Storage-resistant anti-cracking type cigarette blasting bead and preparation method thereof
By using mixed glue powder, cellulose nanocrystals and polysaccharide reinforced coating materials in smoke explosion beads, the problem of existing smoke explosion beads is easily broken during storage and transportation, and its anti-rupture performance is significantly improved and stability, extends shelf life and improves biocompatibility and environmental friendliness.
Patent Information
- Application Number
- CN202411292822.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-14
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-09-14
AI Technical Summary
Existing smoke-burning bead materials are prone to lose toughness when temperature and humidity change, resulting in damage, and have poor strength, which can easily break during storage and transportation.
Consisting of wall materials with mixed glue powder, modified agent and skeleton filler materials, including carrageenan, gellan gum, gelatin and instant agar, cellulose nanocrystals and chitosan gel solution, and inorganic skeleton modifier nanotitanium dioxide particles and polysaccharide strengthen the cladding layer to enhance the toughness and structural strength of the burst beads.
It significantly improves the anti-breaking performance and storage stability of the blast beads, extends the shelf life of the product, and has advantages in terms of biocompatibility and environmental friendliness.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of cigarette explosive beads, in particular to a storage-resistant and rupture-resistant cigarette explosive bead and a preparation method thereof. Background Art
[0002] Exploding beads, also known as tobacco microcapsules, flavoring beads, and fragrance pills, are widely used in the daily chemical, food, and tobacco industries because of their stable aroma, large aroma-carrying capacity, diversity, personalization, and increased moisturizing properties. The design concept of cigarette blasting beads is to embed small beads in cigarettes, which are filled with different flavor liquids. Users can easily squeeze the beads to break them when smoking, thereby releasing a variety of aromas and flavors. This unique experience not only increases the fun of smoking, but also meets the needs of modern consumers for personalization and diversity.
[0003] However, tobacco popping beads are usually made of relatively weak plastic or other lightweight materials, which are prone to lose toughness when the temperature and humidity change, resulting in breakage. In addition, due to the poor strength of tobacco popping beads themselves, improper storage environment, that is, high temperature, high humidity or improper stacking method may cause premature breakage of the popping beads.
[0004] In view of the above-mentioned related technologies, the inventors found that the existing cigarette bursting bead materials have poor strength and are prone to cracking during production, processing and transportation. Summary of the invention
[0005] In order to improve the defect that the existing tobacco bursting beads are not storable and are easy to break, the present application provides a storage-resistant and rupture-resistant tobacco bursting bead and a preparation method thereof.
[0006] In the first aspect, the present application provides a storage-resistant and rupture-resistant cigarette explosive bead, which adopts the following technical solution:
[0007] A storage-resistant and rupture-resistant cigarette explosive bead comprises a wall material and a core material, wherein the core material is essential oil, and the wall material comprises the following substances in parts by weight:
[0008] 70-80 parts of mixed rubber powder;
[0009] Improver 0.5-10 parts;
[0010] 0.5-3.0 parts of skeleton filling material;
[0011] The mixed gum powder comprises a mixture of at least three of carrageenan, gellan gum, gelatin and instant agar.
[0012] Through the above technical scheme, the present application optimizes the storage-resistant and rupture-resistant popping beads for cigarettes through special wall materials and core material components. The composition of the wall material includes mixed rubber powder, modifiers and skeleton filling materials, so that the popping beads are not easy to break when subjected to force. In particular, the mixed use of carrageenan, gellan gum, gelatin and instant agar can enhance the elasticity and toughness of the wall material while maintaining good fluidity, ensuring the stability of the popping beads during storage and transportation. In addition, the selection of essential oil core materials not only improves the taste experience of cigarettes, but also extends the shelf life of the product to a certain extent.
[0013] Furthermore, the skeleton filling material is cellulose nanocrystals.
[0014] Through the above technical solution, this application introduces cellulose nanocrystals as skeleton filling materials, which significantly improves the structural strength and anti-rupture performance of the explosive beads. Cellulose nanocrystals have excellent mechanical properties and high specific surface area. Their addition can enhance the toughness and durability of the wall material and reduce the risk of breakage under external impact. At the same time, due to the natural source of cellulose, the material also has advantages in biocompatibility and environmental friendliness.
[0015] Furthermore, the cellulose nanocrystals are provided with a loading matrix, and the loading matrix is a chitosan gel solution.
[0016] Through the above technical solution, the present application uses chitosan gel liquid as a loading matrix, which helps to further improve the stability and functionality of cellulose nanocrystals. Chitosan, as a natural polysaccharide, provides an additional protective layer for the tobacco beads while improving the dispersion of cellulose nanocrystals inside the wall material, thereby making the prepared wall material structure uniform and having good mechanical properties and mechanical strength.
[0017] Furthermore, the improver includes an inorganic skeleton modifier, and the inorganic curing modifier is nano titanium dioxide particles.
[0018] Through the above technical solution, the present application further adds an inorganic skeleton modifier (nano titanium dioxide particles) to improve the mechanical properties and antioxidant capacity of the wall material. Through the structure of inorganic and organic materials, the mechanical strength and mechanical properties of the wall material structure can be further improved, thereby improving its anti-cracking performance.
[0019] Furthermore, the wall material is also provided with a strengthening layer, and the strengthening layer is a polysaccharide strengthening coating layer coated on the surface of the wall material.
[0020] Furthermore, the polysaccharide-enhanced coating layer is formed by coating a polysaccharide-enhanced coating liquid, and the polysaccharide-enhanced coating liquid includes the following substances in parts by weight:
[0021] Inulin 30-45 parts;
[0022] Calcium chloride 0.5-1.0 part;
[0023] 80-120 parts of water.
[0024] Through the above technical scheme, the present application further enhances the anti-rupture performance and storage stability of the bursting beads through the design of the strengthening layer. The polysaccharide coating not only provides additional physical protection, but also may increase the lubricity of the bursting beads, making it easier to control the force during the extrusion process and reducing the risk of rupture. At the same time, the mixed gum structure interacts locally with inulin at the edge of the binding band, such as hydrogen bonds and hydrophobic bonds, thereby forming a highly cross-linked gel network with a reinforced structure. The mechanical properties and mechanical strength of the wall material are further improved by changing the microstructure of the mixed gum, inulin and calcium chloride.
[0025] In a second aspect, the present application provides a method for preparing storage-resistant and rupture-resistant cigarette explosive beads, which adopts the following technical scheme:
[0026] A method for preparing storage-resistant and rupture-resistant cigarette explosive beads comprises the following preparation steps:
[0027] Mix the mixed rubber powder with deionized water and stir, and collect the mixed liquid;
[0028] The mixed liquid is placed in a heating device, heated and kept warm for gelling treatment, and the mixed gel liquid is collected;
[0029] Take the mixed glue and place it in a heating device to adjust the viscosity. After stirring and testing the viscosity until it is moderate, place it in an oil bath heating device, evacuate the air and let it stand for use.
[0030] Mix the tobacco flavor with liquid paraffin, collect the core liquid and cool it;
[0031] Using a pellet dropping device, the wall material solution is dripped into the cooled core material liquid under pressure, and wet pellets are collected;
[0032] The wet pellets are immersed in a polysaccharide-enhanced coating solution, and after the immersion is completed, they are washed, dried for equilibrium, and sieved to prepare storage-resistant and rupture-resistant tobacco explosive beads.
[0033] Furthermore, the temperature of the gelling treatment is 50-60°C.
[0034] Furthermore, the viscosity of the viscosity adjustment treatment is 880-920 MPa·s.
[0035] Furthermore, the cooling treatment temperature is 10-15°C.
[0036] Through the above technical scheme, the present application optimizes the preparation parameters of the bursting bead material, improves the processing performance of the product by adjusting the viscosity range and improving the cooling temperature, and also helps prevent cracking during use. At the same time, the cooling treatment temperature is optimized to further promote the solidification and solidification of the wall material, ensuring the stability of the bursting bead morphology, thereby reducing the fluidity of the material at a lower temperature, helping to form a more solid structure and reduce the risk of breakage due to external stress.
[0037] In summary, this application has the following beneficial effects:
[0038] First, the present application optimizes storage-resistant and rupture-resistant popping beads for cigarettes through special wall and core material components. The wall material composition includes mixed rubber powder, modifiers and skeleton filling materials, so that the popping beads are not easy to break when subjected to force. In particular, the mixed use of carrageenan, gellan gum, gelatin and instant agar can enhance the elasticity and toughness of the wall material while maintaining good fluidity, ensuring the stability of the popping beads during storage and transportation. In addition, the selection of essential oil core materials not only improves the taste experience of cigarettes, but also extends the shelf life of the product to a certain extent.
[0039] Second, the application introduces cellulose nanocrystals as skeleton filling materials, which significantly improves the structural strength and anti-rupture performance of the explosive beads. Cellulose nanocrystals have excellent mechanical properties and high specific surface area. Their addition can enhance the toughness and durability of the wall material and reduce the risk of breakage under external impact. At the same time, due to the natural source of cellulose, the material also has advantages in biocompatibility and environmental friendliness.
[0040] Third, the present application uses chitosan gel liquid as a loading matrix, which helps to further improve the stability and functionality of cellulose nanocrystals. Chitosan, as a natural polysaccharide, provides an additional protective layer for the tobacco beads while improving the dispersion of cellulose nanocrystals inside the wall material, thereby making the prepared wall material structure uniform and having good mechanical properties and mechanical strength.
[0041] Fourth, the present application optimizes the preparation parameters of the bursting bead material. By adjusting the viscosity range and improving the cooling temperature, the processing performance of the product is improved, and it also helps prevent cracking during use. At the same time, the cooling treatment temperature is optimized to further promote the solidification and solidification of the wall material, ensuring the stability of the bursting bead shape, so that the fluidity of the material is reduced at a lower temperature, which helps to form a more solid structure and reduce the risk of damage caused by external stress. DETAILED DESCRIPTION
[0042] The present application is further described in detail below in conjunction with embodiments.
[0043] In the examples of the present application, the raw materials and instruments used are as follows, but not limited thereto. Raw materials not otherwise specified are of analytical grade.
[0044] Preparation Example 1
[0045] Mixed rubber powder 1
[0046] Take 500-550 g of carrageenan, 500-550 g of instant agar, and 400-450 g of gellan gum, stir and mix, and collect the mixed gum powder 1.
[0047] Preparation Example 2
[0048] Take 500-550 g of gelatin, 500-550 g of instant agar, and 400-450 g of gellan gum, stir and mix, and collect the mixed gum powder 2.
[0049] Preparation Example 3
[0050] Take 200-250 g of gelatin, 250-350 g of carrageenan, 500-550 g of instant agar and 400-450 g of gellan gum, stir and mix, and collect the mixed gum powder 3.
[0051] Preparation Example 4
[0052] Skeleton filling material 1: cellulose nanocrystals.
[0053] Preparation Example 5
[0054] Skeleton filling material 2: Take 2 g of cellulose nanocrystals and 10 g of chitosan, stir and mix, and collect to obtain skeleton filling material 2.
[0055] Preparation Example 6
[0056] Polysaccharide enhanced coating solution 1
[0057] Take 300 g of PEG-100, 5 g of inulin, calcium chloride and 800 g of water, stir and mix, and collect the polysaccharide-enhanced coating solution 1.
[0058] Preparation Example 7
[0059] Polysaccharide enhanced coating liquid 2
[0060] Take 375 g of PEG-1000, 8 g of inulin, calcium chloride and 1000 g of water, stir and mix, and collect the polysaccharide-enhanced coating liquid 2.
[0061] Preparation Example 9
[0062] Polysaccharide enhanced coating liquid 3
[0063] Take 450g of PEG-100, 10g of inulin, calcium chloride and 1200g of water, stir and mix, and collect the polysaccharide-enhanced coating liquid 3.
[0064] Example 1
[0065] A storage-resistant and rupture-resistant cigarette explosive bead comprises 70 kg of mixed rubber powder 1, 0.5 kg of improver nano titanium dioxide particles and 0.5 kg of skeleton filling material 1.
[0066] A method for preparing storage-resistant and crack-resistant cigarette explosive beads comprises the following preparation steps:
[0067] According to the mass ratio of 1:30, 70 kg of mixed rubber powder 1 was mixed with deionized water and stirred, and the mixed liquid was collected;
[0068] The mixed solution is placed in a heating device, heated to 50°C, kept warm for gelling treatment, and the mixed gel solution is collected;
[0069] Take the mixed glue and place it in a heating device to adjust the viscosity to 880 MPa·s. After stirring and testing the viscosity until the viscosity is moderate, place it in an 85°C oil bath heating device, evacuate the air and let it stand for use;
[0070] Mix mint essence and liquid paraffin at a mass ratio of 1:25, collect the core liquid and cool it at 10°C;
[0071] The wall material solution is dripped into the cooled core material liquid by a pellet dropping device under pressure, and the wet pellets are collected, washed, dried, balanced and sieved to prepare storage-resistant and rupture-resistant cigarette bursting beads.
[0072] Example 2
[0073] A storage-resistant and rupture-resistant cigarette explosive bead comprises 75 kg of mixed rubber powder 1, 2 kg of nano titanium dioxide particles as an improver and 1.5 kg of skeleton filling material 1.
[0074] A method for preparing storage-resistant and crack-resistant cigarette explosive beads comprises the following preparation steps:
[0075] According to the mass ratio of 1:30, 75 kg of mixed rubber powder 1 was mixed with deionized water and stirred, and the mixed liquid was collected;
[0076] The mixed solution is placed in a heating device, heated to 55°C, kept warm for gelling treatment, and the mixed gel solution is collected;
[0077] Take the mixed glue and place it in a heating device to adjust the viscosity to 900 MPa·s. After stirring and testing the viscosity until the viscosity is moderate, place it in an 80°C oil bath heating device, evacuate the air and let it stand for use;
[0078] Mix mint essence and liquid paraffin at a mass ratio of 1:25, collect the core liquid and cool it at 12°C;
[0079] The wall material solution is dripped into the cooled core material liquid by a pellet dropping device under pressure, and the wet pellets are collected, washed, dried, balanced and sieved to prepare storage-resistant and rupture-resistant cigarette bursting beads.
[0080] Example 3
[0081] A storage-resistant and crack-resistant cigarette explosive bead comprises 80 kg of mixed rubber powder 1, 5 kg of nano titanium dioxide particles as an improver and 3.0 kg of skeleton filling material 1.
[0082] A method for preparing storage-resistant and crack-resistant cigarette explosive beads comprises the following preparation steps:
[0083] Take 80 kg of mixed rubber powder 1 and deionized water at a mass ratio of 1:30, mix and stir, and collect the mixed liquid;
[0084] The mixed liquid is placed in a heating device, heated to 50-60°C, kept warm for gelling treatment, and the mixed gelatin solution is collected;
[0085] Take the mixed glue and place it in a heating device to adjust the viscosity to 920 MPa·s. After stirring and testing the viscosity until the viscosity is moderate, place it in a 90°C oil bath heating device, evacuate the air and let it stand for use;
[0086] Mix mint essence and liquid paraffin at a mass ratio of 1:25, collect the core liquid and cool it at 15°C;
[0087] The wall material solution is dripped into the cooled core material liquid by a pellet dropping device under pressure, and the wet pellets are collected, washed, dried, balanced and sieved to prepare storage-resistant and rupture-resistant cigarette bursting beads.
[0088] Example 4
[0089] A storage-resistant and rupture-resistant cigarette explosive bead comprises 75 kg of mixed rubber powder 2, 2 kg of improver nano titanium dioxide particles and 1.5 kg of skeleton filling material 1.
[0090] A method for preparing storage-resistant and crack-resistant cigarette explosive beads comprises the following preparation steps:
[0091] According to the mass ratio of 1:30, 75 kg of mixed rubber powder 1 was mixed with deionized water and stirred, and the mixed liquid was collected;
[0092] The mixed solution is placed in a heating device, heated to 55°C, kept warm for gelling treatment, and the mixed gel solution is collected;
[0093] Take the mixed glue and place it in a heating device to adjust the viscosity to 900 MPa·s. After stirring and testing the viscosity until the viscosity is moderate, place it in an 80°C oil bath heating device, evacuate the air and let it stand for use;
[0094] Mix mint essence and liquid paraffin at a mass ratio of 1:25, collect the core liquid and cool it at 12°C;
[0095] The wall material solution is dripped into the cooled core material liquid by a pellet dropping device under pressure, and the wet pellets are collected, washed, dried, balanced and sieved to prepare storage-resistant and rupture-resistant cigarette bursting beads.
[0096] Example 5
[0097] A storage-resistant and rupture-resistant cigarette explosive bead comprises 75 kg of mixed rubber powder 3, 2 kg of nano titanium dioxide particles as a modifier and 1.5 kg of skeleton filling material 1.
[0098] A method for preparing storage-resistant and crack-resistant cigarette explosive beads comprises the following preparation steps:
[0099] According to the mass ratio of 1:30, 75 kg of mixed rubber powder 1 was mixed with deionized water and stirred, and the mixed liquid was collected;
[0100] The mixed solution is placed in a heating device, heated to 55°C, kept warm for gelling treatment, and the mixed gel solution is collected;
[0101] Take the mixed glue and place it in a heating device to adjust the viscosity to 900 MPa·s. After stirring and testing the viscosity until the viscosity is moderate, place it in an 80°C oil bath heating device, evacuate the air and let it stand for use;
[0102] Mix mint essence and liquid paraffin at a mass ratio of 1:25, collect the core liquid and cool it at 12°C;
[0103] The wall material solution is dripped into the cooled core material liquid by a pellet dropping device under pressure, and the wet pellets are collected, washed, dried, balanced and sieved to prepare storage-resistant and rupture-resistant cigarette bursting beads.
[0104] Example 6
[0105] A storage-resistant and rupture-resistant cigarette explosive bead comprises 75 kg of mixed rubber powder 1, 2 kg of nano titanium dioxide particles as an improver and 1.5 kg of skeleton filling material 2.
[0106] A method for preparing storage-resistant and crack-resistant cigarette explosive beads comprises the following preparation steps:
[0107] According to the mass ratio of 1:30, 75 kg of mixed rubber powder 1 was mixed with deionized water and stirred, and the mixed liquid was collected;
[0108] The mixed solution is placed in a heating device, heated to 55°C, kept warm for gelling treatment, and the mixed gel solution is collected;
[0109] Take the mixed glue and place it in a heating device to adjust the viscosity to 900 MPa·s. After stirring and testing the viscosity until the viscosity is moderate, place it in an 80°C oil bath heating device, evacuate the air and let it stand for use;
[0110] Mix mint essence and liquid paraffin at a mass ratio of 1:25, collect the core liquid and cool it at 12°C;
[0111] The wall material solution is dripped into the cooled core material liquid by a pellet dropping device under pressure, and the wet pellets are collected, washed, dried, balanced and sieved to prepare storage-resistant and rupture-resistant cigarette bursting beads.
[0112] Example 7
[0113] A storage-resistant and rupture-resistant cigarette explosive bead comprises 75 kg of mixed rubber powder 1, 2 kg of nano titanium dioxide particles as an improver and 1.5 kg of skeleton filling material 2.
[0114] A method for preparing storage-resistant and crack-resistant cigarette explosive beads comprises the following preparation steps:
[0115] According to the mass ratio of 1:30, 75 kg of mixed rubber powder 1 was mixed with deionized water and stirred, and the mixed liquid was collected;
[0116] The mixed solution is placed in a heating device, heated to 55°C, kept warm for gelling treatment, and the mixed gel solution is collected;
[0117] Take the mixed glue and place it in a heating device to adjust the viscosity to 900 MPa·s. After stirring and testing the viscosity until the viscosity is moderate, place it in an 80°C oil bath heating device, evacuate the air and let it stand for use;
[0118] Mix mint essence and liquid paraffin at a mass ratio of 1:25, collect the core liquid and cool it at 12°C;
[0119] Using a pellet dropping device, the wall material solution is dripped into the cooled core material liquid under pressure, and wet pellets are collected;
[0120] The wet pellets are placed in the polysaccharide enhanced coating liquid 1 and soaked for 60 seconds. After the soaking is completed, they are washed with water, dried for balance and sieved to prepare storage-resistant and rupture-resistant tobacco bursting beads. After the soaking is completed, they are washed with water, dried for balance and sieved to prepare storage-resistant and rupture-resistant tobacco bursting beads.
[0121] Example 8
[0122] A storage-resistant and rupture-resistant cigarette explosive bead comprises 75 kg of mixed rubber powder 1, 2 kg of nano titanium dioxide particles as an improver and 1.5 kg of skeleton filling material 2.
[0123] A method for preparing storage-resistant and crack-resistant cigarette explosive beads comprises the following preparation steps:
[0124] According to the mass ratio of 1:30, 75 kg of mixed rubber powder 1 was mixed with deionized water and stirred, and the mixed liquid was collected;
[0125] The mixed solution is placed in a heating device, heated to 55°C, kept warm for gelling treatment, and the mixed gel solution is collected;
[0126] Take the mixed glue and place it in a heating device to adjust the viscosity to 900 MPa·s. After stirring and testing the viscosity until the viscosity is moderate, place it in an 80°C oil bath heating device, evacuate the air and let it stand for use;
[0127] Mix mint essence and liquid paraffin at a mass ratio of 1:25, collect the core liquid and cool it at 12°C;
[0128] Using a pellet dropping device, the wall material solution is dripped into the cooled core material liquid under pressure, and wet pellets are collected;
[0129] The wet pellets are immersed in the polysaccharide enhanced coating liquid 2 for 60 seconds. After the immersion is completed, they are washed with water, dried for balance and sieved to prepare storage-resistant and rupture-resistant tobacco bursting beads. After the immersion is completed, they are washed with water, dried for balance and sieved to prepare storage-resistant and rupture-resistant tobacco bursting beads.
[0130] Example 9
[0131] A storage-resistant and rupture-resistant cigarette explosive bead comprises 75 kg of mixed rubber powder 1, 2 kg of nano titanium dioxide particles as an improver and 1.5 kg of skeleton filling material 2.
[0132] A method for preparing storage-resistant and crack-resistant cigarette explosive beads comprises the following preparation steps:
[0133] According to the mass ratio of 1:30, 75 kg of mixed rubber powder 1 was mixed with deionized water and stirred, and the mixed liquid was collected;
[0134] The mixed solution is placed in a heating device, heated to 55°C, kept warm for gelling treatment, and the mixed gel solution is collected;
[0135] Take the mixed glue and place it in a heating device to adjust the viscosity to 900 MPa·s. After stirring and testing the viscosity until the viscosity is moderate, place it in an 80°C oil bath heating device, evacuate the air and let it stand for use;
[0136] Mix mint essence and liquid paraffin at a mass ratio of 1:25, collect the core liquid and cool it at 12°C;
[0137] Using a pellet dropping device, the wall material solution is dripped into the cooled core material liquid under pressure, and wet pellets are collected;
[0138] The wet pellets are placed in the polysaccharide enhanced coating liquid 3 and soaked for 60 seconds. After the soaking is completed, they are washed with water, dried for balance and sieved to prepare storage-resistant and rupture-resistant tobacco bursting beads. After the soaking is completed, they are washed with water, dried for balance and sieved to prepare storage-resistant and rupture-resistant tobacco bursting beads.
[0139] Performance Testing
[0140] The storage-resistant and rupture-resistant tobacco bursting beads prepared in Examples 1-9 were subjected to performance tests, specifically testing their appearance, hardness and storage stability.
[0141] Appearance: Use a beaker to collect an appropriate amount of wet capsules and observe the appearance of the capsules on a light inspection table.
[0142] Hardness: measured using CTSII comprehensive cigarette capsule tester.
[0143] Storage stability: The popping beads are packaged and stored, and the appearance and quality of the popping beads are regularly inspected. The warehouse environment temperature is 22°C and the humidity is 50%.
[0144] The recorded results are shown in Table 1 below:
[0145] Table 1 Performance test table
[0146] sample Appearance Hardness / N Storage stability / 3 months Example 1 Good appearance 15.87 No leakage Example 2 Good appearance 16.87 No leakage Example 3 Good appearance 16.23 No leakage Example 4 Good appearance 16.18 No leakage Example 5 Good appearance 16.05 No leakage Example 6 Good appearance 16.85 No leakage Example 7 Good appearance 17.05 No leakage Example 8 Good appearance 17.59 No leakage Example 9 Good appearance 17.21 No leakage
[0147] From the above examples 1-9, combined with the test results in Table 1, it can be found that:
[0148] It can be seen from the performance tests of Examples 1-6 that the present application optimizes the storage-resistant and rupture-resistant tobacco beads through special wall material and core material components. The wall material composition includes mixed rubber powder, modifiers and skeleton filling materials, so that the beads are not easy to break when subjected to force. At the same time, the present application introduces cellulose nanocrystals as skeleton filling materials, which significantly improves the structural strength and anti-rupture performance of the beads. Cellulose nanocrystals have excellent mechanical properties and high specific surface area. Their addition can enhance the toughness and durability of the wall material and reduce the risk of breakage under external impact. At the same time, due to the natural source of cellulose, the material also has advantages in biocompatibility and environmental friendliness.
[0149] Comparison of Examples 1-6 and 7-9 further illustrates that the anti-rupture performance and storage stability of the popping beads are further enhanced by the design of the reinforcement layer. Polysaccharide coating not only provides additional physical protection, but also may increase the lubricity of the popping beads, making it easier to control the force during the extrusion process and reducing the risk of rupture. At the same time, the mixed gel structure interacts locally with inulin at the edge of the binding zone, such as hydrogen bonds and hydrophobic bonds, to form a highly cross-linked gel network with a reinforced structure. The mechanical properties and mechanical strength of the wall material are further improved by changes in the microstructure of the mixed gel, inulin and calcium chloride.
[0150] The present invention has been described in detail above in conjunction with specific implementations and exemplary examples, but these descriptions cannot be understood as limiting the present invention. Those skilled in the art understand that, without departing from the spirit and scope of the present invention, a variety of equivalent substitutions, modifications or improvements may be made to the technical solution of the present invention and its implementation methods, all of which fall within the scope of the present invention. The scope of protection of the present invention shall be subject to the attached claims.
[0151] All publications, patent applications, patents and other references mentioned in this specification are incorporated herein by reference. Unless otherwise defined, all technical and scientific terms used in this specification have the meanings conventionally understood by those skilled in the art. In the event of a conflict, the definition in this specification shall prevail.
[0152] When this specification uses the prefix "well-known to those skilled in the art", "prior art" or similar terms to introduce materials, substances, methods, steps, devices or components, etc., the objects introduced by the prefix cover those commonly used in the art when this application is filed, but also include those that are not commonly used at present but will become recognized in the art as being suitable for similar purposes.
[0153] In the context of the present specification, any matters or items not mentioned are directly applicable to those known in the art without any changes except those explicitly stated.
Claims
1. A storage-resistant and crack-resistant cigarette explosion bead, characterized in that: It comprises a wall material and a core material, wherein the core material is essential oil, and the wall material comprises the following substances in parts by weight: 70-80 parts of mixed rubber powder; Improver 0.5-10 parts; 0.5-3.0 parts of skeleton filling material; The mixed gum powder comprises a mixture of at least three of carrageenan, gellan gum, gelatin and instant agar.
2. The storage-resistant and rupture-resistant cigarette explosive beads according to claim 1, characterized in that: The skeleton filling material is cellulose nanocrystal.
3. The storage-resistant and rupture-resistant cigarette explosive beads according to claim 2, characterized in that: The cellulose nanocrystals are provided with a loading matrix, and the loading matrix is a chitosan gel solution.
4. The storage-resistant and rupture-resistant cigarette explosive beads according to claim 2, characterized in that: The improver includes an inorganic skeleton modifier, and the inorganic curing modifier is nano titanium dioxide particles.
5. The storage-resistant and rupture-resistant cigarette explosive beads according to claim 1, characterized in that: The wall material is also provided with a strengthening layer, and the strengthening layer is a polysaccharide strengthening coating layer coated on the surface of the wall material.
6. The storage-resistant and rupture-resistant cigarette explosive beads according to claim 5, characterized in that: The polysaccharide-enhanced coating layer is formed by coating a polysaccharide-enhanced coating liquid, and the polysaccharide-enhanced coating liquid includes the following materials in parts by weight: Inulin 30-45 parts; Calcium chloride 0.5-1.0 part; 80-120 parts of water.
7. The method for preparing the storage-resistant and rupture-resistant tobacco explosive beads according to any one of claims 1 to 6, characterized in that: The method comprises the following preparation steps: Mix the mixed rubber powder with deionized water and stir, and collect the mixed liquid; The mixed liquid is placed in a heating device, heated and kept warm for gelling treatment, and the mixed gel liquid is collected; Take the mixed glue and place it in a heating device to adjust the viscosity. After stirring and testing the viscosity until it is moderate, place it in an oil bath heating device, evacuate the air and let it stand for use. Mix the tobacco flavor with liquid paraffin, collect the core liquid and cool it; Using a pellet dropping device, the wall material solution is dripped into the cooled core material liquid under pressure, and wet pellets are collected; The wet pellets are immersed in a polysaccharide-enhanced coating solution, and after the immersion is completed, they are washed, dried for equilibrium, and sieved to prepare storage-resistant and rupture-resistant tobacco explosive beads.
8. The method for preparing storage-resistant and rupture-resistant cigarette explosive beads according to claim 7, characterized in that: The temperature of the gelling treatment is 50-60°C.
9. The method for preparing storage-resistant and rupture-resistant cigarette explosive beads according to claim 7, characterized in that: The viscosity of the viscosity adjustment treatment is 880-920 MPa·s.
10. The method for preparing storage-resistant and rupture-resistant tobacco explosive beads according to claim 7, characterized in that: The cooling treatment temperature is 10-15°C.
Citation Information
Patent Citations
Cigarette blast bead and preparation method thereof
CN106666822A
Microcapsule compositions prepared from polysaccharides
CN113453653A
Novel cigarette blasting bead wall material and preparation method thereof
CN114617292A
Fragrance particle for tobacco and its production
JP1989027461A
Spherical core-shell-particle
US20110081451A1