Method for preparing nitrogen-doped carbon-loaded transition metal oxide catalyst by recycling waste plastics and application of nitrogen-doped carbon-loaded transition metal oxide catalyst
Preparation of nitrogen-doped carbon-supported transition metal oxide catalysts by hydrothermal method solves the problems of high cost of precious metal catalysts and poor stability of Ni-N4 coordination structure, and achieves efficient H2O2 selectivity and 2e− oxygen reduction catalysis, which is suitable for electrical The organic pollutants of the Fenton system are degraded and the use of waste plastics reduces costs.
Patent Information
- Application Number
- CN202411167295.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-29
AI Technical Summary
In the prior art, precious metal catalysts exhibit excellent catalytic activity under the electrofenton system, but their high cost limits their wide application. The poor stability of the Ni-N4 coordination structure and the uncontrollability of the synthesis process also affect the Its industrial application.
The waste plastic (PET) was prepared by hydrothermal method, and a metal organic frame (POMOF) centered on Ni atoms was prepared by carbonization, and a nitrogen-doped carbon-supported transition metal oxide catalyst was prepared, using electron modulation of coordination oxygen atoms and Ni center The spin and charge density redistribution achieves efficient H2O2 selectivity and 2e− oxygen reduction catalysis.
The catalyst exhibits more than 90% H2O2 selectivity and a theoretical limit current density close to 2e− oxygen reduction, which can efficiently degrade organic pollutants, and is cheap to use because of the use of waste plastic as raw materials, and is suitable for large-scale applications.
Smart Images

Figure CN119034821A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of preparation of catalysts for degradation of organic pollutants, and specifically relates to a method for preparing nitrogen-doped carbon-loaded transition metal oxide catalysts by recycling waste plastics and application thereof. Background Art
[0002] With the rapid advancement of industrialization, a large number of refractory organic pollutants are discharged into water bodies, causing them to remain in the water for a long time, posing a serious threat to human health. To solve this problem, the development of efficient sewage treatment technology is particularly important for protecting the water environment. Among the many sewage treatment technologies, the electro-Fenton (EF) technology stands out for its unique advantages. This technology generates H in situ through the cathode oxygen reduction reaction (ORR). 2 O 2 , and then activated into •OH, thus achieving efficient degradation of organic pollutants. − Oxygen reduction catalyst to promote H 2 O 2 The efficient production of is crucial to the EF system.
[0003] At present, noble metal and its alloy catalysts show excellent catalytic activity in EF system. However, the high cost has become a bottleneck restricting their wide application. Therefore, it is necessary to explore new high-activity and noble metal-free 2e - Oxygen reduction catalysts are particularly important. Transition metals and heteroatom nitrogen coordinated carbon-based materials (MNCs) have attracted much attention from researchers due to their abundant resources, low cost, and excellent durability in acidic environments. 4 Coordination structure, in the field of electrocatalytic ORR, with its excellent 2e - However, despite the fact that Ni-N 4 The coordination structure has excellent catalytic performance, but its poor stability and uncontrollable synthesis process still restrict its industrial application. In contrast, Ni-based oxides can well solve the above technical problems.
[0004] In view of this, the present invention uses waste polyester plastic (PET) as a precursor and prepares a Ni-centered metal organic framework (POMOF) by a hydrothermal method, thereby realizing the value-added recycling of waste plastics. POMOF is further carbonized to prepare a nitrogen-doped carbon-supported transition metal oxide catalyst. Finally, due to the electronic modulation of the coordinated oxygen atoms and the related redistribution of the spin and charge density of the Ni center, the synthesized EF catalyst has more than 90% H 2 O 2 Selectivity, close to 2e −The theoretical limiting current density of oxygen reduction confirms that the nitrogen-doped carbon-supported transition metal oxide catalyst has excellent EF performance for degradation of organic pollutants. There are currently no related reports in this regard. Summary of the invention
[0005] The technical problem solved by the present invention is to provide a simple and efficient method for preparing nitrogen-doped carbon-supported transition metal oxide catalysts from waste plastic resources. The catalyst is prepared by hydrothermal calcination. First, Na 2 WO 4 •2H 2 O and deionized water mixture was stirred until completely dissolved, phosphoric acid and glacial acetic acid were added in sequence, the precipitate was collected and filtered to dry, and the precipitate was mixed with NiCl 2 •6H 2 O was added to sodium acetate buffer and stirred, and then ethylenediamine and waste polyester plastic were added dropwise, and after continuous stirring, it was transferred to a hydrothermal reactor for hydrothermal reaction. The obtained green solid was rinsed with deionized water and ethanol, vacuum dried, and finally placed in a tube furnace for high-temperature calcination to finally obtain a nitrogen-doped carbon-supported transition metal oxide catalyst. The obtained nitrogen-doped carbon-supported transition metal oxide catalyst exhibits excellent H 2 O 2 Selective, can be used in EF degradation of organic pollutants system.
[0006] The present invention adopts the following technical solution to solve the above technical problems, a method for preparing nitrogen-doped carbon-supported transition metal oxide catalysts from waste plastic resources, characterized in that the specific process is: Step S1: Na 2 WO 4 •2H 2 O is mixed with deionized water and stirred until completely dissolved to obtain material A; Step S2: adding phosphoric acid and glacial acetic acid in sequence to the material A obtained in step S1 under stirring conditions, collecting the precipitate and filtering and drying to obtain material B; Step S3: Mix the material B obtained in step S2 with NiCl 2 •6H 2 O is added into sodium acetate buffer and stirred to mix evenly, and then ethylenediamine and waste polyester plastic are added dropwise, and stirred to mix evenly to obtain material C; Step S4: transferring the material C obtained in step S3 to a hydrothermal reactor for hydrothermal reaction at 160-200° C. for 60-80 hours, then washing the obtained green solid with deionized water and ethanol, and vacuum drying to obtain material D; Step S5: placing the material D obtained in step S4 in a tube furnace and calcining it at 500-900°C for 1-3h to finally obtain the target product, a nitrogen-doped carbon-supported transition metal oxide catalyst, which exhibits excellent H 2 O 2 Selective, can be used in electro-Fenton degradation of organic pollutants system.
[0007] The method for preparing nitrogen-doped carbon-supported transition metal oxide catalyst from waste plastic resources of the present invention is characterized by the following specific steps: Step S1: 120 g Na 2 WO 4 •2H 2 O and 150 mL of deionized water were mixed and stirred until the solid was completely dissolved to obtain material A; Step S2: Add 4.0 mL of 85 wt% phosphoric acid solution to the material A obtained in step S1 under stirring, and then add 22.5 mL of glacial acetic acid solution dropwise under vigorous stirring. After continuous stirring and mixing, collect the precipitate and filter and dry it on a glass medium to obtain material B; Step S3: Take 0.15g of material B obtained in step S2 and 0.40g of NiCl 2 •6H 2 O was added into 5 mL of 0.5 M sodium acetate buffer solution with pH = 4.8, and stirred to obtain a green solution, and then 0.15 mL of ethylenediamine and 0.10 g of waste polyester plastic were added dropwise and stirred to obtain material C; Step S4: After continuously stirring the material C obtained in step S3 for 2 hours, transfer it to a hydrothermal reactor and perform hydrothermal reaction at 180° C. for 72 hours. Rinse the obtained green solid with deionized water and ethanol and vacuum dry it to obtain material D. Step S5: The material D obtained in step S4 is heated in a nitrogen atmosphere at 5°C min −1 The temperature was raised to 600 °C at a heating rate of 2 to 3 h and carbonized for 2 to 3 h to finally obtain the target product, a nitrogen-doped carbon-supported transition metal oxide catalyst. The nitrogen-doped carbon-supported transition metal oxide catalyst has more than 90% H 2 O 2 Selectivity, close to 2e − Theoretical limiting current density for oxygen reduction.
[0008] The invention discloses an application of the nitrogen-doped carbon-supported transition metal oxide catalyst in electro-Fenton degradation of organic pollutants.
[0009] Compared with the prior art, the present invention has the following advantages and beneficial effects: 1. The present invention uses PET as a carbon precursor, which has a wide source and low price, realizes "using waste to treat pollution", and is conducive to large-scale preparation and application.
[0010] 2. The present invention prepares a metal organic framework centered on Ni atoms based on PET, and further uses Ni-POMOF as a precursor. The catalyst prepared by annealing has a three-dimensional interconnected mesoporous structure and a high specific surface area, thereby exposing more active sites and providing a convenient channel for material transport.
[0011] 3. The excellent hydrophilicity of the material of the present invention may be due to the fact that during the heat treatment process, heteroatoms such as N, O, and P in the precursor are introduced into the carbon substrate, thereby accelerating the diffusion rate of reactants and products.
[0012] 4. The catalyst prepared by the present invention has highly uniform NiO nanoparticle morphology, high specific surface area, high element doping content and high H 2 O 2 Selectivity: in the EF degradation of organic pollutants system, more than 95% of the MB solution was efficiently degraded within 20 minutes. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] Figure 1 This is a scanning electron microscope image of the product E3 prepared in Example 3; Figure 2 is a transmission electron micrograph of the product E3 prepared in Example 3; Figure 3 A diagram showing the carbon material functional group types of products E2-E4 prepared in Examples 2-4; Figure 4 The specific surface area and pore distribution diagram of the products E3-E4 prepared in Examples 3-4; Figure 5 The degradation rate diagram of the products E1-E5 prepared in Examples 1-5; DETAILED DESCRIPTION
[0014] The above contents of the present invention are further described in detail below through examples, but this should not be understood as the scope of the above subject matter of the present invention being limited to the following examples, and all technologies implemented based on the above contents of the present invention belong to the scope of the present invention. Example 1
[0015] Step S1: 120 g Na 2 WO 4 •2H2 O and 150 mL of deionized water were mixed and stirred until the solid was completely dissolved to obtain material A1; Step S2: Add phosphoric acid solution (85wt%, 4.0mL, 0.06mol) to the material A1 obtained in step S1 under stirring, and add glacial acetic acid solution (22.5mL, 0.40mol) dropwise under vigorous stirring. After continuous stirring for 1h, collect the precipitate and filter and dry it on a glass medium to obtain material B1; Step S3: Take 0.15g of the material B1 obtained in step S2 and 0.40g of NiCl 2 •6H 2 O was added into 5 mL of sodium acetate buffer (pH = 4.8, 0.5 M), stirred for 5 min to obtain a green solution, and then 0.15 mL of ethylenediamine and 0.10 g of PET (0.52 mmol, pre-cut into small pieces of 5.5 mm × 4.0 mm × 0.2 mm) were added dropwise to obtain material C1; Step S4: After continuously stirring the material C1 obtained in step S3 for 2 hours, transfer it to a 15 mL hydrothermal reactor and perform hydrothermal reaction at 180° C. for 72 hours. Rinse the obtained green solid with deionized water and ethanol, and vacuum dry it to obtain material D1; Step S5: The material D1 obtained in step S4 is heated in a nitrogen atmosphere at 5°C min −1 The temperature was raised to 500 °C and carbonized for 2 h to finally obtain product E1. Example 2
[0016] Step S1: 120 g Na 2 WO 4 •2H 2 O and 150 mL of deionized water were mixed and stirred until the solid was completely dissolved to obtain material A2; Step S2: Add phosphoric acid solution (85wt%, 4.0mL, 0.06mol) to the material A2 obtained in step S1 under stirring, and add glacial acetic acid solution (22.5mL, 0.40mol) dropwise under vigorous stirring. After continuous stirring for 1h, collect the precipitate and filter and dry it on a glass medium to obtain material B2; Step S3: Take 0.15g of material B2 obtained in step S2 and 0.40g NiCl 2 •6H 2 O was added to 5 mL of sodium acetate buffer (pH = 4.8, 0.5 M), stirred for 5 min to obtain a green solution, and then 0.15 mL of ethylenediamine and 0.10 g of PET (0.52 mmol, pre-cut into small pieces of 5.5 mm × 4.0 mm × 0.2 mm) were added dropwise to obtain material C2; Step S4: After continuously stirring the material C2 obtained in step S3 for 2 hours, transfer it to a 15 mL hydrothermal reactor and perform hydrothermal reaction at 180° C. for 72 hours. Rinse the obtained green solid with deionized water and ethanol, and vacuum dry it to obtain material D2; Step S5: The material D2 obtained in step S4 was heated in a nitrogen atmosphere at 5°C min −1 The temperature was raised to 600 °C and carbonized for 2 h to finally obtain product E2. Example 3
[0017] Step S1: 120 g Na 2 WO 4 •2H 2 O and 150 mL of deionized water were mixed and stirred until the solid was completely dissolved to obtain material A3; Step S2: Add phosphoric acid solution (85wt%, 4.0mL, 0.06mol) to the material A3 obtained in step S1 under stirring, and add glacial acetic acid solution (22.5mL, 0.40mol) dropwise under vigorous stirring. After continuous stirring for 1h, collect the precipitate and filter and dry it on a glass medium to obtain material B3; Step S3: Take 0.15g of material B3 obtained in step S2 and 0.40g NiCl 2 •6H 2 O was added into 5 mL of sodium acetate buffer (pH = 4.8, 0.5 M), stirred for 5 min to obtain a green solution, and then 0.15 mL of ethylenediamine and 0.10 g of PET (0.52 mmol, pre-cut into small pieces of 5.5 mm × 4.0 mm × 0.2 mm) were added dropwise to obtain material C3; Step S4: After continuously stirring the material C3 obtained in step S3 for 2 hours, transfer it to a 15 mL hydrothermal reactor and perform hydrothermal reaction at 180° C. for 72 hours. Rinse the obtained green solid with deionized water and ethanol, and vacuum dry it to obtain material D3; Step S5: The material D3 obtained in step S4 is heated in a nitrogen atmosphere at 5°C min −1 The temperature was raised to 700 °C and carbonized for 2 h to finally obtain product E3. Example
[0018] Step S1: 120 g Na 2 WO 4 •2H 2 O and 150 mL of deionized water were mixed and stirred until the solid was completely dissolved to obtain material A4; Step S2: Add phosphoric acid solution (85wt%, 4.0mL, 0.06mol) to the material A4 obtained in step S1 under stirring, and add glacial acetic acid solution (22.5mL, 0.40mol) dropwise under vigorous stirring. After continuous stirring for 1h, collect the precipitate and filter and dry it on a glass medium to obtain material B4; Step S3: Take 0.15g of material B4 obtained in step S2 and 0.40g NiCl 2 •6H 2 O was added into 5 mL of sodium acetate buffer (pH = 4.8, 0.5 M), stirred for 5 min to obtain a green solution, and then 0.15 mL of ethylenediamine and 0.10 g of PET (0.52 mmol, pre-cut into small pieces of 5.5 mm × 4.0 mm × 0.2 mm) were added dropwise to obtain material C4; Step S4: After continuously stirring the material C4 obtained in step S3 for 2 hours, transfer it to a 15 mL hydrothermal reactor and perform hydrothermal reaction at 180° C. for 72 hours. Rinse the obtained green solid with deionized water and ethanol, and vacuum dry it to obtain material D4; Step S5: The material D4 obtained in step S4 is heated in a nitrogen atmosphere at 5°C min −1 The temperature was raised to 800 °C and carbonized for 2 h to finally obtain product E4. Example
[0019] Step S1: 120 g Na 2 WO 4 •2H 2 O and 150 mL of deionized water were mixed and stirred until the solid was completely dissolved to obtain material A5; Step S2: phosphoric acid (85 wt%, 4.0 mL, 0.06 mol) was added to the material A5 obtained in step S1 under stirring, and glacial acetic acid (22.5 mL, 0.40 mol) was added dropwise under vigorous stirring. After continuous stirring for 1 h, the precipitate was collected and filtered and dried on a glass medium to obtain material B5; Step S3: Take 0.15g of material B5 obtained in step S2 and 0.40g NiCl 2 •6H 2 O was added to 5 mL of sodium acetate buffer (pH = 4.8, 0.5 M), stirred for 5 min to obtain a green solution, and 0.15 mL of ethylenediamine and 0.10 g of PET (0.52 mmol, pre-cut into small pieces of 5.5 mm × 4.0 mm × 0.2 mm) were added dropwise to obtain material C5; Step S4: After continuously stirring the material C5 obtained in step S3 for 2 hours, transfer it to a 15 mL hydrothermal reactor and perform hydrothermal reaction at 180° C. for 72 hours. Rinse the obtained green solid with deionized water and ethanol, and vacuum dry it to obtain material D5; Step S5: The material D5 obtained in step S4 is heated in a nitrogen atmosphere at 5°C min −1 The temperature was raised to 900 °C and carbonized for 2 h to finally obtain product E5.
[0020] Physical characterization of the obtained product: Figure 1 The scanning electron microscope image of the product E3 prepared in Example 2 shows that it has a honeycomb shape with a relatively rough surface morphology. Figure 2 Transmission electron microscopy images show that it is composed of metal nanoparticles wrapped in interconnected carbon materials, which indicates that the experimental scheme can prepare waste polyester plastic into an electro-Fenton catalyst with a specific structure. Finally, FTIR was used to verify that the wave number range was 4000~500cm −1 The functional group types of carbon materials. Figure 3 The carbon material functional group type diagram of products E2 to E4 prepared in Examples 2-4 is shown at 1057 cm −1 、1380cm −1 、1456cm −1 、1645cm −1 and 1700cm −1 The positions show obvious absorption peaks, which are attributed to COC, C-OH, CN, C=O, and OC=O respectively. Figure 4 The specific surface area and pore distribution diagrams of products E3 and E4 prepared in Examples 3 to 4 indicate that product E3 has a multi-level pore structure in which micropores and mesopores coexist, and compared with product E4, product E3 has a higher specific surface area and a larger pore structure.
[0021] Electrochemical performance test and degradation performance: Taking methylene blue as the representative pollutant, the degradation reaction was driven by an electrochemical workstation in a single-chamber electrolytic cell, and the electrolyte was N 2 / O 2 Saturated N 2 SO 4 (pH=2.0, 0.5mmol) solution. A 1cm×1cm stainless steel mesh coated with the sample, a platinum sheet of equal area, and a calomel electrode were used as the working electrode, counter electrode, and reference electrode, respectively. The linear sweep voltammetry (LSV) test was completed in a three-electrode system. The rotating disk ring electrode (RRDE) loaded with electrocatalyst, a platinum sheet (1cm 2 ) and saturated calomel electrode (Hg / HgCl 2, SCE) as working electrode, counter electrode and reference electrode respectively. The reaction electrolyte is N 2 / O 2 Saturated Na 2 SO 4 Solution (pH=2.0, 0.5mmol). Figure 5 The degradation rate diagram of products E1-E5 prepared in Examples 1-5 shows that product E2 has the best EF activity, and the degradation efficiency reaches 97% in 20 minutes.
[0022] The above embodiments describe the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The above embodiments and descriptions are only for illustrating the principles of the present invention. Without departing from the scope of the principles of the present invention, the present invention may have various changes and improvements, and these changes and improvements all fall within the scope of protection of the present invention.
Claims
1. A method for preparing nitrogen-doped carbon-supported transition metal oxide catalysts from waste plastic resources, characterized in that The specific process is: Step S1: Mix Na2WO4•2H2O and deionized water and stir until completely dissolved to obtain material A; Step S2: adding phosphoric acid and glacial acetic acid in sequence to the material A obtained in step S1 under stirring conditions, collecting the precipitate and filtering and drying to obtain material B; Step S3: adding the material B obtained in step S2 and NiCl2•6H2O into sodium acetate buffer and stirring to mix evenly, then adding ethylenediamine and waste polyester plastic dropwise, stirring to mix evenly to obtain material C; Step S4: transferring the material C obtained in step S3 to a hydrothermal reactor for hydrothermal reaction at 160-200° C. for 60-80 hours, then washing the obtained green solid with deionized water and ethanol, and vacuum drying to obtain material D; Step S5: The material D obtained in step S4 is placed in a tubular furnace and calcined at 500-900°C for 1-3 hours to finally obtain the target product, a nitrogen-doped carbon-supported transition metal oxide catalyst. The nitrogen-doped carbon-supported transition metal oxide catalyst exhibits excellent H2O2 selectivity due to the electronic modulation of the coordinated oxygen atoms and the related redistribution of the spin and charge density of the Ni center, and can be used in the electro-Fenton degradation of organic pollutants system.
2. The method for preparing nitrogen-doped carbon-supported transition metal oxide catalysts by recycling waste plastics according to claim 1, characterized in that The specific steps are: Step S1: 120 g of Na2WO4•2H2O and 150 mL of deionized water were mixed and stirred until the solid was completely dissolved to obtain material A; Step S2: Add 4.0 mL of 85 wt% phosphoric acid solution to the material A obtained in step S1 under stirring, and then add 22.5 mL of glacial acetic acid solution dropwise under vigorous stirring. After continuous stirring and mixing, collect the precipitate and filter and dry it on a glass medium to obtain material B; Step S3: 0.15 g of the material B obtained in step S2 and 0.40 g of NiCl2•6H2O were added to 5 mL of 0.5 M sodium acetate buffer solution with pH = 4.8, and stirred to obtain a green solution, and then 0.15 mL of ethylenediamine and 0.10 g of waste polyester plastic were added dropwise and stirred to obtain material C; Step S4: After continuously stirring the material C obtained in step S3 for 2 hours, transfer it to a hydrothermal reactor and perform hydrothermal reaction at 180° C. for 72 hours. Rinse the obtained green solid with deionized water and ethanol and vacuum dry it to obtain material D. Step S5: The material D obtained in step S4 is heated in a nitrogen atmosphere at 5°C min −1 The temperature was raised to 600 °C at a heating rate of 2 to 3 h and carbonized for 2 to 3 h to finally obtain the target product, a nitrogen-doped carbon-supported transition metal oxide catalyst. The nitrogen-doped carbon-supported transition metal oxide catalyst has a H2O2 selectivity of more than 90% and a near 2e − Theoretical limiting current density for oxygen reduction.
3. Use of the nitrogen-doped carbon-supported transition metal oxide catalyst prepared according to the method described in any one of claims 1 to 2 in electro-Fenton degradation of organic pollutants.