Method for preparing high-grade titanium dioxide and rutile based on titanium slag
Through the steps of sulfuric acid leaching, water leaching reaction and sodium hydroxide solution purification, combined with the treatment of high-pressure carbonization reactor, the problem of synchronous processing and extraction of titanium dioxide and rutile is solved, high-grade production and cost reduction are achieved, and the high purity of rutile is ensured. and low impurity content.
Patent Information
- Application Number
- CN202411186654.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-11-29
AI Technical Summary
The prior art lacks the synchronous processing and extraction method of titanium dioxide and rutile, and the rutile raw material cannot be effectively utilized during the acid-leakage process of high titanium slag.
High-grade titanium dioxide is prepared by sulfuric acid leaching, water leaching reaction, filtrate crystallization and roasting, and purified twice through sodium hydroxide solution and deep purification reuse solution, combined with the boost and heating treatment of the high-pressure carbonization reactor, and gradually Purified rutile.
The simultaneous high-grade production of titanium dioxide and rutile is achieved, which reduces production costs. The rutile grades obtained are all above 97%, and the Ca and Mg contents are less than 0.1%, which improves the purity and utilization rate of the product.
Smart Images

Figure CN119038598A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of titanium resource utilization, and in particular to a method for preparing high-grade titanium dioxide and rutile based on titanium slag. Background Art
[0002] Titanium is a rare metal with a high abundance in the earth's crust. However, it is dispersed in nature and difficult to extract, making it difficult to produce titanium on a large scale. With the gradual depletion of titanium ore, a non-renewable resource, people are committed to finding substitutes or improving the smelting process to improve the extraction efficiency of titanium compounds.
[0003] High titanium slag is a common name for titanium ore concentrates formed through a physical production process. Titanium ore is heated and melted in an electric furnace to melt and separate titanium dioxide and iron in the titanium ore to obtain a high-content titanium dioxide concentrate. High titanium slag is neither waste slag nor a by-product, but a high-quality raw material for the production of titanium tetrachloride, titanium dioxide and sponge titanium products. Titanium slag is smelted from titanium concentrate.
[0004] Titanium dioxide is an important inorganic chemical pigment, the main component of which is titanium dioxide. There are two production processes for titanium dioxide: sulfuric acid process and chlorination process. It is used in coatings, inks, papermaking, plastics and rubber, chemical fibers, ceramics and other industries.
[0005] Rutile is a relatively pure form of titanium dioxide, an important mineral raw material for refining titanium, but its reserves in the earth's crust are relatively small. It has excellent properties such as high temperature resistance, low temperature resistance, corrosion resistance, high strength, and low specific gravity, and is widely used in military aviation, aerospace, navigation, machinery, chemical industry, and seawater desalination. Rutile itself is one of the necessary raw materials for high-grade welding rods, and is also the best raw material for producing rutile titanium dioxide.
[0006] At present, the extraction process of titanium dioxide is generally based on acid leaching, and the purification process of rutile is mainly based on wet process. The main methods include reduction-rusting method, hydrochloric acid leaching method, sulfuric acid leaching method, etc., which can obtain high-grade rutile. However, there is still a lack of relevant research on the simultaneous processing and extraction of titanium dioxide and rutile. At the same time, there are some raw materials that can be used to extract rutile during the acid leaching of high-titanium slag. Therefore, the simultaneous processing and extraction of titanium dioxide and rutile needs further improvement and optimization. Summary of the invention
[0007] In view of the above problems, the present invention provides a method for preparing high-grade titanium dioxide and rutile based on titanium slag.
[0008] The technical solution of the present invention is:
[0009] A method for preparing high-grade titanium dioxide and rutile based on titanium slag, comprising:
[0010] S1, sulfuric acid leaching: leaching the titanium slag with concentrated sulfuric acid;
[0011] S2. Water immersion reaction: adding ultrapure water for water immersion reaction to obtain slurry;
[0012] S3, titanium dioxide preparation: filtering the slurry to obtain filter residue and filtrate;
[0013] The filtrate is crystallized to obtain a titanyl sulfate solution, the titanyl sulfate solution is hydrolyzed at 90-100° C. for 1-3 hours to form metatitanic acid, and the metatitanic acid is roasted for 1-2 hours to obtain titanium dioxide;
[0014] S4, crude extraction of filter residue: the filter residue obtained in S3 is washed and dried with distilled water, completely immersed in a hydrochloric acid solution, then heated to 100-140°C, and stirred for reaction for 0.5-3h to acid-hydrolyze the hydrochloric acid solution to obtain a crude extraction mixture, and then the crude mixture is filtered to obtain a crude extraction residue and a crude extract, and the crude extraction residue is washed and dried with distilled water, and then roasted to form a crude extraction oxide rich in iron, magnesium and calcium;
[0015] S5. Rutile purification: The crude oxide is subjected to primary purification and secondary purification to obtain a first high-grade rutile and a second high-grade rutile, respectively.
[0016] Further, in S5, the method for purifying rutile is:
[0017] S5-1, primary purification: the crude oxide is divided into 15 parts, 9 to 12 parts are placed in a sealable reactor, sodium hydroxide solution is added, and the solid-liquid ratio of the crude oxide to the sodium hydroxide solution is 1g:2.5 to 5mL, then the temperature is raised to 100 to 130°C for reaction for 1 to 3h, and the primary insoluble matter and the recycled filtrate are obtained by filtering, and the primary insoluble matter is washed with distilled water and dried to obtain the first high-grade rutile;
[0018] S5-2, deep purification and reuse: the reuse filtrate is placed in a high-pressure carbonization reactor and CO is introduced 2 gas, and gradually pressurize the high-pressure carbonization reactor to 7.5-8MPa, raise the temperature to 65-70°C, form a reaction system, adjust the pH value of the reaction system to 8-8.5, continue the reaction for 0.5-1h, filter to obtain silica gel, dissolve the silica gel in ammonium fluoride solution, the solid-liquid ratio of silica gel to ammonium fluoride solution is 1g:3-4mL, stir and pass ammonia to obtain a solid-liquid mixture, filter to remove solids, obtain a purified liquid, age the purified liquid, evaporate and concentrate, then pass hydrofluoric acid to react, the volume ratio of the purified liquid to hydrofluoric acid is 2:1, and react for 1-2h to obtain a deeply purified reuse liquid;
[0019] S5-3, secondary purification: place the remaining 3 to 6 portions of the crude oxide in S5-1 in a reactor, add the deep purification recycling liquid prepared in S5-2, the solid-liquid ratio of the crude oxide to the deep purification recycling liquid is 1 g: 2 to 3 mL, react at room temperature for 1 to 3 hours, filter to obtain secondary insoluble matter, wash the secondary insoluble matter with distilled water and dry to obtain the second highest grade rutile.
[0020] Furthermore, the titanium slag in S1 is completely immersed in concentrated sulfuric acid with a mass fraction of more than 95%, and is continuously stirred and reacted for 0.5 to 3 hours under high temperature heating. The stirring rate of the stirring reaction is 300 to 400 rpm, and the high temperature heating temperature is 230 to 270°C.
[0021] Furthermore, ultrapure water is added to S2 for water leaching reaction to reduce the mass concentration of concentrated sulfuric acid to 50-70%, the water leaching reaction temperature is 60-90° C., and the water leaching reaction time is 1-3 hours.
[0022] Furthermore, the crystallization in S3 is to evaporate the filtrate at 130-150°C, condense the evaporated gas and reflux it into the reaction container to obtain a titanyl sulfate solution, and the calcination temperature is 850-950°C.
[0023] Note: Iron sulfate and magnesium sulfate in the filtrate can be effectively removed by evaporation crystallization.
[0024] Furthermore, in S4, the number of times of distilled water washing is 3 to 4 times, the drying temperature is 100 to 105° C., the mass fraction of the hydrochloric acid solution is 30 to 40%, and the stirring rate of the stirring reaction is 300 to 400 rpm.
[0025] Furthermore, in S4, the crude extract is evaporated and concentrated at 100°C to obtain a hydrochloric acid concentrate for recycling, and the roasting temperature is 850-950°C.
[0026] Description: By evaporating and concentrating the crude extract for reuse, the utilization rate can be improved and the cost can be saved.
[0027] Furthermore, the mass fraction of the sodium hydroxide solution in S5-1 is 40-60%, and the drying temperatures in S5-1 and S5-3 are both 100-105°C.
[0028] Description: The crude oxide is processed by optimizing the sodium hydroxide solution to obtain high-grade rutile.
[0029] Furthermore, the pressurization rate of the high-pressure carbonization reactor in S5-2 is 0.2-0.3 MPa / min, the heating rate is 3-5°C / min, and the pH value of the reaction system is adjusted by using a hydrochloric acid solution with a mass fraction of 20-30%, or a sodium hydroxide solution with a mass fraction of 20-30%. The silica gel obtained after filtration is washed three times with anhydrous ethanol.
[0030] Note: By limiting the pressurization speed and heating speed of the high-pressure carbonization reactor, the CO 2 The gas gradually becomes supercritical, and when CO 2 When the gas is in a gaseous state, it can react with the recycled filtrate to first precipitate a portion of the precipitate, while carrying out some impurity salts. When it fully reaches the supercritical state, the obtained silica gel is purer, thus providing support for the subsequent secondary purification of high-grade rutile.
[0031] Furthermore, the mass fraction of hydrofluoric acid in S5-2 is 40-60%, and the amount of ammonia introduced is 0.05-0.1m 3 / h.
[0032] The beneficial effects of the present invention are:
[0033] (1) The method for preparing high-grade titanium dioxide and rutile based on titanium slag of the present invention can simultaneously produce high-grade titanium dioxide and rutile, and utilizes the crude oxide produced in the production of titanium dioxide as the raw material of rutile, which is divided into two parts and purified twice with sodium hydroxide solution and deep purification recycling liquid (mainly composed of ammonium bifluoride), respectively. It not only takes advantage of the easy storage and low cost of sodium hydroxide solution, but also extracts the deep purification recycling liquid from the by-product of the sodium hydroxide solution reaction and continuously applies it to the secondary rutile purification. At the same time, it also takes advantage of the easy reaction and low energy demand of ammonium bifluoride as an extractant, further reducing the overall cost. The grades of the two types of rutile produced are both above 97%, and the Ca and Mg contents are less than 0.1%.
[0034] (2) The method of preparing high-grade titanium dioxide and rutile based on titanium slag of the present invention adopts supercritical CO 2 The recycled filtrate is purified by gradually increasing the gas pressure to obtain pure silica gel, which provides a guarantee for the subsequent secondary purification of rutile. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 This is a flow chart of a method for preparing high-grade titanium dioxide and rutile based on titanium slag of the present invention;
[0036] Figure 2It is a schematic diagram comparing the grades of the second highest grade rutile prepared by Example 13 and Comparative Examples 1 and 2 in Experimental Example 3 of the present invention. DETAILED DESCRIPTION
[0037] Example 1
[0038] A method for preparing high-grade titanium dioxide and rutile based on titanium slag comprises the following steps:
[0039] S1. Sulfuric acid leaching: place the titanium slag in a reaction vessel, add concentrated sulfuric acid into the reaction vessel, completely immerse the titanium slag in the concentrated sulfuric acid, the mass fraction of the concentrated sulfuric acid is more than 98%, heat to 240°C, continue stirring and react for 1.5h, and the stirring rate of the stirring reaction is 350rpm;
[0040] S2. Water immersion reaction: ultrapure water is added to the reaction container for water immersion reaction, the volume ratio of ultrapure water to concentrated sulfuric acid is 1.8:1, the water immersion reaction temperature is 75° C., the water immersion reaction time is 2 h, and a slurry is obtained;
[0041] S3, titanium dioxide preparation: filtering the slurry to obtain a filter residue and a filtrate, and crystallizing the filtrate to obtain a titanyl sulfate solution, wherein the crystallization is performed by evaporating the filtrate at 140° C., condensing the evaporated gas and refluxing it into a reaction container to obtain a titanyl sulfate solution, and hydrolyzing the titanyl sulfate solution at 95° C. for 2 h to form metatitanic acid, and then roasting the metatitanic acid at 900° C. for 1.5 h to obtain titanium dioxide;
[0042] S4, crude extraction of filter residue: wash the filter residue with distilled water, then dry it at 102°C, add hydrochloric acid solution to the dried filter residue to obtain a crude extraction system, the mass fraction of the hydrochloric acid solution is 35%, the mass concentration of the hydrochloric acid solution in the crude extraction system is 15%, and the remainder is the filter residue, then heat to 120°C, continue stirring and react for 2h, the stirring rate of the stirring reaction is 350rpm, and the hydrochloric acid solution is acidolyzed to obtain a crude extraction mixture, then filter the crude mixture to obtain a crude extraction residue and a crude extract, wash the crude extraction residue with distilled water for 3 times, and after drying at 102°C, roast it to form a crude extraction oxide rich in iron, magnesium and calcium, and evaporate and concentrate the crude extract at 100°C to obtain a hydrochloric acid concentrate for reuse;
[0043] S5. Rutile purification: The purification of rutile includes primary purification and secondary purification to obtain the first high-grade rutile and the second high-grade rutile;
[0044] S5-1, primary purification: the crude oxide is divided into 15 parts, 9 to 12 parts are placed in a sealable reactor, sodium hydroxide solution is added, the mass fraction of the sodium hydroxide solution is 40 to 60%, and the solid-liquid ratio of the crude oxide to the sodium hydroxide solution is 1g:2.5 to 5mL, then the temperature is raised to 100 to 130°C for reaction for 1 to 3h, and the primary insoluble matter and the recycled filtrate are obtained by filtering, the primary insoluble matter is washed with distilled water, and then dried at 100 to 105°C to obtain the first high-grade rutile;
[0045] S5-2, deep purification and reuse: the reused filtrate is placed in a high-pressure carbonization reactor and CO is introduced 2 Gas, and gradually increase the pressure of the high-pressure carbonization reactor to 7.5-8MPa, the temperature rises to 65-70°C, a reaction system is formed, the pH value of the reaction system is adjusted to 8-8.5, the reaction is continued for 0.5-1h, and silica gel is obtained after filtration. The pressure increase rate of the high-pressure carbonization reactor is 0.2-0.3MPa / min, the heating rate is 3-5°C / min, and the pH value of the reaction system is adjusted to use a hydrochloric acid solution with a mass fraction of 20-30%, or a sodium hydroxide solution with a mass fraction of 20-30%. The silica gel obtained after filtration is washed three times with anhydrous ethanol, and the silica gel is dissolved in an ammonium fluoride solution. The solid-liquid ratio of the silica gel to the ammonium fluoride solution is 1g:3-4mL. Stir and introduce ammonia gas, and the amount of ammonia introduced is 0.05-0.1m 3 / h, to obtain a solid-liquid mixture, filter to remove solids, obtain a purified liquid, age the purified liquid, evaporate and concentrate it, then introduce hydrofluoric acid to react, the mass fraction of hydrofluoric acid is 40-60%, the volume ratio of the purified liquid to the hydrofluoric acid is 2:1, and after reacting for 1-2h, a deeply purified reuse liquid is obtained;
[0046] S5-3. Secondary purification: place the remaining 3 to 6 parts of crude oxide in S5-1 in a reactor, add the deep purification recycling liquid prepared in S5-2, the solid-liquid ratio of crude oxide to deep purification recycling liquid is 1g:2-3mL, react at room temperature for 1-3h, filter to obtain secondary insoluble matter, wash the secondary insoluble matter with distilled water, and then dry at 100-105°C to obtain the second highest grade rutile.
[0047] Example 2
[0048] The difference between this embodiment and embodiment 1 is that:
[0049] S1. Sulfuric acid leaching: place titanium slag in a reaction vessel, add concentrated sulfuric acid into the reaction vessel, completely immerse the titanium slag in the concentrated sulfuric acid, the mass fraction of the concentrated sulfuric acid is 97%, heat to 230°C, continue stirring the reaction for 3 hours, and the stirring rate of the stirring reaction is 300 rpm.
[0050] Example 3
[0051] The difference between this embodiment and embodiment 1 is that:
[0052] S1. Sulfuric acid leaching: place titanium slag in a reaction vessel, add concentrated sulfuric acid into the reaction vessel, completely immerse the titanium slag in the concentrated sulfuric acid, the mass fraction of the concentrated sulfuric acid is 96%, heat to 270°C, continue stirring the reaction for 0.5h, and the stirring rate of the stirring reaction is 400rpm.
[0053] Note: In Examples 1 to 3, three groups of specific parameter settings for sulfuric acid leaching are mainly given. When the amount of concentrated sulfuric acid added and the reaction temperature are both high, the reaction time and stirring rate can be appropriately reduced, and appropriate parameters can be selected according to needs.
[0054] Example 4
[0055] The difference between this embodiment and embodiment 1 is that:
[0056] S2. Water immersion reaction: ultrapure water is added to the reaction container for water immersion reaction, the volume ratio of ultrapure water to concentrated sulfuric acid is 1.5:1, the water immersion reaction temperature is 60° C., the water immersion reaction time is 3 h, and a slurry is obtained.
[0057] Example 5
[0058] The difference between this embodiment and embodiment 1 is that:
[0059] S2. Water immersion reaction: ultrapure water is added to the reaction container for water immersion reaction, the volume ratio of ultrapure water to concentrated sulfuric acid is 2:1, the water immersion reaction temperature is 90° C., the water immersion reaction time is 1 h, and a slurry is obtained.
[0060] Note: Example 1, Example 4 and Example 5 mainly provide three groups of specific parameter settings for water immersion reactions. When a large amount of ultrapure water is added, the reaction time can be appropriately reduced, and the temperature can be adjusted within the temperature range provided in the three groups of examples as needed.
[0061] Example 6
[0062] The difference between this embodiment and embodiment 1 is that:
[0063] S3. Preparation of titanium dioxide: Filter the slurry to obtain filter residue and filtrate, and crystallize the filtrate to obtain titanyl sulfate solution. The crystallization is to evaporate the filtrate at 130°C, condense the evaporated gas and reflux it into the reaction container to obtain titanyl sulfate solution, hydrolyze the titanyl sulfate solution at 90°C for 3h to form metatitanic acid, and calcine the metatitanic acid at 850°C for 2h to obtain titanium dioxide.
[0064] Example 7
[0065] The difference between this embodiment and embodiment 1 is that:
[0066] S3. Preparation of titanium dioxide: Filter the slurry to obtain filter residue and filtrate, and crystallize the filtrate to obtain titanyl sulfate solution. The crystallization is to evaporate the filtrate at 150°C, condense the evaporated gas and reflux it into the reaction container to obtain titanyl sulfate solution, hydrolyze the titanyl sulfate solution at 100°C for 1 hour to form metatitanic acid, and calcine the metatitanic acid at 950°C for 1 hour to obtain titanium dioxide.
[0067] Note: Example 1, Example 6 and Example 7 mainly provide three groups of specific titanium dioxide preparation parameter settings. When a higher hydrolysis temperature is selected, the hydrolysis time is appropriately reduced. When a higher roasting temperature is selected, the roasting time is appropriately reduced, and vice versa.
[0068] Example 8
[0069] The difference between this embodiment and embodiment 1 is that:
[0070] S4. Crude extraction of filter residue: wash the filter residue with distilled water, and then dry it at 100°C, add hydrochloric acid solution to the dried filter residue to obtain a crude extraction system, the mass fraction of the hydrochloric acid solution is 30%, the mass concentration of the hydrochloric acid solution in the crude extraction system is 10%, and the remainder is the filter residue, then heat to 100°C, continue stirring and react for 3 hours, the stirring rate of the stirring reaction is 300 rpm, and the hydrochloric acid solution is acidolyzed to obtain a crude extraction mixture, and then the crude mixture is filtered to obtain a crude extraction residue and a crude extract, the crude extraction residue is washed with distilled water for 3 times, and after drying at 100°C, it is calcined to form a crude extraction oxide rich in iron, magnesium and calcium, and the crude extract is evaporated and concentrated at 100°C to obtain a hydrochloric acid concentrate for reuse.
[0071] Example 9
[0072] The difference between this embodiment and embodiment 1 is that:
[0073] S4. Crude extraction of filter residue: wash the filter residue with distilled water, and then dry it at 105°C, add hydrochloric acid solution to the dried filter residue to obtain a crude extraction system, the mass fraction of the hydrochloric acid solution is 40%, the mass concentration of the hydrochloric acid solution in the crude extraction system is 20%, and the remainder is the filter residue, then heat to 140°C, continue stirring and react for 0.5h, the stirring rate of the stirring reaction is 400rpm, and the hydrochloric acid solution is acidolyzed to obtain a crude extraction mixture, and then the crude mixture is filtered to obtain a crude extraction residue and a crude extract, the crude extraction residue is washed with distilled water 4 times, and after drying at 105°C, it is calcined to form a crude extraction oxide rich in iron, magnesium and calcium, and the crude extract is evaporated and concentrated at 100°C to obtain a hydrochloric acid concentrate for reuse.
[0074] Note: The parameter adjustments in Example 1, Example 6 and Example 7 are conventional parameter adjustments for crude extraction of filter residues. The same extraction effect can be achieved by selecting the parameters in any one of the examples.
[0075] Example 10
[0076] The difference between this embodiment and embodiment 1 is that:
[0077] S5-1, primary purification: the crude oxide is divided into 15 parts, 9 parts are placed in a sealable reactor, sodium hydroxide solution is added, the mass fraction of the sodium hydroxide solution is 40-60%, and the solid-liquid ratio of the crude oxide to the sodium hydroxide solution is 1g:2.5mL, then the temperature is raised to 100°C for reaction for 3h, and the primary insoluble matter and the recycled filtrate are obtained by filtering, the primary insoluble matter is washed with distilled water, and then dried at 100°C to obtain the first high-grade rutile;
[0078] S5-3. Secondary purification: The remaining 6 portions of crude oxide in S5-1 are placed in a reactor, and the deep purification recycling liquid prepared in S5-2 is added, the solid-liquid ratio of crude oxide to deep purification recycling liquid is 1g:2mL, and the reaction is carried out at room temperature for 3h, and the secondary insoluble matter is obtained by filtration. The secondary insoluble matter is washed with distilled water and then dried at 100°C to obtain the second highest grade rutile.
[0079] Embodiment 11
[0080] The difference between this embodiment and embodiment 1 is that:
[0081] S5-1, primary purification: the crude oxide is divided into 15 parts, 12 parts are placed in a sealable reactor, sodium hydroxide solution is added, the mass fraction of the sodium hydroxide solution is 60%, and the solid-liquid ratio of the crude oxide to the sodium hydroxide solution is 1g:5mL, then the temperature is raised to 130°C for reaction for 1h, and the primary insoluble matter and the recycled filtrate are obtained by filtering, the primary insoluble matter is washed with distilled water, and then dried at 105°C to obtain the first high-grade rutile;
[0082] S5-3. Secondary purification: The remaining 3 portions of crude oxide in S5-1 are placed in a reactor, and the deep purification recycling liquid prepared in S5-2 is added. The solid-liquid ratio of the crude oxide to the deep purification recycling liquid is 1g:3mL. The mixture is reacted at room temperature for 1h, and the secondary insoluble matter is obtained by filtration. The secondary insoluble matter is washed with distilled water and then dried at 105°C to obtain the second highest grade rutile.
[0083] Example 12
[0084] The difference between this embodiment and embodiment 1 is that:
[0085] S5-2, deep purification and reuse: the reused filtrate is placed in a high-pressure carbonization reactor and CO is introduced 2 Gas, and gradually pressurize the high-pressure carbonization reactor to 7.5MPa, raise the temperature to 65°C, form a reaction system, adjust the pH value of the reaction system to 8, continue the reaction for 0.5h, and obtain silica gel after filtration. The pressurization rate of the high-pressure carbonization reactor is 0.2MPa / min, and the heating rate is 3°C / min. A 20% by mass hydrochloric acid solution or a 20% by mass sodium hydroxide solution is used to adjust the pH value of the reaction system. The silica gel obtained after filtration is washed three times with anhydrous ethanol, and the silica gel is dissolved in an ammonium fluoride solution. The solid-liquid ratio of silica gel to ammonium fluoride solution is 1g:3mL. Stir and introduce ammonia gas, and the amount of ammonia introduced is 0.05m 3 / h to obtain a solid-liquid mixture, filter to remove solids, obtain a purified liquid, age the purified liquid, evaporate and concentrate it, then introduce hydrofluoric acid to react, the mass fraction of hydrofluoric acid is 40%, the volume ratio of the purified liquid to hydrofluoric acid is 2:1, and after reacting for 1h, a deeply purified reuse liquid is obtained.
[0086] Embodiment 13
[0087] The difference between this embodiment and embodiment 1 is that:
[0088] S5-2, deep purification and reuse: the reused filtrate is placed in a high-pressure carbonization reactor and CO is introduced 2 Gas, and gradually pressurize the high-pressure carbonization reactor to 8MPa, raise the temperature to 70°C to form a reaction system, adjust the pH value of the reaction system to 8.5, continue the reaction for 1h, and obtain silica gel after filtration. The pressurization rate of the high-pressure carbonization reactor is 0.3MPa / min, and the heating rate is 5°C / min. A 30% by mass hydrochloric acid solution or a 30% by mass sodium hydroxide solution is used to adjust the pH value of the reaction system. The silica gel obtained after filtration is washed three times with anhydrous ethanol, and the silica gel is dissolved in an ammonium fluoride solution. The solid-liquid ratio of silica gel to ammonium fluoride solution is 1g:4mL. Stir and introduce ammonia gas, and the amount of ammonia introduced is 0.1m 3 / h to obtain a solid-liquid mixture, filter to remove solids, obtain a purified liquid, age the purified liquid, evaporate and concentrate it, then introduce hydrofluoric acid to react, the mass fraction of hydrofluoric acid is 60%, the volume ratio of the purified liquid to hydrofluoric acid is 2:1, and after reacting for 2h, a deeply purified reuse liquid is obtained.
[0089] Experimental Example 1
[0090] Next, we tested the grades of titanium dioxide and rutile prepared in Example 1. The results are shown in Table 1.
[0091] Table 1 Titanium dioxide and rutile grade prepared in Example 1
[0092]
[0093]
[0094] It can be seen that the titanium dioxide and two rutiles prepared by the method in Example 1 have high grades, reaching more than 97%, among which the grade of the first high-grade rutile is higher than that of the second high-grade rutile. This is because some impurities may still exist in the deep purification recycling liquid in Example 1, which affects the grade of the second high-grade rutile. However, considering the cost factor comprehensively, the method in Example 1 is 20-30% lower in cost than directly using ammonium bifluoride instead of deep purification recycling liquid. After testing, the Ca and Mg contents of the three products are less than 0.1%.
[0095] Experimental Example 2
[0096] Next, we compare the first high-grade rutile and the second high-grade rutile prepared in Example 1, Example 10 and Example 11 as well as the recovery rate. The results are shown in Table 2.
[0097] Table 2 Comparison of the first high-grade rutile and the second high-grade rutile in Example 1, Example 10 and Example 11
[0098]
[0099] It can be seen from the data in Table 2 that by adjusting the amount of crude oxide used in the subsequent extraction method, the grade and recovery rate of the second highest grade rutile are mainly affected to a certain extent. When more crude oxide is applied to the secondary purification in Example 10, the grade of the prepared second highest grade rutile decreases, but the recovery rate remains at a high level. When less crude oxide is applied to the secondary purification in Example 11, the grade of the prepared second highest grade rutile is improved, but the recovery rate decreases slightly. This is because the raw materials for the secondary purification are based on the primary purification. When the raw materials produced by the primary purification are small, the quality of the secondary purification will be affected, and additional ammonium bifluoride may be required. When the raw materials for the primary purification are more, the raw materials produced synchronously are also more, and the quality of the secondary purification is correspondingly improved, but it will also cause a part of the raw materials to be wasted. Overall, the cost difference between the three is not large, and the difference in grade and recovery rate is also small. Any one parameter in the three groups of embodiments given in the present invention can be selected, and the preparation parameters in Example 1 are preferred.
[0100] Experimental Example 3
[0101] Next, we tested the second highest grade rutile prepared in Example 13. For comparison, we set up two comparative examples for comparison. In Comparative Example 1, we did not use the deep purification and recycling method of gradually increasing pressure and temperature, but directly added raw materials after the high-pressure carbonization reactor reached supercritical conditions, so that the reaction was always in supercritical CO. 2 In Comparative Example 2, we used CO 2 The gas reacts and the experimental results are as follows Figure 2 shown.
[0102] It can be seen that the grade of the second highest grade rutile can be further improved by adopting the stepwise pressurization and temperature increase method of the present invention. This is probably because the pressure increase rate and temperature increase rate of the high-pressure carbonization reactor are limited, so that the CO 2 The gas gradually becomes supercritical, and when CO 2 When the gas is in a gaseous state, it can react with the recycled filtrate to first precipitate a portion of the precipitate, while carrying out some impurity salts. When it fully reaches the supercritical state, the obtained silica gel is purer, thus providing support for the subsequent secondary purification of high-grade rutile.
Claims
1. A method for preparing high-grade titanium dioxide and rutile based on titanium slag, comprising: S1, sulfuric acid leaching: leaching the titanium slag with concentrated sulfuric acid; S2. Water immersion reaction: adding ultrapure water for water immersion reaction to obtain slurry; S3, titanium dioxide preparation: filtering the slurry to obtain filter residue and filtrate; The method is characterized in that the filtrate is crystallized to obtain a titanyl sulfate solution, the titanyl sulfate solution is hydrolyzed at 90-100° C. for 1-3 hours to form metatitanic acid, and the metatitanic acid is roasted for 1-2 hours to obtain titanium dioxide; S4, crude extraction of filter residue: the filter residue obtained in S3 is washed and dried with distilled water, completely immersed in a hydrochloric acid solution, heated to 100-140° C., stirred and reacted for 0.5-3 h, filtered to obtain a crude extraction residue and a crude extract, washed and dried with distilled water, and then calcined to form a crude extraction oxide rich in iron, magnesium and calcium; S5. Rutile purification: The crude oxide is subjected to primary purification and secondary purification to obtain a first high-grade rutile and a second high-grade rutile, respectively.
2. A method for preparing high-grade titanium dioxide and rutile based on titanium slag as claimed in claim 1, characterized in that: In S5, the method for purifying rutile is: S5-1, primary purification: the crude oxide is divided into 15 parts, 9 to 12 parts are placed in a sealable reactor, sodium hydroxide solution is added, the temperature is raised for reaction, and then filtered to obtain a primary insoluble matter and a reused filtrate, and the primary insoluble matter is washed with distilled water and dried to obtain a first high-grade rutile; The solid-liquid ratio of the crude oxide to the sodium hydroxide solution is 1 g: 2.5-5 mL, the heating temperature is 100-130° C., and the reaction time is 1-3 h. S5-2, deep purification and reuse: the reuse filtrate is placed in a high-pressure carbonization reactor, CO2 gas is introduced, the pressure and temperature are gradually increased and the reaction is continued for 0.5 to 1 hour, and silica gel is obtained after filtration, the silica gel is dissolved in an ammonium fluoride solution, stirred and ammonia gas is introduced to obtain a solid-liquid mixture, solids are removed by filtration to obtain a purified liquid, the purified liquid is aged and evaporated and concentrated, and then hydrofluoric acid is introduced to react to obtain a deeply purified reuse liquid; The high-pressure carbonization reactor is gradually pressurized to 7.5-8 MPa, the temperature is raised to 65-70°C, the pH value of the reaction system is adjusted to 8-8.5, the reaction is continued for 0.5-1h, the solid-liquid ratio of silica gel to ammonium fluoride solution is 1g:3-4mL, the volume ratio of the purification liquid to hydrofluoric acid is 2:1, and the reaction time is 1-2h; S5-3, secondary purification: the remaining 3 to 6 parts of the crude oxide in S5-1 are placed in a reactor, the deep purification recycling liquid prepared in S5-2 is added, reacted at room temperature, filtered to obtain secondary insoluble matter, the secondary insoluble matter is washed with distilled water and dried to obtain the second highest grade rutile. The solid-liquid ratio of the crude oxide to the deep purification recycled liquid is 1 g: 2-3 mL, and the reaction is carried out at room temperature for 1-3 hours.
3. The method for preparing high-grade titanium dioxide and rutile based on titanium slag according to claim 1, characterized in that: The titanium slag in S1 is completely immersed in concentrated sulfuric acid with a mass fraction of more than 95%. The high-temperature heating is continued with stirring for 0.5 to 3 hours. The stirring rate of the stirring reaction is 300 to 400 rpm and the high-temperature heating temperature is 230 to 270°C.
4. The method for preparing high-grade titanium dioxide and rutile based on titanium slag according to claim 1, characterized in that: Ultrapure water is added to the S2 for water leaching reaction to reduce the mass concentration of concentrated sulfuric acid to 50-70%, the water leaching reaction temperature is 60-90° C., and the water leaching reaction time is 1-3 hours.
5. The method for preparing high-grade titanium dioxide and rutile based on titanium slag according to claim 1, characterized in that: The crystallization in S3 is to evaporate the filtrate at 130-150°C, condense the evaporated gas and reflux it into the reaction container to obtain titanyl sulfate solution, and the roasting temperature is 850-950°C.
6. The method for preparing high-grade titanium dioxide and rutile based on titanium slag according to claim 1, characterized in that: In the S4, the washing times of distilled water are 3 to 4 times, the drying temperature is 100 to 105° C., the mass fraction of the hydrochloric acid solution is 30 to 40%, and the stirring speed of the stirring reaction is 300 to 400 rpm.
7. The method for preparing high-grade titanium dioxide and rutile based on titanium slag according to claim 1, characterized in that: In S4, the crude extract is evaporated and concentrated at 100°C to obtain a hydrochloric acid concentrate for recycling, and the roasting temperature is 850-950°C.
8. The method for preparing high-grade titanium dioxide and rutile based on titanium slag according to claim 2, characterized in that: The mass fraction of the sodium hydroxide solution in S5-1 is 40-60%, and the drying temperatures in S5-1 and S5-3 are both 100-105°C.
9. The method for preparing high-grade titanium dioxide and rutile based on titanium slag according to claim 2, characterized in that: The pressurization rate of the S5-2 medium-pressure carbonization reactor is 0.2-0.3 MPa / min, the heating rate is 3-5°C / min, and the pH value of the reaction system is adjusted by using a hydrochloric acid solution with a mass fraction of 20-30%, or a sodium hydroxide solution with a mass fraction of 20-30%. The silica gel obtained after filtration is washed three times with anhydrous ethanol.
10. The method for preparing high-grade titanium dioxide and rutile based on titanium slag according to claim 2, characterized in that: The mass fraction of hydrofluoric acid in S5-2 is 40-60%, and the amount of ammonia introduced is 0.05-0.1m 3 / h.