Washable business suit and manufacturing method thereof

By using polyaspartate resin in suits to anti-wrinkle layer and non-woven fabric layer, combined with microhook-like fabric layer, the suit deformation and bacterial breeding problems are solved, and the folding effect is not easy to cause wrinkles after washing and high antibacterial effect is achieved. .

CN119033170AActive Publication Date: 2024-11-29SHANGHAI QINGHE CLOTHING CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202411226609.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-11-29
Estimated Expiration
2044-09-03

AI Technical Summary

Technical Problem

Suits are prone to deformity when used and are not easy to clean, causing bacteria to grow, and lack anti-wrinkle and antibacterial functions.

Method used

Design a washable suit, using a wrinkle-proof layer to soak the polyaspartate resin solution in cotton cloth and then treat it at high temperature, combining the non-woven fabric layer and the micro-hook-like protruding fabric layer to form a tightly fit structure to reduce radial direction Shrinkage rate and enhance antibacterial effect.

Benefits of technology

It realizes that the suit is not easy to wrinkle after washing, has a small radial shrinkage rate and good antibacterial properties, keeps the style consistent and does not easily get stained.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119033170A_ABST
    Figure CN119033170A_ABST
Patent Text Reader

Abstract

The invention discloses a washable business suit and a manufacturing method thereof.The washable business suit comprises a business suit body, the business suit body comprises a crease-resistant layer, an outer fabric layer is arranged on one side of the crease-resistant layer, and an inner fabric layer is arranged on the other side of the crease-resistant layer; the crease-resistant layer is prepared by soaking cotton cloth in a polyaspartic acid ester resin solution and then performing high-temperature treatment, and a plurality of rhombic through holes are uniformly distributed in the cotton cloth; a non-woven fabric layer is arranged between the crease-resistant layer and the outer fabric layer, and a non-woven fabric layer is arranged between the crease-resistant layer and the inner fabric layer. According to the washable business suit disclosed by the invention, the crease-resistant layer and the non-woven fabric layer are arranged between the inner fabric layer and the outer fabric layer, so that not only is slippage among fibers prevented, but also the layers are attached more tightly, and the model is more fitting, so that a washing mode can be adopted, wrinkles are not easy to form, the radial shrinkage rate is very small, and the washable business suit is not easy to be contaminated by stains; and a better antibacterial effect is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a suit and a manufacturing method thereof, in particular to a washable suit and a manufacturing method thereof. Background Art

[0006] Usually, when a suit is used, it needs to be kept in a perfect straight state. However, it usually does not have an anti-wrinkle function. It is easy to deform after washing, which affects the shape. Moreover, if the suit is not washed frequently, bacteria will grow. Therefore, it is necessary to design a washable suit. Summary of the invention

[0007] The technical problem to be solved by the present invention is to provide a washable suit and a method for making the same, which can make the fit between the layers tighter and the shape more fitting, so that it can be washed by water, is not easy to wrinkle and has a very small radial shrinkage rate, is not easy to be stained, and has a better antibacterial effect.

[0008] The technical solution adopted by the present invention to solve the above-mentioned technical problems is to provide a washable suit, including a suit body, wherein the suit body includes an anti-wrinkle layer, an outer fabric layer is arranged on one side of the anti-wrinkle layer, and an inner fabric layer is arranged on the other side of the anti-wrinkle layer; the anti-wrinkle layer is made of cotton cloth soaked in a polyaspartic acid ester resin solution and then subjected to high-temperature treatment, and a plurality of diamond-shaped through holes are evenly distributed on the cotton cloth; a non-woven fabric layer is arranged between the anti-wrinkle layer and the outer fabric layer, and a non-woven fabric layer is arranged between the anti-wrinkle layer and the inner fabric layer.

[0009] Furthermore, the general formula of the polyaspartic acid ester resin structure monomer is:

[0010]

[0011] Wherein, R is an alkyl group, and X is a straight chain or alicyclic carbon chain structure.

[0012] Furthermore, the weight of the anti-wrinkle layer is 50-80 g / m 2 , the radial shrinkage rate is 1%-1.5%.

[0013] Furthermore, in parts by weight, the polyaspartic acid ester resin solution contains 50-60 parts of polyaspartic acid ester resin and 350-400 parts of water.

[0014] Furthermore, the outer fabric layer includes blended wool and polyester, with 60-70 parts of wool and 30-40 parts of polyester in parts by weight; the inner fabric layer includes wool and polyester, with 60-70 parts of wool and 30-40 parts of polyester in parts by weight; micro-hook-shaped protrusions are formed on the outer surfaces of the outer fabric layer and the inner fabric layer that are in contact with the anti-wrinkle layer.

[0015] Furthermore, an inner liner cotton layer is provided on a side of the inner fabric layer away from the outer fabric layer.

[0016] In order to solve the above technical problems, the present invention also provides a method for making the above-mentioned washable suit, which comprises the following steps: S1: treating a cotton cloth evenly distributed with a plurality of diamond-shaped through holes with a polyaspartic acid ester resin solution at high temperature to obtain an anti-wrinkle layer; S2: bonding non-woven fabrics on both sides of the anti-wrinkle layer by using an environmentally friendly water-based waterproof glue and a compounding machine; S3: bonding an outer fabric layer and an inner fabric layer respectively by using an environmentally friendly water-based waterproof glue and a compounding machine on the side where the two layers of non-woven fabrics are away from each other;

[0017] S4: installing an inner cotton layer on the side of the inner fabric layer away from the outer fabric layer; S5: cutting the fabric obtained in S4 according to a preset size to prepare a washable suit.

[0018] Furthermore, the step S1 includes the following steps: soaking: preparing a solution with 50-60 parts of polyaspartic acid ester resin and 350-400 parts of water, and heating it to 120-170°C, and completely immersing the cotton cloth in the solution so that the cotton cloth is fully in contact with the solution; drying: taking out the soaked cotton cloth and putting it into a dryer for baking until it is dry; bleaching: putting the dried cotton cloth into bleaching water and soaking it for 20-30 minutes; washing and dehydrating: washing and dehydrating the bleached cotton cloth.

[0019] Furthermore, the outer fabric layer and the inner fabric layer are blended by wool and polyester. During blending, the wool and polyester on one side are cut and overfed to form micro-hook-shaped protrusions, and then the surface with the micro-hook-shaped protrusions is bonded to the non-woven fabric.

[0020] Furthermore, in step S3, hot melt adhesive is evenly applied on the anti-wrinkle layer and the non-woven fabric on one side thereof to bond the inner fabric layer, and dried at 100-120°C for 2-5 minutes, and then hot melt adhesive is evenly applied on the anti-wrinkle layer and the non-woven fabric on the other side thereof to bond the outer fabric layer, and dried at 140-150°C for 2-5 minutes.

[0021] Compared with the prior art, the present invention has the following beneficial effects: the washable suit and the manufacturing method thereof provided by the present invention, by arranging an anti-wrinkle layer and a non-woven fabric layer between the inner and outer fabric layers, not only prevents slippage between fibers, but also makes the fit between the layers tighter and the pattern more fitting, so it can be washed in water, is not easy to wrinkle and has a very small radial shrinkage rate, is not easy to be stained, and has a better antibacterial effect. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is a schematic diagram of the structure of the washable suit of the present invention;

[0023] Figure 2 It is a partial cross-sectional structural schematic diagram of the washable suit of the present invention;

[0024] Figure 3 It is a schematic diagram of the structure of the anti-wrinkle layer of the washable suit of the present invention.

[0025] The markings in the figure are: 1. outer fabric layer; 2. non-woven fabric layer; 3. anti-wrinkle layer; 4. inner fabric layer; 5. inner cotton layer; 6. diamond-shaped through holes; 7. cotton cloth. DETAILED DESCRIPTION

[0026] The present invention is further described below by means of specific examples, but the scope of the present invention is not limited thereto. The components described in the present invention are generally commercially available.

[0027] Figure 1 This is a schematic diagram of the structure of the washable suit of the present invention; Figure 2 It is a partial cross-sectional structural schematic diagram of the washable suit of the present invention; Figure 3 It is a schematic diagram of the structure of the anti-wrinkle layer of the washable suit of the present invention.

[0028] See also Figure 1 , Figure 2 and Figure 3 The present invention provides a washable suit, comprising a suit body, wherein the suit body comprises an anti-wrinkle layer 3, an outer fabric layer 1 is arranged on one side of the anti-wrinkle layer 3, and an inner fabric layer 4 is arranged on the other side of the anti-wrinkle layer 3;

[0029] The anti-wrinkle layer 3 is made of cotton cloth 7 soaked in a polyaspartic acid ester resin solution and then subjected to high temperature treatment, and a plurality of diamond-shaped through holes 6 are evenly distributed on the cotton cloth 7;

[0030] A non-woven fabric layer 2 is arranged between the anti-wrinkle layer 3 and the outer fabric layer 1 , and a non-woven fabric layer 2 is arranged between the anti-wrinkle layer 3 and the inner fabric layer 4 .

[0031] The washable suit provided by the present invention has a general formula of the polyaspartic acid ester resin structure monomer:

[0032]

[0033] Wherein, R is an alkyl group, and X is a straight chain or alicyclic carbon chain structure.

[0034] Radial shrinkage refers to the reduction in length in the longitudinal direction (i.e. radial direction) of the fabric after it has been processed, soaked in water for a certain period of time, and then naturally dried, and is usually expressed as a percentage. For cotton cloth, its radial shrinkage will be affected by many factors such as the hygroscopicity of the fiber, the density of the fabric, the thickness of the yarn count, and the production process. In the national standard, for first-class cotton cloth, its warp (i.e. radial) shrinkage is generally stipulated to be 3%. This means that after washing, the cotton cloth will be shortened to a certain extent in the longitudinal direction, and it is obviously not directly applicable as the main body of the anti-wrinkle skeleton. The present invention greatly reduces its radial shrinkage by subjecting the cotton cloth 7 to high-temperature treatment with polyaspartic acid resin and water. The anti-wrinkle layer 3 obtained by the treatment of the present invention can have a gram weight as thin as 50-80 grams / m 2 , the radial shrinkage rate is 1%-1.5%.

[0035] The washable suit provided by the present invention comprises 50-60 parts of polyaspartic acid ester resin and 350-400 parts of water in the polyaspartic acid ester resin solution in parts by weight.

[0036] The washable suit provided by the present invention, wherein the outer fabric layer 1 comprises blended wool and polyester, with 60-70 parts by weight of wool and 30-40 parts of polyester;

[0037] The inner fabric layer 4 comprises wool and polyester, with 60-70 parts by weight of wool and 30-40 parts of polyester;

[0038] Micro-hook-shaped protrusions are formed on the outer surfaces of the outer fabric layer 1 and the inner fabric layer 4 that are in contact with the anti-wrinkle layer 3 .

[0039] The washable suit provided by the present invention has an inner cotton layer 5 arranged on the side of the inner fabric layer 4 away from the outer fabric layer 1, so that the suit can have a certain warmth-keeping effect; the outer fabric layer 1 and the inner fabric layer 4 are relatively skin-friendly, making the suit comfortable to wear.

[0040] The present invention also provides a method for making the above-mentioned washable suit, which comprises the following steps:

[0041] S1: a cotton cloth 7 having a plurality of diamond-shaped through holes 6 evenly distributed thereon is subjected to high temperature treatment using a polyaspartic acid resin solution to obtain an anti-wrinkle layer 3;

[0042] S2: The non-woven fabric 2 is bonded on both sides of the anti-wrinkle layer 3 by using an environmentally friendly water-based waterproof glue and a laminating machine;

[0043] S3: On the side where the two layers of non-woven fabrics 2 are away from each other, the outer fabric layer 1 and the inner fabric layer 4 are also bonded respectively by using environmentally friendly water-based waterproof glue and a laminating machine;

[0044] S4: Install the inner liner cotton layer 5 on the side of the inner fabric layer 4 away from the outer fabric layer;

[0045] S5: Cut the fabric obtained in S4 according to a preset size to prepare a washable suit.

[0046] The method for making a washable suit provided by the present invention, wherein step S1 comprises the following steps:

[0047] Soaking: Prepare a solution with 50-60 parts of polyaspartic acid ester resin and 350-400 parts of water, and heat it to 120-170° C., and completely immerse the cotton cloth 7 in the solution so that the cotton cloth 7 is fully in contact with the solution;

[0048] Drying: Take out the soaked cotton cloth 7 and put it into a dryer to bake until it is dry;

[0049] Bleaching: Soak the dried cotton cloth 7 in bleaching water for 20-30 minutes;

[0050] Cleaning and dehydration: The bleached cotton cloth 7 is cleaned and dehydrated.

[0051] The method for making a washable suit provided by the present invention, wherein the outer fabric layer 1 and the inner fabric layer 4 are blended with wool and polyester, the wool and polyester on one side are cut off during blending, and overfeeding is performed to form micro-hook-shaped protrusions, and then the surface with the micro-hook-shaped protrusions is bonded to the non-woven fabric 2. In step S3, firstly, hot melt adhesive is uniformly applied on the anti-wrinkle layer 3 and the non-woven fabric 2 on one side thereof to bond the inner fabric layer 4, and dried at 100-120°C for 2-5 minutes, and then hot melt adhesive is uniformly applied on the anti-wrinkle layer 3 and the non-woven fabric 2 on the other side thereof to bond the outer fabric layer 1, and dried at 140-150°C for 2-5 minutes. In this way, the micro-hook-shaped protrusions on the surface of the outer fabric layer 1 and the inner fabric layer 4 can penetrate into the diamond-shaped through-holes 6 on the non-woven fabric 2 and the wrinkle-proof layer 3 to form more bonding points, which not only prevents the slippage between fibers, but also makes the fit between the layers more compact and the pattern more docile, so it can be washed by water, is not easy to wrinkle and has a small radial shrinkage rate. At the same time, the tensile strength can be improved by drying and bonding twice and increasing the heating temperature of the second drying and bonding, because at high temperature, the micro-hook-shaped protrusions on the surface of the outer fabric layer 1 and the inner fabric layer 4 can better diffuse into the non-woven fabric 2 and the diamond-shaped through-holes 6 and form a three-dimensional mesh-like tight structure that intersects each other, so it is not easy to be stained and has a better antibacterial effect.

[0052] Embodiment 1:

[0053] Disclosed is a washable suit and a method for making the same, comprising:

[0054] The anti-wrinkle layer 3 is prepared by a method of high-temperature treatment of polyaspartic acid resin, water, and cotton cloth 7, and a plurality of diamond-shaped through holes 6 are evenly distributed on the cotton cloth 7;

[0055] 50 parts of polyaspartic acid resin and 350 parts of water;

[0056] Non-woven fabric 2:

[0057] Outer fabric layer 1: blended wool and polyester, in parts by weight, 62 parts of wool and 37 parts of polyester;

[0058] Outer fabric layer 4: blended wool and polyester, in parts by weight, 62 parts of wool and 37 parts of polyester;

[0059] Liner cotton layer 5: cotton velvet material.

[0060] First, a solution is prepared with 50 parts of polyaspartic acid ester resin and 350 parts of water, so that the cotton cloth 7 with multiple diamond-shaped through holes 6 evenly distributed thereon is completely immersed therein, the cotton cloth 7 is stirred so that the cotton cloth 7 is fully in contact with the solution, the cotton cloth 7 is taken out and dried, and then bleached for 30 minutes, and washed and dehydrated after completion, so as to obtain the anti-wrinkle skeleton body of the suit;

[0061] The non-woven fabric 2 is mounted on both sides of the anti-wrinkle body of the suit by using environmentally friendly water-based waterproof glue and a laminating machine;

[0062] On the side where the two non-woven fabrics 2 are away from each other, the outer fabric layer 1 and the inner fabric layer 4 are respectively installed by using environmentally friendly water-based waterproof glue and a laminating machine;

[0063] Install the inner liner cotton layer 5 on the side of the inner fabric layer 4 away from the outer fabric layer;

[0064] The above-mentioned fabric is cut according to a preset size to prepare a washable suit.

[0065] Embodiment 2:

[0066] Disclosed is a washable suit and a method for making the same, comprising:

[0067] The anti-wrinkle layer is prepared by a method of high-temperature treatment of polyaspartic acid resin, water, and cotton cloth 7, and a plurality of diamond-shaped through holes are evenly distributed on the cotton cloth 7;

[0068] 50 parts of polyaspartic acid resin and 400 parts of water;

[0069] Non-woven fabric layer 2;

[0070] Inner fabric layer 4: blended wool and polyester, in parts by weight, 60 parts of wool and 37 parts of polyester;

[0071] Outer fabric layer 1: blended wool and polyester, by weight, 60 parts wool, 37 parts polyester;

[0072] Liner cotton layer 5: cotton velvet material.

[0073] First, a solution is prepared with 50 parts of polyaspartic acid ester resin and 400 parts of water, so that the cotton cloth 7 with multiple diamond-shaped through holes 6 evenly distributed thereon is completely immersed in the solution, the cotton cloth 7 is stirred so that the cotton cloth 7 is fully in contact with the solution, the cotton cloth 7 is taken out and dried for tying, and then bleached for 30 minutes, and washed and dehydrated after completion, so as to obtain the anti-wrinkle skeleton body of the suit;

[0074] The non-woven fabric 2 is mounted on both sides of the anti-wrinkle body of the suit by using environmentally friendly water-based waterproof glue and a laminating machine;

[0075] On the side where the two non-woven fabrics 2 are away from each other, the outer fabric layer 1 and the inner fabric layer 4 are respectively installed by using environmentally friendly water-based waterproof glue and a laminating machine;

[0076] Install the inner liner cotton layer 5 on the side of the inner fabric layer 4 away from the outer fabric layer;

[0077] The above-mentioned fabric is cut according to a preset size to prepare a washable suit.

[0078] Embodiment 3:

[0079] Disclosed is a washable suit and a method for making the same, comprising:

[0080] The anti-wrinkle layer is prepared by a method of high-temperature treatment of polyaspartic acid resin, water, and cotton cloth 7, and a plurality of diamond-shaped through holes are evenly distributed on the cotton cloth 7;

[0081] 60 parts of polyaspartic acid resin and 350 parts of water;

[0082] Non-woven fabric layer 2;

[0083] Inner fabric layer 4: blended wool and polyester, in parts by weight, 65 parts of wool and 31 parts of polyester;

[0084] Outer fabric layer 1: blended wool and polyester, in parts by weight, 65 parts of wool and 31 parts of polyester;

[0085] Liner cotton layer 5: cotton velvet material.

[0086] First, a solution is prepared with 60 parts of polyaspartic acid ester resin and 350 parts of water, so that the cotton cloth 7 with multiple diamond-shaped through holes 6 evenly distributed thereon is completely immersed therein, the cotton cloth 7 is stirred so that the cotton cloth 7 is fully in contact with the solution, the cotton cloth 7 is taken out and dried, and then bleached for 30 minutes, and washed and dehydrated after completion, so as to obtain the anti-wrinkle skeleton body of the suit;

[0087] The non-woven fabric 2 is mounted on both sides of the anti-wrinkle body of the suit by using environmentally friendly water-based waterproof glue and a laminating machine;

[0088] On the side where the two non-woven fabrics 2 are away from each other, the outer fabric layer 1 and the inner fabric layer 4 are respectively installed by using environmentally friendly water-based waterproof glue and a laminating machine;

[0089] Install the inner liner cotton layer 5 on the side of the inner fabric layer 4 away from the outer fabric layer;

[0090] The above-mentioned fabric is cut according to a preset size to prepare a washable suit.

[0091] Embodiment 4:

[0092] Disclosed is a washable suit and a method for making the same, comprising:

[0093] The wrinkle-proof layer 3 is prepared by a method of high-temperature treatment of polyaspartic acid resin, water, and cotton cloth 7, and a plurality of diamond-shaped through holes are evenly distributed on the cotton cloth 7;

[0094] 60 parts of polyaspartic acid resin and 400 parts of water;

[0095] Non-woven fabric layer 2;

[0096] Inner fabric layer 1: blended wool and polyester, by weight, 66 parts wool, 33 parts polyester;

[0097] Outer fabric layer 4: blended wool and polyester, in parts by weight, 66 parts of wool and 33 parts of polyester;

[0098] Liner cotton layer 5: cotton velvet material.

[0099] First, a solution is prepared with 60 parts of polyaspartic acid ester resin and 400 parts of water, so that the cotton cloth 7 with multiple diamond-shaped through holes 6 evenly distributed thereon is completely immersed in the solution, the cotton cloth 7 is stirred so that the cotton cloth 7 is fully in contact with the solution, the cotton cloth is taken out and dried for tying, and then bleached for 30 minutes, and washed and dehydrated after completion, so as to obtain the anti-wrinkle skeleton body of the suit;

[0100] The non-woven fabric 2 is mounted on both sides of the anti-wrinkle body of the suit by using environmentally friendly water-based waterproof glue and a laminating machine;

[0101] On the side where the two non-woven fabrics 2 are away from each other, the outer fabric layer 1 and the inner fabric layer 4 are respectively installed by using environmentally friendly water-based waterproof glue and a laminating machine;

[0102] Install the inner liner cotton layer 5 on the side of the inner fabric layer 4 away from the outer fabric layer;

[0103] The above-mentioned fabric is cut according to a preset size to prepare a washable suit.

[0104] Embodiment 5:

[0105] Disclosed is a washable suit and a method for making the same, comprising:

[0106] The wrinkle-proof layer 3 is prepared by a method of high-temperature treatment of polyaspartic acid resin, water, and cotton cloth 7, and a plurality of diamond-shaped through holes are evenly distributed on the cotton cloth 7;

[0107] 56 parts of polyaspartic acid resin and 360 parts of water;

[0108] Non-woven fabric 2;

[0109] Inner fabric layer 4: blended wool and polyester, in parts by weight, 63 parts of wool and 37 parts of polyester;

[0110] Outer fabric layer 1: blended wool and polyester, in parts by weight, 63 parts of wool and 37 parts of polyester;

[0111] Liner cotton layer: cotton velvet material.

[0112] First, a solution is prepared with 56 parts of polyaspartic acid resin and 360 parts of water, so that the cotton cloth 7 with multiple diamond-shaped through holes 6 evenly distributed thereon is completely immersed in the solution, the cotton cloth 7 is stirred so that the cotton cloth 7 is fully in contact with the solution, the cotton cloth 7 is taken out and dried, and then bleached for 30 minutes, and washed and dehydrated after completion, so as to obtain the anti-wrinkle skeleton body of the suit;

[0113] The non-woven fabric 2 is mounted on both sides of the anti-wrinkle body of the suit by using environmentally friendly water-based waterproof glue and a laminating machine;

[0114] On the side where the two non-woven fabrics 2 are away from each other, the outer fabric layer 1 and the inner fabric layer 4 are respectively installed by using environmentally friendly water-based waterproof glue and a laminating machine;

[0115] Install the inner liner cotton layer 5 on the side of the inner fabric layer 4 away from the outer fabric layer;

[0116] The above-mentioned fabric is cut according to a preset size to prepare a washable suit.

[0117] Comparative Example 1:

[0118] Purchase existing suit A.

[0119] Comparative Example 2:

[0120] Purchase existing suit B.

[0121] After the suit prepared in Example 1 was washed and folded 100 times, there were no wrinkles and the radial shrinkage rate was 1.1%. It was placed in the outside for 48 hours, and its antibacterial performance reached 99.8%, and the ventilation performance was good.

[0122] After the suit prepared in Example 2 was washed and folded 100 times, there were no wrinkles and the radial shrinkage rate was 1.1%. It was placed in the outside for 48 hours, and its antibacterial performance reached 99.1%, and the ventilation performance was good.

[0123] The suit prepared in Example 3 had no wrinkles after being washed and folded 100 times, and the radial shrinkage rate was 1.2%. It was placed in the outside for 48 hours, and its antibacterial performance reached 99.2%, and the ventilation performance was good.

[0124] The suit prepared in Example 4 had no wrinkles after being washed and folded 100 times, and the radial shrinkage rate was 1.1%. It was placed in the outside for 48 hours, and its antibacterial performance reached 99.1%, and the ventilation performance was good.

[0125] The suit prepared in Example 5 had no wrinkles after being washed and folded 100 times, and the radial shrinkage rate was 1.1%. It was placed in the outside for 48 hours, and its antibacterial performance reached 98.8%, and the ventilation performance was good.

[0126] Suit A of Comparative Example 1 had slight wrinkles after being washed and folded 100 times, and its radial shrinkage rate was 3%. It was placed in the outside for 48 hours, and its antibacterial performance reached 78%, and its ventilation performance was good.

[0127] Suit B of Comparative Example 2 had slight wrinkles after being washed and folded 100 times, and its radial shrinkage rate was 4%. It was placed in the outside for 48 hours, and its antibacterial performance reached 76%, and its ventilation performance was good.

[0128] From the above experimental data, it can be seen that the solution of the present application has a better anti-wrinkle effect, the radial shrinkage rate after washing is greatly reduced to nearly 1%, and the antibacterial effect is better.

[0129] In summary, the polyaspartic acid ester resin, water, and high temperature used in the present invention make the cotton cloth not easy to fold, and the wrinkle-proof layer formed can be restored to the state before folding without easily producing wrinkle marks; and the radial shrinkage rate is low, which is very environmentally friendly, odorless, and harmless to the human body. Its elastic performance is 2-3 times stronger than that of ordinary resin compound reactions. The diamond-shaped through holes set on the cotton cloth can not only make the prepared wrinkle-proof layer very thin, but also weigh as little as 50-80 grams / m 2 , ensuring that each layer fits more closely, the shape is more fit, and does not affect breathability. The non-woven fabric on both sides can inhibit the production of bacteria.

[0130] Although the present invention has been disclosed as above with preferred embodiments, it is not intended to limit the present invention. Any person skilled in the art may make some modifications and improvements without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention shall be based on the definition of the claims.

Claims

1. A washable suit, comprising a suit body, characterized in that: The suit body comprises an anti-wrinkle layer (3), an outer fabric layer (1) is arranged on one side of the anti-wrinkle layer (3), and an inner fabric layer (4) is arranged on the other side of the anti-wrinkle layer (3); The anti-wrinkle layer (3) is made by soaking cotton cloth (7) in a polyaspartic acid ester resin solution and then subjecting it to high temperature treatment, and the cotton cloth (7) is evenly distributed with a plurality of diamond-shaped through holes (6); A non-woven fabric layer (2) is arranged between the anti-wrinkle layer (3) and the outer fabric layer (1), and a non-woven fabric layer (2) is arranged between the anti-wrinkle layer (3) and the inner fabric layer (4).

2. A washable suit according to claim 1, characterized in that: The general formula of the polyaspartic acid ester resin structure monomer is: Wherein, R is an alkyl group, and X is a straight chain or alicyclic carbon chain structure.

3. A washable suit according to claim 1, characterized in that: The anti-wrinkle layer (3) has a gram weight of 50-80 g / m 2 , the radial shrinkage rate is 1%-1.5%.

4. A washable suit according to claim 1, characterized in that: In parts by weight, the polyaspartic acid ester resin solution contains 50-60 parts of polyaspartic acid ester resin and 350-400 parts of water.

5. The washable suit according to claim 1, characterized in that: The outer fabric layer (1) comprises blended wool and polyester, with 60-70 parts by weight of wool and 30-40 parts of polyester; The inner fabric layer (4) comprises wool and polyester, with the wool comprising 60-70 parts and the polyester comprising 30-40 parts by weight; Micro-hook-shaped protrusions are formed on the outer surfaces of the outer fabric layer (1) and the inner fabric layer (4) that are in contact with the anti-wrinkle layer (3).

6. A washable suit according to claim 1, characterized in that: An inner liner cotton layer (5) is provided on the side of the inner fabric layer (4) away from the outer fabric layer (1).

7. A method for making a washable suit according to any one of claims 1 to 6, characterized in that: The steps include: S1: treating a cotton cloth (7) having a plurality of diamond-shaped through holes (6) evenly distributed thereon at high temperature using a polyaspartic acid ester resin solution to obtain an anti-wrinkle layer (3); S2: bonding the non-woven fabric (2) on both sides of the anti-wrinkle layer (3) by using an environmentally friendly water-based waterproof adhesive and a laminating machine; S3: On the side of the two layers of non-woven fabric (2) away from each other, the outer fabric layer (1) and the inner fabric layer (4) are respectively bonded by using environmentally friendly water-based waterproof glue and a laminating machine; S4: installing an inner liner cotton layer (5) on a side of the inner fabric layer (4) away from the outer fabric layer; S5: Cut the fabric obtained in S4 according to a preset size to prepare a washable suit.

8. The method for making a washable suit according to claim 7, characterized in that: The step S1 comprises the following steps: Soaking: preparing a solution with 50-60 parts of polyaspartic acid ester resin and 350-400 parts of water, and heating the solution to 120-170° C., and completely immersing the cotton cloth (7) in the solution so that the cotton cloth (7) is fully in contact with the solution; Drying: taking out the soaked cotton cloth (7) and putting it into a dryer to bake until it is dry; Bleaching: Soak the dried cotton cloth (7) in bleaching water for 20-30 minutes; Cleaning and dehydrating: the bleached cotton cloth (7) is cleaned and dehydrated.

9. The method for making a washable suit according to claim 7, characterized in that: The outer fabric layer (1) and the inner fabric layer (4) are blended from wool and polyester. During blending, the wool and polyester on one side are cut and overfed to form micro-hook-shaped protrusions. The side with the micro-hook-shaped protrusions is then bonded to the non-woven fabric (2).

10. The method for making a washable suit according to claim 7, characterized in that: In step S3, the inner fabric layer (4) is firstly evenly coated with hot melt adhesive on the anti-wrinkle layer (3) and the non-woven fabric (2) on one side thereof, and then dried at 100-120°C for 2-5 minutes. Then, the outer fabric layer (1) is evenly coated with hot melt adhesive on the anti-wrinkle layer (3) and the non-woven fabric (2) on the other side thereof, and then dried at 140-150°C for 2-5 minutes.

Citation Information

Patent Citations

  • Crease-resist cotton cloth and processing technology thereof

    CN109736085A

  • Crease-resistant fabric and preparation method thereof

    CN113564926A

  • Antibacterial and crease-resistant fabric as well as production method and application thereof

    CN115559049A

  • Rhombic linen fabric with grains

    CN211307688U

  • Novel composite cloth

    CN211363813U