Method for preparing battery grade ferrous sulfate by taking copper smelting tailings as raw material through conversion method

By using steps such as leaching, reducing, neutralizing and deweighting and iron depositing in copper sludge, the problem of difficult removal of impurities in copper sludge was successfully solved, and efficient and low-cost battery-grade ferrous sulfate preparation was achieved. , simplifies the process flow and improves resource utilization efficiency.

CN119038620APending Publication Date: 2024-11-29GUANGXI HUIJIN NEW ENERGY CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411174107.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-29

Smart Images

  • Figure CN119038620A_ABST
    Figure CN119038620A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of hydrometallurgy, and discloses a method for preparing battery grade ferrous sulfate by taking copper smelting tailings as a raw material through a conversion method, which comprises the following steps: S1, proportioning the copper smelting tailings and concentrated sulfuric acid, adding hydrated slurry for reaction leaching, and filtering to obtain a leaching solution; s2, adding a reducing agent to reduce the concentration of Fe < 3 + > ions in the leachate; s3, metering and adding hydrogen sulfide and alkali into the solution in the step S2, precipitating impurities, and filtering to remove slag to obtain filtrate; s4, continuously metering and introducing hydrogen sulfide and alkali into the filtrate in the step 3, filtering and washing to obtain FeS precipitate; and S5, adding acid into the FeS precipitate for re-dissolution to prepare a pure ferrous sulfate nearly saturated solution, and performing freezing crystallization and centrifugal separation to obtain a battery-grade ferrous sulfate product. According to the method, the copper smelting tailings are used as raw materials to prepare the ferrous sulfate through a conversion method, impurity element ions which are high in content and difficult to remove in the ferrous sulfate solution can be removed, and the battery-grade ferrous sulfate solution is prepared.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of hydrometallurgy, and in particular relates to a method for preparing battery-grade ferrous sulfate by a conversion method using copper smelting tailings as raw materials. Background Art

[0002] Copper smelting tailings are secondary tailings discarded after copper selection from copper smelting slag. In the copper production process, about 2.2 tons of copper smelting tailings are produced for every ton of copper produced. According to incomplete statistics, the annual copper tailings produced in the world and China are about 36 million tons and 16 million tons respectively, and the historical cumulative amount is as high as 300 million tons and 130 million tons, which wastes a lot of land resources, not only causing the waste and loss of valuable metal resources such as iron and zinc, but also causing serious pollution to groundwater, soil and atmosphere. Its main mineral components are amorphous glass composed of fayalite (2FeO﹒SiO2), magnetite (Fe3O4) and some gangue, with an iron content of about 40% and a silicon dioxide content of about 30%. Because the iron content does not meet the requirements of steelmaking raw materials, it can only be used as an iron-enhancing agent for cement production at present, with an ex-factory price of 2 to 10 yuan / ton. The metal recovery and resource comprehensive utilization of copper smelting tailings have always been an industry problem.

[0003] Battery-grade ferrous sulfate refers to ferrous sulfate heptahydrate with strictly controlled impurities such as potassium, sodium, calcium, magnesium, aluminum, copper, zinc, and lead. It is mainly used for positive electrode materials of lithium iron phosphate (manganese) battery grade and sodium ion battery grade, with a market price of about 2,500 yuan / ton. As lithium iron phosphate batteries become the mainstream of electric vehicles and energy storage, their iron source mainly comes from ferrous sulfate. In 2023, the domestic output of lithium iron phosphate positive electrode materials will be 1.56 million tons, which is equivalent to 1.6 million tons of battery-grade ferrous sulfate. In 2023, China's sales of new energy passenger vehicles will be 8.5 million, and the penetration rate of new energy vehicles will be about 36%. In 2023, China's cumulative installed capacity of energy storage batteries will be about 32GWH, accounting for as much as 38% of all types of energy storage. With the vigorous development of the electric vehicle and energy storage markets, the market demand for ferrous sulfate will further expand.

[0004] However, there are many difficulties in the process of leaching copper slag to prepare battery-grade ferrous sulfate. Because of its unique phase composition, which is mainly an amorphous glass composed of fayalite (2FeO﹒SiO2), magnetite (Fe3O4) and some gangue, the leaching rate of the lower-priced sulfuric acid leaching system is low. In addition, due to the complex impurity composition and high content in the copper slag, the content of impurity ions such as Cu, Zn, Mn, Mg, As, and Cr in the leachate is very high. 2+Taking 120g / L as an example, the main impurity elements are Cu: 650mg / L, Zn: 6500mg / L, Mn: 250mg / L, Mg: 1500mg / L, As: 300mg / L, Cr: 300mg / L. The traditional hydrometallurgical impurity removal and purification method is difficult to remove impurities, with a long process and high cost. From a cost perspective, the resource utilization of low-value copper smelting tailings is of little significance to enterprises, which is the main reason for the accumulation of copper smelting tailings resources and the lack of large-scale resource utilization. Summary of the invention

[0005] The purpose of the present invention is to provide a method for preparing battery-grade ferrous sulfate by a conversion method using copper smelting tailings as raw materials in view of the above problems, thereby solving the problem that the impurity components in the copper smelting tailings are complex and high in content, and the impurity element ions used in preparing ferrous sulfate solution are difficult to remove.

[0006] In order to achieve the above object, the technical solution adopted by the present invention is as follows: a method for preparing battery-grade ferrous sulfate by a conversion method using copper smelting tailings as raw materials, comprising the following steps:

[0007] S1. Leaching: copper smelting tailings and concentrated sulfuric acid are mixed in a weight ratio of 0.5 to 0.8:1, water is added to make a slurry, and the reaction is carried out at a temperature of 95 to 160°C for 6 to 8 hours, and hot-pressed and filtered to obtain a leachate;

[0008] S2. Reduction: Add a reducing agent to the leaching solution at a temperature of 50-80°C and react for 2-4 hours to reduce the trivalent iron to divalent iron, so that Fe 3+ The concentration is reduced to 0.2-3 g / L;

[0009] S3, neutralization and weight removal: hydrogen sulfide and alkali are added to the solution in step S2 in an amount such that the Fe 2+ The solution is adjusted to a pH value of 4.0 to 6.5, and reacted for 2 to 4 hours at a temperature of 50 to 80°C, and then filtered under hot pressure to remove the residue to obtain a filtrate;

[0010] S4, iron precipitation: continue to meter hydrogen sulfide and alkali into the filtrate of step 3, the amount of hydrogen sulfide and alkali introduced is 0.95-1.05 times the theoretical amount required for precipitation of FeS, keep the solution pH 3.5-7.0, react at 60°C for 2-4h, hot-press filter, wash, and obtain FeS precipitate;

[0011] S5. Redissolution and crystallization: Add acid to dissolve the FeS precipitate to make a pure ferrous sulfate nearly saturated solution. After freezing crystallization and centrifugal separation, battery-grade ferrous sulfate product is obtained.

[0012] Preferably, in step S1, Fe2+ The ion content is 100-160g / L.

[0013] Preferably, in step S1, the weight ratio of the copper smelting tailings to water is 1:4 to 1:2.

[0014] Preferably, in step S2, the reducing agent is one of metallic iron or H2S.

[0015] Preferably, in step S2, the amount of the reducing agent added is to replace Fe 3+ 1.1 to 1.5 times the theoretical amount of ions.

[0016] Preferably, in step S3 or step S4, the base is one or more of NH3, Na2O, NaOH, K2O, KOH solid or its aqueous solution and hydrazine hydrate.

[0017] Preferably, in step S4, the mother liquor generated by filtration in the iron precipitation process is combined with the washing liquid generated by washing, and after impurities are removed, the mother liquor is evaporated, concentrated and crystallized by MVR to produce a by-product sulfate product.

[0018] Preferably, in step S5, the acid is sulfuric acid, and the concentration of the sulfuric acid is 150-350 g / L.

[0019] Preferably, in step S5, the H2S gas generated during the re-dissolution process is enriched and recovered, and then returned to the iron precipitation process for continued recycling.

[0020] Due to the adoption of the above technical solution, the present invention has the following beneficial effects:

[0021] 1. Add concentrated sulfuric acid to the copper smelting tailings, and destroy the phase structure of iron olivine and glass in the copper smelting tailings through high temperature and high acid leaching conditions, and leach the Fe element. The leaching rate is high, and the total iron leaching rate can reach more than 85%;

[0022] 2. Use H2S and alkali to neutralize and remove heavy metals and other impurity ions. No additional heavy-removal additives are required to adjust the solution pH and remove the weight, thus avoiding the introduction of other impurities and increasing costs.

[0023] 3. By precipitating FeS and then washing with deionized water, the element ions such as Ca, Zn, Mn, Mg, which are difficult to remove and have high content and are not easy to precipitate in the hydrometallurgical industry, are removed from the ferrous sulfate solution, simplifying the impurity removal process;

[0024] 4. After the FeS precipitate is washed, the concentration of the pure ferrous sulfate solution prepared by adding sulfuric acid to dissolve is close to saturation, and no pre-concentration is required, which increases the yield of the primary frozen crystallization and further reduces the production cost;

[0025] 5. The H2S generated after re-dissolution is recovered through enrichment and returned to the iron precipitation process for continued recycling. The alkali is converted into sulfate by-product for sale, which can offset the cost of iron precipitation raw materials and reduce the production cost.

[0026] 6. The main Zn, Mg and Si elements in the copper smelting tailings can be well utilized, reducing the production cost;

[0027] Compared with other similar production processes on the market, the process of the present invention is concise, simple to operate, has low requirements on equipment, short process flow, high production efficiency, and has high production application value. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 It is a production process flow chart of the present invention; DETAILED DESCRIPTION

[0029] The specific implementation modes of the present invention are further described below in conjunction with examples.

[0030] Example 1

[0031] A method for preparing battery-grade ferrous sulfate by a conversion method using copper smelting tailings as raw materials comprises the following steps:

[0032] S1. Leaching: Copper smelting tailings and concentrated sulfuric acid are prepared in a weight ratio of 0.5:1, water is added to make a slurry, and the reaction is carried out at a temperature of 130°C for 6 hours, and hot-pressed filtration is performed to obtain a leachate; wherein the weight ratio of copper smelting tailings to water is 1:4; Fe 2+ The ion content is 130g / L;

[0033] S2. Reduction: Add reducing agent H2S to the leaching solution at 60°C for 2h. The amount of reducing agent H2S added is to replace Fe 3+ ion theoretical dosage, reducing trivalent iron to divalent iron, making Fe in the leaching solution 3+ The concentration was reduced to 0.2 g / L;

[0034] S3, neutralization and weight removal: hydrogen sulfide and ammonia (NH3) are added to the solution in step S2 in an amount such that the Fe 2+ The solution pH was adjusted to 6.0, and the reaction was carried out at 60°C for 2 hours. The residue was removed by hot-pressing and filtering to remove Fe 3+ 、Al 3+ and heavy metal and other impurity element ions to obtain a filtrate;

[0035] S4, iron precipitation: hydrogen sulfide and ammonia (NH3) are continuously metered into the filtrate after impurity removal, and the amount of hydrogen sulfide and ammonia (NH3) introduced is 1.05 times the theoretical amount required for precipitation of FeS, the solution pH is maintained at 6.0, the temperature is 60°C, the reaction is carried out for 2 hours, hot-pressed filtration, and deionized water washing is performed to obtain FeS precipitate; the mother liquor produced by filtration in the iron precipitation process is combined with the washing liquid produced by washing, and after impurities are removed, the by-product sulfate product is obtained by MVR evaporation, concentration and crystallization;

[0036] S5, re-dissolution crystallization: FeS precipitate is re-dissolved with sulfuric acid, and the concentration of sulfuric acid added is 300g / L to make a pure ferrous sulfate nearly saturated solution. After freezing crystallization and centrifugal separation, battery-grade ferrous sulfate products are obtained. The H2S gas generated during the re-dissolution process is enriched and recovered, and returned to the iron precipitation process for continued recycling. The product crystallization indicators are as follows:

[0037] Table 1 Product crystallization index

[0038]

[0039] Example 2

[0040] A method for preparing battery-grade ferrous sulfate by a conversion method using copper smelting tailings as raw materials comprises the following steps:

[0041] S1. Leaching: Copper smelting tailings and concentrated sulfuric acid are prepared in a weight ratio of 0.6:1, water is added to make pulp, and the reaction is carried out at 130°C for 6 hours, and hot-pressed filtration is performed to obtain a leachate; wherein the weight ratio of copper smelting tailings to water is 1:4; Fe 2+ The ion content is 140g / L;

[0042] S2. Reduction: Add reducing agent H2S to the leaching solution at 60°C for 2h. The amount of reducing agent H2S added is to replace Fe 3+ ion theoretical dosage, reducing trivalent iron to divalent iron, making Fe in the leaching solution 3+ The concentration was reduced to 0.5 g / L;

[0043] S3, neutralization and weight removal: hydrogen sulfide and NaOH are added to the solution in step S2 in an amount sufficient to precipitate out Fe 2+ The solution pH was adjusted to 6.0, and the reaction was carried out at 60°C for 2 hours. The residue was removed by hot-pressing and filtering to remove Fe 3+ 、Al 3+ and heavy metal and other impurity element ions to obtain a filtrate;

[0044] S4, iron precipitation: hydrogen sulfide and NaOH are continuously metered into the filtrate after impurity removal, and the amount of hydrogen sulfide and NaOH introduced is 1.05 times the theoretical amount required for precipitation of FeS, the solution pH is maintained at 6.0, the temperature is 60°C, the reaction is carried out for 2 hours, hot-pressed filtration is performed, and deionized water is washed to obtain FeS precipitate; the mother liquor produced by filtration in the iron precipitation process is combined with the washing liquid produced by washing, and after impurities are removed, the by-product sulfate product is obtained by MVR evaporation, concentration and crystallization;

[0045] S5, re-dissolution crystallization: FeS precipitate is re-dissolved with sulfuric acid, and the concentration of sulfuric acid added is 300g / L to make a pure ferrous sulfate nearly saturated solution. After freezing crystallization and centrifugal separation, battery-grade ferrous sulfate products are obtained. The H2S gas generated during the re-dissolution process is enriched and recovered, and returned to the iron precipitation process for continued recycling. The product crystallization indicators are as follows:

[0046] Table 2 Product crystallization index

[0047]

[0048] Example 3

[0049] A method for preparing battery-grade ferrous sulfate by a conversion method using copper smelting tailings as raw materials comprises the following steps:

[0050] S1. Leaching: Copper smelting tailings and concentrated sulfuric acid are prepared in a weight ratio of 0.8:1, water is added to make a slurry, and the reaction is carried out at a temperature of 130°C for 6 hours, and hot-pressed filtration is performed to obtain a leachate; wherein the weight ratio of copper smelting tailings to water is 1:4; Fe 2+ The ion content is 150g / L;

[0051] S2. Reduction: Add reducing agent H2S to the leaching solution at 60°C for 2h. The amount of reducing agent H2S added is to replace Fe 3+ ion theoretical dosage, reducing trivalent iron to divalent iron, making Fe in the leaching solution 3+ The concentration was reduced to 0.8 g / L;

[0052] S3, neutralization and weight removal: hydrogen sulfide and KOH are added to the solution in step S2 in an amount sufficient to precipitate out the Fe 2+ The solution pH was adjusted to 6.0, and the reaction was carried out at 60°C for 2 hours. The residue was removed by hot-pressing and filtering to remove Fe 3+ 、Al 3+ and heavy metal and other impurity element ions to obtain a filtrate;

[0053] S4, iron precipitation: hydrogen sulfide and KOH are continuously metered into the filtrate after impurity removal, and the amount of hydrogen sulfide and KOH introduced is 1.05 times the theoretical amount required for precipitation of FeS, the solution pH is maintained at 6.0, the temperature is 60°C, the reaction is carried out for 2 hours, hot-pressed filtration is carried out, and deionized water is washed to obtain FeS precipitate; the mother liquor produced by filtration in the iron precipitation process is combined with the washing liquid produced by washing, and after impurities are removed, the by-product sulfate product is obtained by MVR evaporation, concentration and crystallization;

[0054] S5, re-dissolution crystallization: FeS precipitate is re-dissolved with sulfuric acid, and the concentration of sulfuric acid added is 300g / L to make a pure ferrous sulfate nearly saturated solution. After freezing crystallization and centrifugal separation, battery-grade ferrous sulfate products are obtained. The H2S gas generated during the re-dissolution process is enriched and recovered, and returned to the iron precipitation process for continued recycling. The product crystallization indicators are as follows:

[0055] Table 3 Product crystallization index

[0056]

[0057] The above description is a detailed description of the preferred embodiments of the present invention, but the embodiments are not intended to limit the scope of the patent application of the present invention. All equivalent changes or modified modifications accomplished under the guidance of the present invention should belong to the patents covered by the present invention.

Claims

1. A method for preparing battery-grade ferrous sulfate by a conversion method using copper smelting tailings as raw materials, characterized in that: The following steps are involved: S1. Leaching: copper smelting tailings and concentrated sulfuric acid are mixed in a weight ratio of 0.5 to 0.8:1, water is added to make a slurry, and the reaction is carried out at a temperature of 95 to 160°C for 6 to 8 hours, and hot-pressed and filtered to obtain a leachate; S2. Reduction: Add a reducing agent to the leaching solution at a temperature of 50-80°C and react for 2-4 hours to reduce the trivalent iron to divalent iron, so that Fe 3+ The concentration is reduced to 0.2-3 g / L; S3, neutralization and weight removal: hydrogen sulfide and alkali are added to the solution in step S2 in an amount such that the Fe 2+ The solution is adjusted to a pH value of 4.0 to 6.5, and reacted for 2 to 4 hours at a temperature of 50 to 80°C, and then filtered under hot pressure to remove the residue to obtain a filtrate; S4, iron precipitation: continue to meter hydrogen sulfide and alkali into the filtrate of step 3, the amount of hydrogen sulfide and alkali introduced is 0.95-1.05 times the theoretical amount required for precipitation of FeS, keep the solution pH 3.5-7.0, react at 60°C for 2-4h, hot-press filter, wash, and obtain FeS precipitate; S5. Redissolution and crystallization: Add acid to dissolve the FeS precipitate to make a pure ferrous sulfate nearly saturated solution. After freezing crystallization and centrifugal separation, battery-grade ferrous sulfate product is obtained.

2. The method for preparing battery-grade ferrous sulfate by a conversion method using copper smelting tailings as raw materials according to claim 1, characterized in that: In step S1, Fe 2+ The ion content is 100-160g / L.

3. The method for preparing battery-grade ferrous sulfate by a conversion method using copper smelting tailings as raw materials according to claim 1, characterized in that: In step S1, the weight ratio of the copper smelting tailings to water is 1:4 to 1:

2.

4. The method for preparing battery-grade ferrous sulfate by a conversion method using copper smelting tailings as raw materials according to claim 1, characterized in that: In step S2, the reducing agent is one of metallic iron or H2S.

5. The method for preparing battery-grade ferrous sulfate by a conversion method using copper smelting tailings as raw materials according to claim 1, characterized in that: In step S2, the amount of the reducing agent added is to replace Fe 3+ 1.1 to 1.5 times the theoretical dosage of ions.

6. The method for preparing battery-grade ferrous sulfate by a conversion method using copper smelting tailings as raw materials according to claim 1, characterized in that: In step S3 or step S4, the base is one or more of NH3, Na2O, NaOH, K2O, KOH solid or its aqueous solution and hydrazine hydrate.

7. The method for preparing battery-grade ferrous sulfate by a conversion method using copper smelting tailings as raw materials according to claim 1, characterized in that: In step S4, the mother liquor generated by filtration in the iron precipitation process is combined with the washing liquid generated by washing, and after impurities are removed, the mother liquor is evaporated, concentrated and crystallized by MVR to produce a by-product sulfate product.

8. The method for preparing battery-grade ferrous sulfate by conversion method using copper smelting tailings as raw materials according to claim 1, characterized in that: In step S5, the acid is sulfuric acid with a concentration of 150 to 350 g / L.

9. The method for preparing battery-grade ferrous sulfate by conversion method using copper smelting tailings as raw materials according to claim 1, characterized in that: In step S5, the H2S gas generated during the re-dissolution process is enriched and recovered, and then returned to the iron precipitation process for further recycling.

Citation Information

Cited By

  • Method for preparing ferrous sulfate for batteries from spent sulfuric acid of stainless steel pickling and application thereof