cycle is performed is 1:(1-5).

[0035] In some embodiments of the present disclosure, the number of the first deposition cycles is 40 to 500 times.

[0036] In some embodiments of the present disclosure, in the step of depositing the metal-based organic hybrid film, the temperature of the deposition chamber is controlled to be 150° C. to 300° C.

[0037] In some embodiments of the present disclosure, the step of preparing an anti-reflection base layer on the substrate includes:

[0038] A high refractive index film and a low refractive index film are alternately deposited on the substrate, wherein the refractive index of the high refractive index film is higher than that of the low refractive index film, and each of the high refractive index film and the low refractive index film has at least one layer.

[0039] In a third aspect, the present disclosure also provides an application of a metal-based organic hybrid film in an anti-reflection film layer structure, wherein the anti-reflection film layer structure comprises an anti-reflection enhancement layer, wherein the anti-reflection enhancement layer comprises the metal-based organic hybrid film, and the metal-based organic hybrid film has a porous structure.

[0040] In some embodiments of the present disclosure, the metal-based organic hybrid film constitutes the anti-reflection enhancement layer; or,

[0041] The anti-reflection enhancement layer comprises at least one layer of the metal-based organic hybrid film and at least one layer of metal oxide film, the material of the metal oxide film comprises metal oxide, and the metal-based organic hybrid film and the metal oxide film are alternately stacked.

[0042] In some embodiments of the present disclosure, the overall equivalent refractive index of the anti-reflection enhancement layer is 1.2-1.5.

[0043] In some embodiments of the present disclosure, the anti-reflection enhancement layer satisfies at least one of the following features:

[0044] (1) The thickness of the anti-reflection enhancement layer is 10nm~200nm;

[0045] (2) The pore size of the pores in the anti-reflection enhancement layer is 1 nm to 30 nm;

[0046] (3) The porosity of the anti-reflection enhancement layer is 10% to 70%.

[0047] In some embodiments of the present disclosure, the material of the metal-based organic hybrid film includes one or more of an aluminum-based hydroquinone hybrid material, a zinc-based hydroquinone hybrid material, and a titanium-based hydroquinone hybrid material.

[0048] In some embodiments of the present disclosure, the material of the metal-based organic hybrid film includes one or more of an aluminum-based hydroquinone hybrid material, a zinc-based hydroquinone hybrid material, and a titanium-based hydroquinone hybrid material.

[0049] In some embodiments of the present disclosure, the metal-based organic hybrid film is prepared by molecular layer deposition.

[0050] In some embodiments of the present disclosure, the raw materials for preparing the metal-based organic hybrid film include a first metal precursor and an organic precursor; wherein,

[0051] The first metal precursor is selected from one or more of trimethylaluminum, ethylene dizinc and titanium tetrachloride, and the organic precursor is selected from hydroquinone.

[0052] The anti-reflection device disclosed in the present invention is provided with an anti-reflection film layer structure, which includes an anti-reflection base layer and an anti-reflection enhancement layer stacked on the anti-reflection base layer. The anti-reflection enhancement layer includes a metal-based organic hybrid film with a porous structure. The applicant found in the research process that the porous structure in the metal-based organic hybrid film can make its refractive index between the refractive index of air and other material layers in the anti-reflection film layer structure, and the pore structure in the metal-based organic hybrid film makes its refractive index have the characteristic of gradually changing with thickness, which is equivalent to the stacking of multiple layers of thin films with different refractive indices. Therefore, the metal-based organic hybrid film can play the role of reducing the reflectivity performance in the traditional technology that requires the provision of multiple layers of thin films. Thanks to the above characteristics, the metal-based organic hybrid film can enhance the anti-reflection effect of the anti-reflection base layer, which is conducive to reducing the number of film layers required in the anti-reflection base layer while maintaining the device with a low reflectivity, thereby simplifying the structure of the anti-reflection base layer.

[0053] Furthermore, in at least some embodiments of the present disclosure, the metal-based organic hybrid film can be prepared by molecular layer deposition, and the desired porous structure can be directly formed during the deposition process. Compared with the traditional multi-layer film design, the metal-based organic hybrid film is used to participate in the formation of the anti-reflection film layer structure, and the overall process is simpler, the process difficulty is low and it is easy to implement.

[0054] In addition, metal-based organic hybrid films can be prepared by molecular layer deposition. By controlling the temperature during the deposition process and the thickness of the metal-based organic hybrid film, or by superimposing other metal oxide films on the pore wall surface of the pores in the metal-based organic hybrid film, the porosity and pore distribution can be regulated, so that the refractive index of the metal-based organic hybrid film can be adjusted. This is conducive to broadening the application scope of metal-based organic hybrid films, so that they can form an anti-reflection film layer structure with extremely low reflectivity when combined with a variety of different anti-reflection base layers.

[0055] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention and implement it according to the contents of the specification, the following is a detailed description of the preferred embodiments of the present invention in conjunction with the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0056] In order to more clearly illustrate the technical solutions of the embodiments of the present disclosure, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present disclosure. For ordinary technicians in this field, drawings of other embodiments can be obtained based on these drawings without creative work.

[0057] Figure 1 is a schematic structural diagram of an anti-reflection device according to an embodiment;

[0058] Figure 2 is a schematic structural diagram of an anti-reflection device according to another embodiment;

[0059] Figure 3 A schematic diagram of a curve showing how the reflectivity of the coated glass in Comparative Example 3 varies with wavelength is shown;

[0060] Figure 4 A schematic diagram of a curve showing how the reflectivity of the coated glass in Example 2.1 and Example 2.2 varies with wavelength is shown.

[0061] The reference numerals and their meanings are as follows:

[0062] 100, substrate; 110, anti-reflection enhancement layer; 120, anti-reflection base layer; 121, high refractive index film; 122, low refractive index film; 200, substrate; 210, anti-reflection enhancement layer; 220, anti-reflection base layer; 221, high refractive index film; 222, low refractive index film. DETAILED DESCRIPTION

[0063] To facilitate understanding of the present invention, a more comprehensive description of the present invention is provided below. The preferred embodiments of the present invention are given herein. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the content of the present invention more thorough and comprehensive.

[0064] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this document pertains. The terms used herein in the specification of this document are only for describing specific embodiments and are not intended to limit this document.

[0065] It should be understood that when an element or layer is referred to as being "on, "adjacent to, "connected to, or "coupled to" another element or layer, it may be directly on, adjacent to, connected to, or coupled to the other element or layer, or there may be intervening elements or layers. In contrast, when an element is referred to as being "directly on, "directly adjacent to, "directly connected to, or "directly coupled to" another element or layer, there may be no intervening elements or layers. It should be understood that although the terms first, second, third, etc. may be used to describe various elements, components, regions, layers, and / or portions, these elements, components, regions, layers, and / or portions should not be limited by these terms. These terms are merely used to distinguish one element, component, region, layer, or portion from another element, component, region, layer, or portion.

[0066] Spatially relative terms such as "under," "beneath," "below," "under," "above," "above," and the like may be used herein for ease of description to describe the relationship of one element or feature to other elements or features. It should be understood that the spatially relative terms are intended to also include different orientations of the device in use and operation. For example, if the device in the accompanying drawings is flipped, then the elements or features described as "under other elements" or "under" or "under" will be oriented as "over" the other elements or features. Thus, the exemplary terms "under" and "under" may include both upper and lower orientations. The device may be otherwise oriented (e.g., rotated 90 degrees or other orientations) and the spatial descriptors used may be interpreted accordingly.

[0067] The purpose of the terms used herein is only to describe specific embodiments and is not intended to be a limitation of the present disclosure. When used herein, the singular forms "a", "an" and "the" are also intended to include plural forms, unless the context clearly indicates otherwise. It should also be understood that the terms "consisting of" and / or "comprising", when used in this specification, determine the presence of features, integers, steps, operations, elements and / or parts, but do not exclude the presence or addition of one or more other features, integers, steps, operations, elements, parts and / or groups. When used herein, the term "and / or" includes any and all combinations of the relevant listed items.

[0068] Traditional anti-reflection films usually need to include multiple layers of thin films, and the reflectivity of light is reduced by changing the refractive index of the multi-layer thin films and corresponding parameters such as thickness.

[0069] The present disclosure provides an anti-reflection device, which includes a substrate and an anti-reflection film layer structure stacked on the substrate, the anti-reflection film layer structure includes an anti-reflection enhancement layer, and the anti-reflection enhancement layer includes a metal-based organic hybrid film with a porous structure.

[0070] The anti-reflection device disclosed in the present invention is provided with an anti-reflection film layer structure, which includes an anti-reflection base layer and an anti-reflection enhancement layer stacked on the anti-reflection base layer. The anti-reflection enhancement layer includes a metal-based organic hybrid film with a porous structure. The applicant found in the research process that the porous structure in the metal-based organic hybrid film can make its refractive index between the refractive index of air and other material layers in the anti-reflection film layer structure, and the pore structure in the metal-based organic hybrid film makes its refractive index have the characteristic of gradually changing with thickness, which is equivalent to the stacking of multiple layers of thin films with different refractive indices. Therefore, the metal-based organic hybrid film can play the role of reducing the reflectivity performance in the traditional technology that requires the provision of multiple layers of thin films. Thanks to the above characteristics, the metal-based organic hybrid film can enhance the anti-reflection effect of the anti-reflection base layer, which is conducive to reducing the number of film layers required in the anti-reflection base layer while maintaining the device with a low reflectivity, thereby simplifying the structure of the anti-reflection base layer.

[0071] Furthermore, in at least some embodiments of the present disclosure, the metal-based organic hybrid film can be prepared by molecular layer deposition, and the desired porous structure can be directly formed during the deposition process. Compared with the traditional multi-layer film design, the metal-based organic hybrid film is used to participate in the formation of the anti-reflection film layer structure, and the overall process is simpler, the process difficulty is low and it is easy to implement.

[0072] In addition, metal-based organic hybrid films can be prepared by molecular layer deposition. By controlling the temperature during the deposition process and the thickness of the metal-based organic hybrid film, or by superimposing other metal oxide films on the pore wall surface of the pores in the metal-based organic hybrid film, the porosity and pore distribution can be regulated, so that the refractive index of the metal-based organic hybrid film can be adjusted. This is conducive to broadening the application scope of metal-based organic hybrid films, so that they can form an anti-reflection film layer structure with extremely low reflectivity when combined with a variety of different anti-reflection base layers.

[0073] As an example of this embodiment, the anti-reflection enhancing layer may be a metal-based organic hybrid film.

[0074] As another example of this embodiment, the anti-reflection enhancement layer includes at least one metal-based organic hybrid film and at least one metal oxide film, the material of the metal oxide film includes metal oxide, and the metal-based organic hybrid film and the metal oxide film are alternately stacked. It can be understood that each layer of the metal-based organic hybrid film can have a porous structure, and each layer of the metal oxide film can be attached to the pore wall surface in the adjacent metal-based organic hybrid film.

[0075] It can be understood that the anti-reflection base layer can refer to the film layer with anti-reflection effect known in the present disclosure. As an example of this embodiment, the anti-reflection base layer includes a high refractive index film and a low refractive index film, and the refractive index of the high refractive index film is higher than the refractive index of the low refractive index film. The high refractive index film and the low refractive index film each have at least one layer, and the high refractive index film and the low refractive index film are alternately stacked. The structure designed by stacking the high refractive index film and the low refractive index film can reduce the reflectivity of the substrate in which it is located.

[0076] As an example of this embodiment, each of the high refractive index film and the low refractive index film has at least one layer, and the high refractive index film and the low refractive index film are alternately stacked. It can be understood that as the number of layers of the high refractive index film and the low refractive index film increases, the anti-reflection effect of the anti-reflection base layer composed of them can also be enhanced, but this also increases the structural complexity of the anti-reflection base layer, and correspondingly makes the preparation process more complicated.

[0077] As an example of this embodiment, the number of high refractive index films and low refractive index films is the same, and in the anti-reflection base layer, the high refractive index film is disposed closest to the substrate, and the low refractive index film is disposed closest to the anti-reflection enhancement layer.

[0078] In some examples, the total number of film layers of the high refractive index film and the low refractive index film is 2 to 4 layers, which is conducive to simplifying the structure of the anti-reflection base layer as much as possible. Moreover, as will be explained below, even for the anti-reflection base layer with a simple structure in this example, by correspondingly setting the anti-reflection enhancement layer, the anti-reflection film layer structure can still have a significantly lower reflectivity as a whole.

[0079] Figure 1 Schematic diagram of the structure of an anti-reflection device disclosed in the present invention. Figure 1 As shown, the anti-reflection device includes a substrate 100 and an anti-reflection film layer structure stacked on the substrate 100, the anti-reflection film layer structure includes an anti-reflection base layer 120 and an anti-reflection enhancement layer 110 stacked on the anti-reflection base layer 120, and the anti-reflection enhancement layer 110 includes a metal-based organic hybrid film with a porous structure.

[0080] exist Figure 1 In the illustrated embodiment, the anti-reflection base layer 120 includes a high refractive index film 121 and a low refractive index film 122 , wherein the refractive index of the high refractive index film 121 is higher than that of the low refractive index film 122 .

[0081] As an example of this embodiment, the substrate 100 may be a workpiece that carries the anti-reflection film layer structure. The workpiece may be, but is not limited to, an optical lens. The material of the optical lens may be organic glass or inorganic glass.

[0082] In some examples, the organic glass is resin glass, and the inorganic glass is K9 glass.

[0083] Reference Figure 1 As shown, in this embodiment, in the anti-reflection base layer 120 , the film located at the bottom layer is a high-refractive-index film 121 , and the film located at the top layer is a low-refractive-index film 122 .

[0084] As an example of this embodiment, the refractive index of the high refractive index film 121 is ≥ 1.5. Further, the refractive index of the high refractive index film 121 is 1.5-2.3.

[0085] As an example of this embodiment, the material of the high refractive index film 121 includes one or more of titanium oxide (TiO2), aluminum oxide (Al2O3), tantalum oxide (Ta2O3) and zirconium oxide (ZrO2). Among them, the refractive index of titanium oxide is about 2.31, the refractive index of aluminum oxide is about 1.62, the refractive index of tantalum oxide is about 2.11, and the refractive index of zirconium oxide is about 2.15. It can be understood that the refractive index of the high refractive index film 121 is related to its material, and the material of the high refractive index film 121 can be selected corresponding to the required refractive index.

[0086] As an example of this embodiment, the thickness of the high refractive index film 121 is 3nm to 30nm. In some examples, the thickness of the high refractive index film 121 can be 3nm, 5nm, 6nm, 7nm, 8nm, 10nm, 12nm, 15nm, 17nm, 20nm, 25nm, 30nm, or the thickness of the high refractive index film 121 can also be between any two of the above thicknesses.

[0087] As an example of this embodiment, the refractive index of the low refractive index film 122 is ≤ 1.5. Further, the refractive index of the low refractive index film 122 is 1.35 to 1.5.

[0088] As an example of this embodiment, the material of the low refractive index film 122 includes one or more of silicon oxide (SiO2) and magnesium fluoride (MgF2). The refractive index of silicon oxide is about 1.45, and the refractive index of magnesium fluoride is about 1.38. It can be understood that the refractive index of the low refractive index film 122 is related to its material, and the material of the low refractive index film 122 can be selected corresponding to the required refractive index.

[0089] As an example of this embodiment, the thickness of the low refractive index film 122 is 40 nm to 120 nm.

[0090] In some examples, the thickness of the low refractive index film 122 may be 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm, 100 nm, 110 nm, or 120 nm, or the thickness of the low refractive index film 122 may be between any two of the above thicknesses.

[0091] Reference Figure 1As shown, as an example of this embodiment, the anti-reflection enhancement layer 110 is a metal-based organic hybrid film.

[0092] It is understood that the refractive index of the metal-based organic hybrid film may gradually change along the thickness direction, but the metal-based organic hybrid film as a whole has an equivalent refractive index. As an example of this embodiment, the equivalent refractive index of the anti-reflection enhancement layer 110 is 1.2-1.5, that is, the equivalent refractive index of the metal-based organic hybrid film of this embodiment is 1.2-1.5.

[0093] Furthermore, in this embodiment, the equivalent refractive index of the metal-based organic hybrid film is 1.23-1.3. The metal-based organic hybrid film with an equivalent refractive index within this range can significantly enhance the anti-reflection effect, which is conducive to obtaining an anti-reflection film layer structure with significantly lower reflectivity.

[0094] In some examples, the equivalent refractive index of the metal-based organic hybrid film may be 1.23, 1.24, 1.25, 1.26, 1.27, 1.28, 1.29, or 1.3, or the equivalent refractive index of the metal-based organic hybrid film may be between any two of the above refractive indices.

[0095] In general, the equivalent refractive index of the metal-based organic hybrid membrane is related to factors such as the membrane thickness, pore size, and porosity.

[0096] As an example of this embodiment, the thickness of the metal-based organic hybrid film is 10 nm to 200 nm.

[0097] In some examples, the thickness of the metal-based organic hybrid film can be 10nm, 20nm, 30nm, 40nm, 50nm, 60nm, 70nm, 80nm, 100nm, 120nm, 150nm, 200nm, or the thickness of the metal-based organic hybrid film can be between any two of the above thicknesses.

[0098] As an example of this embodiment, the pore size of the pores in the metal-based organic hybrid membrane is 1 nm to 30 nm.

[0099] In some examples, the pore size of the pores in the metal-based organic hybrid membrane is approximately 1 nm, 2 nm, 3 nm, 5 nm, 7 nm, 10 nm, 12 nm, 14 nm, 15 nm, 17 nm, 20 nm, 25 nm, or 30 nm, or the pore size of the pores in the metal-based organic hybrid membrane may also be between any two of the above pore sizes.

[0100] As an example of this embodiment, the porosity of the metal-based organic hybrid membrane is 10% to 70%.

[0101] In some examples, the porosity of the metal-based organic hybrid membrane is 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, or 70%, or the porosity of the metal-based organic hybrid membrane may be between any two of the above porosities.

[0102] As an example of this embodiment, the material of the metal-based organic hybrid film includes one or more of an aluminum-based hydroquinone hybrid material, a zinc-based hydroquinone hybrid material, and a titanium-based hydroquinone hybrid material. Among them, the aluminum-based hydroquinone hybrid material can be obtained by reacting an aluminum compound with hydroquinone, and the aluminum compound can include but is not limited to trimethyl aluminum. The zinc-based hydroquinone hybrid material can be obtained by reacting a zinc compound with hydroquinone, and the zinc compound can include but is not limited to diethyl zinc. The titanium-based hydroquinone hybrid material can be obtained by reacting a titanium compound with hydroquinone, and the titanium compound can include but is not limited to titanium tetrachloride.

[0103] As an example of this embodiment, the metal-based organic hybrid membrane is prepared by molecular layer deposition. During the molecular layer deposition process, a porous structure can be directly formed in the formed metal-based organic hybrid membrane. By controlling the temperature during the deposition process and the number of deposition cycles, the porous structure in the metal-based organic hybrid membrane can be controlled accordingly.

[0104] As an example of this embodiment, the raw materials for preparing the metal-based organic hybrid film include a first metal precursor and an organic precursor, wherein the first metal precursor is selected from one or more of trimethylaluminum, ethylene dizinc and titanium tetrachloride, and the organic precursor is selected from hydroquinone.

[0105] It can be understood that the material of the metal-based organic hybrid film is related to the raw materials used to prepare it. For example, if the material of the metal-based organic hybrid film includes an aluminum-based hydroquinone hybrid material, the first metal precursor can be trimethylaluminum, and the organic precursor can be hydroquinone. If the material of the metal-based organic hybrid film includes a zinc-based hydroquinone hybrid material, the first metal precursor can be ethylenedizinc, and the organic precursor can be hydroquinone. If the material of the metal-based organic hybrid film includes a titanium-based hydroquinone hybrid material, the first metal precursor can be titanium tetrachloride, and the organic precursor can be hydroquinone.

[0106] As an example of this embodiment, the average reflectivity of the anti-reflection film layer structure for light in the 400nm-800nm ​​band is less than 0.2%.

[0107] Figure 2 FIG. 1 is a schematic diagram of the structure of another anti-reflection device disclosed in the present invention. Figure 2As shown, the anti-reflection device comprises a substrate 200 and an anti-reflection film layer structure stacked on the substrate 200, the anti-reflection film layer structure comprises an anti-reflection base layer 220 and an anti-reflection enhancement layer 210 stacked on the anti-reflection base layer 220, and the anti-reflection enhancement layer 210 comprises a metal-based organic hybrid film with a porous structure. Figure 2 In the illustrated embodiment, the anti-reflection base layer 220 includes two layers of high refractive index films 221 and two layers of low refractive index films 222 , wherein the refractive index of the high refractive index film 221 is higher than that of the low refractive index film 222 .

[0108] In this embodiment, the refractive index and thickness of the two layers of high refractive index films 221 may be different, and the refractive index and thickness of the two layers of low refractive index films 222 may also be different, which mainly depends on the structural design required by the anti-reflection base layer 220.

[0109] As an example of this embodiment, the substrate 200 may be a workpiece that carries the anti-reflection film layer structure. The workpiece may be, but is not limited to, an optical lens. The material of the optical lens may be organic glass or inorganic glass.

[0110] In some examples, the organic glass is resin glass, and the inorganic glass is K9 glass.

[0111] Reference Figure 2 As shown, in this embodiment, in the anti-reflection base layer 220 , the film located at the bottom layer is a high refractive index film 221 , and the film located at the top layer is a low refractive index film 222 .

[0112] As an example of this embodiment, the refractive index of the high refractive index film 221 is ≥ 1.5. Further, the refractive index of the high refractive index film 221 is 1.5-2.3.

[0113] As an example of this embodiment, the material of the high refractive index film 221 includes one or more of titanium oxide, aluminum oxide, tantalum oxide, and zirconium oxide.

[0114] As an example of this embodiment, the thickness of the high refractive index film 221 is 3 nm to 30 nm.

[0115] As an example of this embodiment, the refractive index of the low refractive index film 222 is ≤ 1.5. Further, the refractive index of the low refractive index film 222 is 1.35 to 1.5.

[0116] As an example of this embodiment, the material of the low refractive index film 222 includes one or more of silicon oxide and magnesium fluoride.

[0117] As an example of this embodiment, the thickness of the low refractive index film 222 is 40 nm to 120 nm.

[0118] Reference Figure 2As shown, as an example of this embodiment, the anti-reflection enhancement layer 210 includes at least one metal-based organic hybrid film and at least one metal oxide film, the material of the metal oxide film includes metal oxide, and the metal-based organic hybrid film and the metal oxide film are alternately stacked. The introduction of the metal oxide film can achieve the regulation of the pore structure in the anti-reflection enhancement layer 210, thereby enriching the performance of the anti-reflection enhancement layer 210.

[0119] Furthermore, each layer of the metal-based organic hybrid membrane may have a porous structure, and each layer of the metal oxide film may be attached to the surface of the pore wall in the adjacent metal-based organic hybrid membrane.

[0120] As an example of this embodiment, the equivalent refractive index of the anti-reflection enhancement layer 210 is 1.2-1.5, that is, the equivalent refractive index of the stacked structure composed of the metal-based organic hybrid film and the metal oxide film of this embodiment is 1.2-1.5.

[0121] Furthermore, in this embodiment, the equivalent refractive index of the anti-reflection enhancement layer 210 is 1.23-1.3. The anti-reflection enhancement layer 210 with an equivalent refractive index in this range can have a significantly better enhanced anti-reflection effect, which is conducive to obtaining an anti-reflection film layer structure with significantly lower reflectivity.

[0122] In some examples, the equivalent refractive index of the anti-reflection enhancement layer 210 may be 1.23, 1.24, 1.25, 1.26, 1.27, 1.28, 1.29, or 1.3, or the equivalent refractive index of the anti-reflection enhancement layer 210 may be between any two of the above refractive indices.

[0123] In general, the equivalent refractive index of the anti-reflection enhancement layer 210 is related to factors such as the film thickness, the pore diameter and the porosity. In addition, the ratio of the deposition times between the metal-based organic hybrid film and the metal oxide film during the deposition process will also have a significant impact on the equivalent refractive index of the pore structure.

[0124] As an example of this embodiment, the thickness of the anti-reflection enhancement layer 210 is 10 nm to 200 nm.

[0125] In some examples, the thickness of the anti-reflection enhancement layer 210 may be 10 nm, 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, 100 nm, 120 nm, 150 nm, or 200 nm, or the thickness of the anti-reflection enhancement layer 210 may be between any two of the above thicknesses.

[0126] As an example of this embodiment, the pores in the anti-reflection enhancement layer 210 have a pore diameter of 1 nm to 30 nm.

[0127] In some examples, the pore size of the pores in the anti-reflection enhancement layer 210 is approximately 1 nm, 2 nm, 3 nm, 5 nm, 7 nm, 10 nm, 12 nm, 14 nm, 15 nm, 17 nm, 20 nm, 25 nm, or 30 nm, or the pore size of the pores in the anti-reflection enhancement layer 210 may also be between any two of the above pore sizes.

[0128] As an example of this embodiment, the porosity of the anti-reflection enhancement layer 210 is 10% to 70%.

[0129] In some examples, the porosity of the anti-reflection enhancement layer 210 is 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, or 70%, or the porosity of the anti-reflection enhancement layer 210 can also be between any two of the above porosities.

[0130] As an example of this embodiment, the material of the metal-based organic hybrid film includes one or more of an aluminum-based hydroquinone hybrid material, a zinc-based hydroquinone hybrid material, and a titanium-based hydroquinone hybrid material.

[0131] As an example of this embodiment, the metal-based organic hybrid film is prepared by molecular layer deposition.

[0132] As an example of this embodiment, the raw materials for preparing the metal-based organic hybrid film include a first metal precursor and an organic precursor, wherein the first metal precursor is selected from one or more of trimethylaluminum, ethylene dizinc and titanium tetrachloride, and the organic precursor is selected from hydroquinone.

[0133] As an example of this embodiment, the material of the metal oxide film includes one or more of aluminum oxide, zinc oxide, and titanium oxide.

[0134] As an example of this embodiment, the metal oxide film is formed by atomic layer deposition.

[0135] As an example of this embodiment, the metal element in the metal oxide film is the same as the metal element in the metal-based organic hybrid film, which is conducive to making the metal oxide film and the metal-based organic hybrid film more closely combined and enhancing the stability of the stacked structure.

[0136] It will be appreciated that both the molecular layer deposition and atomic layer deposition processes include multiple deposition cycles.

[0137] As an example of this embodiment, the ratio between the number of deposition cycles of the metal-based organic hybrid film and the number of deposition cycles of the metal oxide film may be 1:(1-5).

[0138] In some examples, the ratio between the deposition cycle number of the metal-based organic hybrid film and the deposition cycle number of the metal oxide film can be 1:1, 1:2, 1:3, 1:4, 1:5, or the ratio between the deposition cycle numbers of the two can also be between any two of the above ratios. As the ratio increases, the pore size and porosity in the formed stacked structure will also decrease, thereby obtaining an anti-reflection enhancement layer 210 with a higher equivalent refractive index.

[0139] As an example of this embodiment, the average reflectivity of the anti-reflection film layer structure for light in the 400nm-800nm ​​band is less than 0.2%.

[0140] In the above embodiments, the anti-reflection device may be an optical device.

[0141] As some examples, the optical device may be an imaging device, such as a display, the substrate of the display includes a panel glass, and the anti-reflection film layer structure may be disposed on the panel glass of the display.

[0142] As some examples, the optical device may be a projection device, such as a projector, the substrate of the projector includes a lens, and the anti-reflection film layer structure may be disposed on the lens of the projector.

[0143] As some examples, the optical device may also include an imaging device, such as a camera, the substrate of the camera includes a lens, and the anti-reflection film layer structure may be disposed on the lens.

[0144] In a first aspect, the present disclosure further provides a method for preparing an anti-reflection device, the preparation method comprising the following steps S1 to S3.

[0145] Step S1, providing a substrate.

[0146] As an example of this embodiment, the substrate may be a workpiece that carries the anti-reflection film layer structure. The workpiece may be, but is not limited to, an optical lens. The material of the optical lens may be organic glass or inorganic glass.

[0147] In some examples, the organic glass is resin glass, and the inorganic glass is K9 glass.

[0148] Step S2, preparing an anti-reflection base layer on the substrate.

[0149] As an example of this embodiment, the step of preparing an anti-reflection base layer on the substrate includes:

[0150] A high refractive index film and a low refractive index film are alternately deposited on the substrate, wherein the refractive index of the high refractive index film is higher than that of the low refractive index film, and each of the high refractive index film and the low refractive index film has at least one layer.

[0151] As an example of this embodiment, the material of the high refractive index film includes one or more of titanium oxide, aluminum oxide, tantalum oxide, and zirconium oxide.

[0152] As an example of this embodiment, the material of the low refractive index film includes one or more of silicon oxide and magnesium fluoride.

[0153] It can be understood that the materials and number of layers of the high refractive index film and the low refractive index film can be set according to specific needs.

[0154] As an example of this embodiment, the method of preparing the high refractive index film may be a physical vapor deposition method or an atomic layer deposition method.

[0155] As an example of this embodiment, the method of preparing the low refractive index film may be a physical vapor deposition method or an atomic layer deposition method.

[0156] Step S3, placing the substrate in a deposition chamber, and preparing an anti-reflection enhancement layer on the substrate.

[0157] Wherein, the step of preparing the anti-reflection enhancement layer includes: depositing and forming a metal-based organic hybrid film with a porous structure.

[0158] As an example of this embodiment, the material of the metal-based organic hybrid film includes one or more of an aluminum-based hydroquinone hybrid material, a zinc-based hydroquinone hybrid material, and a titanium-based hydroquinone hybrid material.

[0159] As an example of this embodiment, the metal-based organic hybrid material is deposited by molecular layer deposition.

[0160] In this example, the step of depositing a metal-based organic hybrid film includes: introducing a first metal precursor into a deposition chamber and attaching it to the substrate to form a first monolayer, and introducing an organic precursor into the deposition chamber and attaching it to the substrate to form a second monolayer. The steps of forming the first monolayer and the steps of forming the second monolayer are taken as a first deposition cycle. It can be understood that each deposition cycle can form a layer of metal-based organic hybrid material, and multiple deposition cycles performed continuously form a continuous metal-based organic hybrid film.

[0161] In this example, the first metal precursor is selected from one or more of trimethylaluminum, ethylene dizinc and titanium tetrachloride, and the organic precursor is selected from hydroquinone.

[0162] As an example of this embodiment, the number of first deposition cycles is 40 to 500 times. It can be understood that the number of first deposition cycles is related to the thickness of the metal-based organic hybrid film. The more the number of first deposition cycles, the thicker the metal-based organic hybrid film. In addition, the number of first deposition cycles is also related to the pore structure in the metal-based organic hybrid film. In general, as the number of first deposition cycles increases, the porosity and pore size in the metal-based organic hybrid film both show a trend of first significantly increasing and then slightly decreasing.

[0163] In some examples, the number of first deposition cycles may be 40, 60, 80, 100, 120, 150, 200, 250, 300, 400, or 500 times, or the number of first deposition cycles may be between any two of the above numbers.

[0164] As an example of this embodiment, after each formation of the first monolayer and each formation of the second monolayer, a step of purging the deposition chamber may be included. The step of purging the deposition chamber includes: introducing a protective gas into the deposition chamber to remove unreacted materials and byproducts generated by the reaction. This helps to ensure the purity of the surface of the first generated material to ensure the continuous deposition.

[0165] As an example of this embodiment, in the step of depositing the metal-based organic hybrid film, the temperature of the deposition chamber is controlled to be 150° C. to 300° C. Experimental verification shows that the temperature of the deposition chamber affects the pore size and porosity in the formed metal-based organic hybrid film, and controlling the temperature of the deposition chamber to be 150° C. to 300° C. is conducive to obtaining a metal-based organic hybrid film with a more suitable pore size and porosity.

[0166] In some examples, in the step of depositing the metal-based organic hybrid film, the temperature of the deposition chamber can be controlled to 150°C, 170°C, 200°C, 220°C, 250°C, 270°C, or 300°C, or the temperature of the deposition chamber can be controlled between any two of the above temperatures.

[0167] It can be understood that if the anti-reflection enhancement layer is a metal-based organic hybrid film, the anti-reflection enhancement layer can be prepared through the above steps.

[0168] As a further example of this embodiment, the step of preparing the anti-reflection enhancement layer further includes depositing to form a metal oxide film, and the step of depositing to form a metal-based organic hybrid film and the step of depositing to form a metal oxide film are performed alternately.

[0169] In this example, the method of depositing the metal oxide film can be atomic layer deposition. The use of atomic layer deposition is not only conducive to making the metal oxide film uniformly adhere to the pore walls of the previously prepared metal-based organic hybrid film, but also conducive to improving the consistency of the preparation process between the metal-based organic hybrid film and the metal oxide film.

[0170] As an example of this embodiment, the step of depositing the metal-based organic hybrid film and the step of depositing the metal oxide film may be performed sequentially in the same deposition chamber.

[0171] As an example of this embodiment, the step of depositing a metal oxide film includes: introducing a second metal precursor into a deposition chamber and attaching it to a substrate to form a third monolayer. Introducing an oxidant into the deposition chamber and attaching it to a substrate to form a fourth monolayer. The steps of forming the third monolayer and forming the fourth monolayer are taken as a second deposition cycle as a whole, and the second deposition cycle is repeated multiple times.

[0172] Wherein, at least one first deposition cycle is continuously performed to form a metal-based organic hybrid film, and at least one second deposition cycle is continuously performed to form a metal oxide film, and at least one metal-based organic hybrid film and at least one metal oxide film are alternately formed. It can be understood that the alternating process can form at least one metal-based organic hybrid film and at least one metal oxide film. Each metal-based organic hybrid film may have a porous structure.

[0173] In this example, when forming each layer of metal-based organic hybrid film, only one first deposition cycle may be performed. Accordingly, after each first deposition cycle is performed to form each layer of metal-based organic hybrid film, one or more second deposition cycles may be performed continuously to form a metal oxide film. It is understood that in other examples, when forming each layer of metal-based organic hybrid film, multiple first deposition cycles may also be performed continuously.

[0174] In this example, the second metal precursor is selected from one or more of trimethylaluminum, ethylene dizinc and titanium tetrachloride. In a further example, the first metal precursor and the second metal precursor are selected from the same material.

[0175] The oxidant may be selected from one or more of ozone and water.

[0176] As an example of this embodiment, in the step of depositing the metal oxide film, the temperature of the deposition chamber is controlled to be 150° C. to 300° C.

[0177] In some examples, during the step of depositing a metal oxide film, the temperature of the deposition chamber can be controlled to be 150°C, 170°C, 200°C, 220°C, 250°C, 270°C, or 300°C, or the temperature of the deposition chamber can be controlled between any two of the above temperatures.

[0178] It can be understood that if the anti-reflection enhancement layer includes a metal-based organic hybrid film and a metal oxide film attached to the pore walls thereof, the anti-reflection enhancement layer can be prepared through the above steps.

[0179] As an example of this embodiment, the ratio of the number of times the first deposition cycle is performed to the number of times the second deposition cycle is performed is 1:(1-5).

[0180] In some examples, the ratio of the number of first deposition cycles to the number of second deposition cycles may be 1:1, 1:2, 1:3, 1:4, 1:5, or the ratio of the number of deposition cycles of the two may be between any two of the above ratios.

[0181] As a further example of this embodiment, each time a metal-based organic hybrid film and a subsequent metal oxide film are formed, the ratio of the number of first deposition cycles to the number of second deposition cycles is 1:(1-5).

[0182] Furthermore, the present disclosure also provides an application of a metal-based organic hybrid film in an anti-reflection film layer structure. The anti-reflection film layer structure includes an anti-reflection enhancement layer, the anti-reflection enhancement layer includes a metal-based organic hybrid film, and the metal-based organic hybrid film has a porous structure.

[0183] In this embodiment, the metal-based organic hybrid film is the metal-based organic hybrid film described in any of the above embodiments.

[0184] As an example of this embodiment, the equivalent refractive index of the entire anti-reflection enhancement layer is 1.2-1.5.

[0185] As an example of this embodiment, the thickness of the anti-reflection enhancement layer is 10 nm to 200 nm.

[0186] As an example of this embodiment, the pore size of the pores in the anti-reflection enhancing layer is 1 nm to 30 nm.

[0187] As an example of this embodiment, the porosity of the anti-reflection enhancement layer is 10% to 70%.

[0188] As an example of this embodiment, the material of the metal-based organic hybrid film includes one or more of an aluminum-based hydroquinone hybrid material, a zinc-based hydroquinone hybrid material, and a titanium-based hydroquinone hybrid material.

[0189] As an example of this embodiment, the metal-based organic hybrid film is prepared by molecular layer deposition.

[0190] The raw materials for preparing the metal-based organic hybrid film include a first metal precursor and an organic precursor; wherein,

[0191] As an example of this embodiment, the first metal precursor is selected from one or more of trimethylaluminum, ethylene dizinc and titanium tetrachloride, and the organic precursor is selected from hydroquinone.

[0192] The present disclosure also provides the following examples to further illustrate some implementations of the above preparation method. Accordingly, the present disclosure also provides the following comparative examples to illustrate the advantages of the preparation method.

[0193] Example 1.1

[0194] K9 glass is used as a substrate, and the substrate is placed in a deposition chamber of a molecular layer deposition device.

[0195] Preparation of metal-based organic hybrid film: The temperature in the deposition chamber is controlled at 200°C, trimethylaluminum is used as the metal precursor, and hydroquinone is used as the organic precursor. A single deposition cycle is: 2s of trimethylaluminum is introduced into the deposition chamber, and then argon is introduced for 30s, and then 3s of hydroquinone is introduced, and then argon is introduced for 60s. The flow rate of all gases is controlled to be 2000sccm. 250 deposition cycles are performed, and the formed metal-based organic hybrid film is used as an anti-reflection enhancement layer.

[0196] Example 1.2

[0197] The only difference between Example 1.2 and Example 1.1 is that in the step of preparing the metal-based organic hybrid film, 50 deposition cycles are performed.

[0198] Example 1.3

[0199] The only difference between Example 1.3 and Example 1.1 is that in the step of preparing the metal-based organic hybrid film, 100 deposition cycles are performed.

[0200] Example 1.4

[0201] The only difference between Example 1.4 and Example 1.1 is that in the step of preparing the metal-based organic hybrid film, 500 deposition cycles are performed.

[0202] Example 1.5

[0203] The only difference between Example 1.5 and Example 1.1 is that in the step of preparing the metal-based organic hybrid film, the temperature in the deposition chamber is controlled to be 150°C.

[0204] Example 1.6

[0205] The only difference between Example 1.6 and Example 1.1 is that in the step of preparing the metal-based organic hybrid film, the temperature in the deposition chamber is controlled to be 250°C.

[0206] Example 1.7

[0207] The only difference between Example 1.7 and Example 1.1 is that in the step of preparing the metal-based organic hybrid film, the temperature in the deposition chamber is controlled to be 300°C.

[0208] Example 1.8

[0209] The only difference between Example 1.8 and Example 1.1 is that the step of preparing the metal-based organic hybrid film also includes preparing a metal oxide film, and the process is as follows: the temperature in the deposition chamber is controlled at 200°C, trimethylaluminum is used as a metal precursor, and water is used as an oxidant. A single deposition cycle is as follows: 2s of trimethylaluminum is introduced into the deposition chamber, and then argon gas is introduced for 30s, and then water vapor is introduced for 3s, and then argon gas is introduced for 60s. The flow rate of all gases is controlled to be 2000sccm. The number of deposition cycles of the metal-based organic hybrid film is 250 times. After each deposition cycle of the metal-based organic hybrid film, a deposition cycle of the metal oxide film is immediately performed. The formed metal-based organic hybrid film and the metal oxide film as a whole serve as an anti-reflection enhancement layer.

[0210] Example 1.9

[0211] The only difference between Example 1.9 and Example 1.8 is that after each deposition cycle of the metal-based organic hybrid film, two deposition cycles of the metal oxide film are performed.

[0212] Example 1.10

[0213] The only difference between Example 1.10 and Example 1.8 is that each time a deposition cycle of the metal-based organic hybrid film is performed, five deposition cycles of the metal oxide film are performed immediately afterwards.

[0214] Example 1.11

[0215] The only difference between Example 1.11 and Example 1.8 is that after each deposition cycle of the metal-based organic hybrid film, 10 deposition cycles of the metal oxide film are performed.

[0216] Example 1.12

[0217] The only difference between Example 1.12 and Example 1.8 is that in the step of preparing the metal-based organic hybrid film, diethyl zinc is used as the metal precursor; in the step of preparing the metal oxide film, diethyl zinc is used as the metal precursor.

[0218] Example 1.13

[0219] The only difference between Example 1.13 and Example 1.8 is that in the step of preparing the metal-based organic hybrid film, titanium tetrachloride is used as the metal precursor; in the step of preparing the metal oxide film, titanium tetrachloride is used as the metal precursor.

[0220] Experiment 1: The thickness, pore size, porosity and equivalent refractive index of each anti-reflection enhancement layer prepared in the above-mentioned Examples 1.1 to 1.11 were tested. The results can be seen in Table 1.

[0221] Table 1

[0222]

[0223] The “~” in Table 1 indicates an approximate number.

[0224] According to Table 1, the parameters such as the pore size and porosity of the anti-reflection enhancement layer in the present disclosure can be controlled by the deposition times, deposition temperature and superposition of metal oxide films of different thicknesses in the preparation process, which is conducive to forming anti-reflection enhancement layers of different equivalent refractive indices, thereby realizing the preparation of an anti-reflection enhancement layer with a variable refractive index. In general, with the increase of deposition cycles, the thickness of the metal-based organic hybrid film gradually increases, and the pore size and porosity show a trend of first increasing and then slightly decreasing. The change trend of the equivalent refractive index is opposite to that of the pore size and porosity, showing a trend of first decreasing and then increasing. With the increase of deposition temperature, the pore size and porosity show a trend of first slightly increasing and then slightly decreasing, and correspondingly, the equivalent refractive index shows a trend of first slightly decreasing and then slightly increasing.

[0225] For example, as shown in Table 1, in the steps of preparing metal-based organic hybrid membranes in Examples 1.1 to 1.4, the number of deposition cycles is different, and accordingly, the thickness, pore size and porosity of the prepared metal-based organic hybrid membranes are also different. The number of deposition cycles in Example 1.1 is more than that in Example 1.2 and Example 1.3, and accordingly, the porosity and pore size of Example 1.1 are higher, and the equivalent refractive index is lower. The number of deposition cycles in Example 1.4 is higher than that in Example 1.1, but compared with Example 1.1, the porosity and pore size of Example 1.4 are slightly lower, and the equivalent refractive index is slightly higher. This may be because when there are too many deposition cycles, the subsequently deposited metal-based organic hybrid materials will cause a certain blockage to the holes.

[0226] As shown in Table 1, in the steps of preparing the metal-based organic hybrid membrane in Example 1.1 and Example 1.5 to Example 1.7, the deposition temperatures are different. The deposition temperature of Example 1.5 is only 150°C, and its pore size and porosity are significantly lower. The deposition temperature of Example 1.6 is 250°C, and its pore size and porosity are close to those of Example 1.1. The deposition temperature of Example 1.7 is further increased to 300°C, and its pore size and porosity are also significantly lower than those of Example 1.1.

[0227] As shown in Table 1, compared with Example 1.1, Examples 1.8 to 1.11 also prepared a metal oxide film. As the amount of metal oxide film deposited increases, the pore size of the anti-reflection enhancement layer as a whole gradually decreases, and the porosity also gradually decreases. Correspondingly, the equivalent refractive index gradually increases. The anti-reflection enhancement layer prepared in Example 1.11 gradually approaches the refractive index of the aluminum oxide crystal material as a whole. At this time, the anti-reflection enhancement layer has basically lost its porous structure and basically has no effect of enhancing the anti-reflection effect.

[0228] Example 2.1

[0229] K9 glass was used as a substrate, and was ultrasonically cleaned with ethanol and ultrapure water in sequence, and then dried for use.

[0230] Preparation of anti-reflection base layer: Place the substrate in a deposition chamber and deposit the following thin films in sequence by atomic layer deposition:

[0231] (1) Titanium dioxide film with a thickness of 12.5 nm and a refractive index of 2.31;

[0232] (2) Silicon dioxide film with a thickness of 89 nm and a refractive index of 1.45.

[0233] An anti-reflection enhancement layer as described in Example 1.1 was prepared on the surface of the anti-reflection base layer.

[0234] Example 2.2

[0235] K9 glass was used as a substrate, and was ultrasonically cleaned with ethanol and ultrapure water in sequence, and then dried for use.

[0236] Preparation of anti-reflection base layer: Place the substrate in a deposition chamber and deposit the following thin films in sequence by atomic layer deposition:

[0237] (1) Aluminum oxide film with a thickness of 12.5 nm and a refractive index of 1.62;

[0238] (2) Silicon dioxide film with a thickness of 44 nm and a refractive index of 1.45;

[0239] (3) Titanium dioxide film with a thickness of 2.8 nm and a refractive index of 2.31;

[0240] (4) Silicon dioxide film with a thickness of 42 nm and a refractive index of 1.45.

[0241] An anti-reflection enhancement layer as described in Example 1.8 was prepared on the surface of the anti-reflection base layer.

[0242] Example 2.3

[0243] K9 glass was used as a substrate, and was ultrasonically cleaned with ethanol and ultrapure water in sequence, and then dried for use.

[0244] Preparation of anti-reflection base layer: Place the substrate in a deposition chamber and deposit the following thin films in sequence by atomic layer deposition:

[0245] (1) Silicon dioxide film with a thickness of 110 nm and a refractive index of 1.45;

[0246] (2) Titanium dioxide film with a thickness of 10.5 nm and a refractive index of 2.31;

[0247] (3) Silicon dioxide film with a thickness of 35.5 nm and a refractive index of 1.45;

[0248] (4) Titanium dioxide film with a thickness of 113 nm and a refractive index of 2.31;

[0249] (5) Silicon dioxide film with a thickness of 43 nm and a refractive index of 1.45;

[0250] (6) Titanium dioxide film with a thickness of 21 nm and a refractive index of 2.31;

[0251] (7) Silicon dioxide film with a thickness of 42 nm and a refractive index of 1.45;

[0252] (8) Titanium dioxide film with a thickness of 108 nm and a refractive index of 2.31;

[0253] (9) Magnesium fluoride film with a thickness of 87.5 nm and a refractive index of 1.38.

[0254] An anti-reflection enhancement layer as described in Example 1.8 was prepared on the surface of the anti-reflection base layer.

[0255] Comparative Example 1

[0256] The only difference between Comparative Example 1 and Example 2.1 is that no anti-reflection enhancement layer is prepared in Comparative Example 1.

[0257] Comparative Example 2

[0258] The only difference between Comparative Example 2 and Example 2.2 is that no anti-reflection enhancement layer is prepared in Comparative Example 2.

[0259] Comparative Example 3

[0260] The only difference between Comparative Example 3 and Example 2.3 is that no anti-reflection enhancement layer is prepared in Comparative Example 3.

[0261] Experiment 2: The reflectivity of the coated glasses of Example 2.1, Example 2.2 and Comparative Example 3 for light in the wavelength range of 400nm~800nm ​​was tested. The results can be seen in Table 2. Figure 3 The figure shows a curve diagram of the reflectivity of the coated glass in Comparative Example 3 as a function of wavelength. Figure 4 A schematic diagram of a curve showing how the reflectivity of the coated glass in Example 2.1 and Example 2.2 varies with wavelength is shown.

[0262] Table 2

[0263]

[0264] Comparative Examples 1 to 3 did not prepare an anti-reflection enhancement layer. As shown in Table 2, as the number of film layers in the anti-reflection base layer increases, the average reflectivity of the coated glass shows a trend of gradual decrease. However, even if an anti-reflection base layer composed of 9 film layers is used, the average reflectivity of the coated glass still reaches 0.53%. Figure 3 As shown, the reflectivity of the coated glass of Comparative Example 3 is generally lower than 1%, but the transmittance for light in a local wavelength band is still above 0.5%.

[0265] Compared with Comparative Examples 1 to 3, Examples 2.1 to 2.3 all prepare the anti-reflection enhancement layer of the present disclosure. As shown in Table 2, compared with Comparative Examples 1 to 3, the average reflectivity of the coated glass of Examples 2.1 to 2.3 is significantly reduced. More importantly, even compared with Comparative Example 3 with a more complex anti-reflection base structure, Examples 2.1 and 2.2 with a simpler anti-reflection base still show lower reflectivity. Figure 4 As shown, the reflectivity of the coated glass of Example 2.1 and Example 2.2 is lower than 0.2%. The above results all indicate that the anti-reflective coated glass of the present disclosure can simplify the anti-reflective film structure while ensuring a low reflectivity.

[0266] Please note that the above embodiments are for illustrative purposes only and are not meant to be limiting of this document.

[0267] It should be understood that, unless otherwise specified herein, there is no strict order restriction for the execution of the steps, and the steps may be executed in other orders. Moreover, at least a portion of the steps in the preparation process may include multiple sub-steps or multiple stages, and these sub-steps or stages are not necessarily executed at the same time, but may be executed at different times, and the execution order of these sub-steps or stages is not necessarily sequential, but may be executed in turn or alternately with other steps or at least a portion of the sub-steps or stages of other steps.

[0268] The various embodiments in this specification are described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the various embodiments can be referenced to each other.

[0269] The technical features of the above embodiments may be combined arbitrarily. To make the description concise, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

Claims

1. An anti-reflection device, characterized in that: The invention comprises a substrate and an anti-reflection film layer structure stacked on the substrate, wherein the anti-reflection film layer structure comprises an anti-reflection base layer and an anti-reflection enhancement layer stacked on the anti-reflection base layer, and the anti-reflection enhancement layer comprises a metal-based organic hybrid film with a porous structure.

2. The anti-reflection device according to claim 1, characterized in that: The anti-reflection enhancement layer is the metal-based organic hybrid film; or, The anti-reflection enhancement layer comprises at least one layer of the metal-based organic hybrid film and at least one layer of metal oxide film, the material of the metal oxide film comprises metal oxide, and the metal-based organic hybrid film and the metal oxide film are alternately stacked.

3. The anti-reflection device according to claim 2, characterized in that: The material of the metal oxide film includes one or more of aluminum oxide, zinc oxide and titanium oxide.

4. The anti-reflection device according to claim 1, characterized in that: The overall equivalent refractive index of the anti-reflection enhancement layer is 1.2-1.

5.

5. The anti-reflection device according to claim 4, characterized in that: The anti-reflection enhancement layer satisfies at least one of the following characteristics: (1) The thickness of the anti-reflection enhancement layer is 10nm~200nm; (2) The pore size of the pores in the anti-reflection enhancement layer is 1 nm to 30 nm; (3) The porosity of the anti-reflection enhancement layer is 10% to 70%.

6. The anti-reflection device according to any one of claims 1 to 5, characterized in that: The material of the metal-based organic hybrid film includes one or more of an aluminum-based hydroquinone hybrid material, a zinc-based hydroquinone hybrid material, and a titanium-based hydroquinone hybrid material.

7. The anti-reflection device according to claim 6, characterized in that: The metal-based organic hybrid film is prepared by molecular layer deposition.

8. The anti-reflection device according to claim 7, characterized in that: The raw materials for preparing the metal-based organic hybrid film include a first metal precursor and an organic precursor; wherein, The first metal precursor is selected from one or more of trimethylaluminum, ethylene dizinc and titanium tetrachloride, and the organic precursor is selected from hydroquinone.

9. The anti-reflection device according to any one of claims 1 to 5 and 7 to 8, characterized in that: The anti-reflection base layer comprises a high refractive index film and a low refractive index film, wherein the refractive index of the high refractive index film is higher than the refractive index of the low refractive index film; The high refractive index film and the low refractive index film each have at least one layer, and the high refractive index film and the low refractive index film are alternately stacked.

10. The anti-reflection device according to claim 9, characterized in that: The total number of film layers of the high refractive index film and the low refractive index film is 2 to 4 layers.

11. The anti-reflection device according to any one of claims 1 to 5, 7 to 8 and 10, characterized in that: The average reflectivity of the anti-reflection film layer structure for light in the 400nm-800nm ​​band is below 0.2%.

12. A method for preparing an anti-reflection device, characterized in that: The steps include: providing a substrate; Preparing an anti-reflection base layer on the substrate; The substrate is placed in a deposition chamber, and an anti-reflection enhancement layer is prepared on the substrate, wherein the step of preparing the anti-reflection enhancement layer includes: depositing a metal-based organic hybrid film having a porous structure.

13. The method for preparing an anti-reflection device according to claim 12, characterized in that: The material of the metal-based organic hybrid film includes one or more of an aluminum-based hydroquinone hybrid material, a zinc-based hydroquinone hybrid material, and a titanium-based hydroquinone hybrid material.

14. The method for preparing an anti-reflection device according to claim 13, characterized in that: The metal-based organic hybrid film is deposited by molecular layer deposition.

15. The method for preparing an anti-reflection device according to any one of claims 12 to 14, characterized in that: The step of preparing the anti-reflection enhancement layer further comprises depositing to form a metal oxide film, and the step of depositing to form a metal-based organic hybrid film and the step of depositing to form a metal oxide film are performed alternately.

16. The method for preparing an anti-reflection device according to claim 15, characterized in that: The step of depositing and forming a metal-based organic hybrid film includes: introducing a first metal precursor into a deposition chamber and attaching it to the substrate to form a first monolayer, introducing an organic precursor into the deposition chamber and attaching it to the substrate to form a second monolayer; The step of depositing the metal oxide material includes: introducing a second metal precursor into the deposition chamber and attaching it to the substrate to form a third monolayer, introducing an oxidant into the deposition chamber and attaching it to the substrate to form a fourth monolayer; The steps of forming the first monolayer and the steps of forming the second monolayer are taken as a first deposition cycle, and the steps of forming the third monolayer and the steps of forming the fourth monolayer are taken as a second deposition cycle; At least one first deposition cycle is continuously performed to form a metal-based organic hybrid film, and at least one second deposition cycle is continuously performed to form a metal oxide film, and at least one metal-based organic hybrid film and at least one metal oxide film are alternately formed.

17. The method for preparing an anti-reflection device according to claim 16, characterized in that: The first metal precursor is selected from one or more of trimethylaluminum, ethylenedizinc and titanium tetrachloride, and the organic precursor is selected from hydroquinone; and / or, The second metal precursor is selected from one or more of trimethylaluminum, ethylene dizinc and titanium tetrachloride, and the oxidant is selected from one or more of water and ozone.

18. The method for preparing an anti-reflection device according to claim 16, characterized in that: The ratio of the number of times the first deposition cycle is performed to the number of times the second deposition cycle is performed is 1:(1-5).

19. The method for preparing an anti-reflection device according to claim 16, characterized in that: The number of the first deposition cycles is 40 to 500 times.

20. The method for preparing an anti-reflection device according to any one of claims 12 to 14 and 16 to 19, characterized in that: In the step of depositing the metal-based organic hybrid film, the temperature of the deposition chamber is controlled to be 150° C. to 300° C.

21. The method for preparing an anti-reflection device according to any one of claims 12 to 14 and 16 to 19, characterized in that: The step of preparing an anti-reflection base layer on the substrate comprises: A high refractive index film and a low refractive index film are alternately deposited on the substrate, wherein the refractive index of the high refractive index film is higher than that of the low refractive index film, and each of the high refractive index film and the low refractive index film has at least one layer.

22. Application of a metal-based organic hybrid film in an anti-reflection film structure, characterized in that: The anti-reflection film layer structure comprises an anti-reflection enhancement layer, the anti-reflection enhancement layer comprises the metal-based organic hybrid film, and the metal-based organic hybrid film has a porous structure.

23. The use according to claim 22, characterized in that The metal-based organic hybrid film constitutes the anti-reflection enhancement layer; or, The anti-reflection enhancement layer comprises at least one layer of the metal-based organic hybrid film and at least one layer of metal oxide film, the material of the metal oxide film comprises metal oxide, and the metal-based organic hybrid film and the metal oxide film are alternately stacked.

24. The use according to claim 22, characterized in that The overall equivalent refractive index of the anti-reflection enhancement layer is 1.2-1.

5.

25. The use according to claim 24, characterized in that The anti-reflection enhancement layer satisfies at least one of the following characteristics: (1) The thickness of the anti-reflection enhancement layer is 10nm~200nm; (2) The pore size of the pores in the anti-reflection enhancement layer is 1 nm to 30 nm; (3) The porosity of the anti-reflection enhancement layer is 10% to 70%.

26. The use according to any one of claims 22 to 25, characterized in that: The material of the metal-based organic hybrid film includes one or more of an aluminum-based hydroquinone hybrid material, a zinc-based hydroquinone hybrid material, and a titanium-based hydroquinone hybrid material.

27. The use according to claim 26, characterized in that The metal-based organic hybrid film is prepared by molecular layer deposition.

28. The use according to claim 27, characterized in that The raw materials for preparing the metal-based organic hybrid film include a first metal precursor and an organic precursor; wherein, The first metal precursor is selected from one or more of trimethylaluminum, ethylene dizinc and titanium tetrachloride, and the organic precursor is selected from hydroquinone.

Citation Information

Cited By

  • Optical device, and preparation method therefor and use thereof

    WO2026051884A1