Transparent front plate, preparation method thereof and photovoltaic module
By introducing methylvinyl silicone rubber and glass fiber into PMMA and using transparent phosphorus-based flame retardant to prepare a halogen-free flame retardant transparent front plate, the environmental and human hazards of halogen flame retardants in the prior art were solved. , achieves high transparency, halogen-free flame retardant effect, and is suitable for photovoltaic building integration field.
Patent Information
- Application Number
- CN202411147411.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-08-20
AI Technical Summary
Existing flame retardant PMMAs produce halogenated hydrocarbon gas during combustion, which can cause harm to the environment and the human body. Halogen-free flame retardant affects optical transparency, making it difficult to develop high-transparent halogen-free flame retardant PMMAs.
Methyl vinyl silicone rubber and glass fiber were introduced into PMMA, and transparent phosphorus-based flame retardant was used to process it through a mixer and an extrusion caster, and then irradiated cross-linking was performed in an electronic accelerator to prepare halogen-free Flame-retardant transparent front panel.
It achieves halogen-free flame retardant effect, reduces smoke and toxic emissions, maintains optical transparency, and is suitable for the field of photovoltaic building integration.
Smart Images

Figure CN119039730A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of photovoltaic modules, and in particular relates to a transparent front plate and a preparation method thereof, and a photovoltaic module. Background Art
[0002] Polymethyl methacrylate (PMMA) is widely used due to its good optical and mechanical properties, and is often used as a substitute for glass. However, PMMA is flammable, and its application in the field of photovoltaic building integration requires flame retardant modification. Currently, most commercial flame-retardant PMMAs are halogen flame-retardant systems, which produce halogenated hydrocarbon gases during combustion, causing harm to the environment and human body. Therefore, the development of halogen-free flame-retardant PMMA is urgent. However, there are very few halogen-free flame retardants suitable for PMMA, and the addition of most halogen-free flame retardants will inevitably affect the optical transparency of PMMA. Therefore, it is imperative to develop highly transparent halogen-free flame-retardant PMMA.
[0003] Ceramic silicone rubber is a new type of fireproof material. During the combustion process, it forms a dense and hard ceramic shell, which can prevent the flame from spreading further and achieve flame retardant and fireproof effects. It is widely used in the field of wires and cables, but its application in the field of photovoltaic backplanes is still in its infancy. Summary of the invention
[0004] Purpose of the invention: In view of the problems and shortcomings in the prior art, the present invention provides a method for preparing a transparent front plate.
[0005] Methyl vinyl silicone rubber has become a commonly used matrix for ceramic silicone rubber due to its excellent physical and chemical properties, good processability and low cost. Moreover, methyl vinyl silicone rubber is a transparent silicone rubber, and its introduction into the PMMA matrix will not damage the optical properties. The addition of glass fiber will promote the formation of its ceramic hard shell. It can achieve a good flame retardant effect in combination with transparent phosphorus flame retardants. Therefore, it is imperative to add an appropriate amount of methyl vinyl silicone rubber to the glass fiber reinforced PMMA system and select a suitable transparent phosphorus flame retardant to prepare a halogen-free flame retardant transparent front plate.
[0006] The method of the present application comprises the following steps:
[0007] S1, placing the dried PMMA, methyl vinyl silicone rubber, modified glass fiber, halogen-free flame retardant, cross-linking accelerator, antioxidant and anti-ultraviolet additive in an internal mixer, mixing them evenly, and then extruding and granulating them by single screw extruder to obtain PMMA halogen-free flame retardant special material;
[0008] S2, placing the PMMA halogen-free flame-retardant special material obtained in S1 in an extrusion casting machine for casting to obtain a halogen-free flame-retardant photovoltaic substrate;
[0009] S3. The halogen-free flame-retardant photovoltaic substrate obtained in S2 is placed under an electron accelerator for irradiation cross-linking to obtain a halogen-free flame-retardant transparent front plate.
[0010] Furthermore, the mass ratio of PMMA:methyl vinyl silicone rubber:modified glass fiber in S1 is in the following range: 30-40:1-5:10-20.
[0011] Furthermore, the halogen-free flame retardant in S1 includes any one or more of the following combinations: 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, resorcinol bis(diphenyl phosphate), hexaphenoxy cyclophosphazene, resorcinol bis[di(2,6-dimethylphenyl) phosphate], and the addition ratio is 15 to 20 wt% of PMMA.
[0012] Furthermore, it is characterized in that the cross-linking accelerator comprises any one or more combinations of the following: trimethylolpropane trimethacrylate, trimethylolpropane triacrylate, pentaerythritol triacrylate, and the addition ratio of the cross-linking accelerator is 0.2wt% to 10wt% of PMMA.
[0013] Further, the antioxidant includes any one or more of the following combinations: the antioxidant includes any one of the following: one or more of tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] pentaerythritol ester, tris(2,4-di-tert-butylphenyl) phosphite, dilauryl thiodipropionate, N,N'-bis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl]hydrazine, and β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, and the added ratio is 0.1wt% to 3wt% of PMMA.
[0014] Furthermore, the anti-ultraviolet auxiliary agent includes any one or more of the following in any combination: bisphenol A disalicylate, cyanuric chloride polymer, p-tert-octylphenyl salicylate, bis-2,2,6,6-tetramethylpiperidinol sebacate, 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, 2-hydroxy-4-octyloxybenzophenone, 2-hydroxy-4-methoxybenzophenone, one or more thereof, and the addition ratio is 0.1wt% to 2wt% of PMMA.
[0015] Furthermore, the temperature of the internal mixer in S1 is 185-195°C, the internal mixing time is 20-25 min, and the temperature of the single screw extrusion granulation is 190-210°C;
[0016] The temperature of the extrusion casting machine in S3 is 231-250°C.
[0017] Furthermore, the modified glass fiber in S2 is a glass fiber treated with a silane coupling agent, and the silane coupling agent includes any one or a mixture of the following: γ-aminopropyltriethoxysilane, γ-(2,3-epoxypropoxy)propyltrimethoxysilane, and γ-methacryloxypropyl.
[0018] Furthermore, the dose of the electron beam irradiation in S4 is 100-150 kGy, and the irradiation atmosphere includes: nitrogen, vacuum, and air atmosphere.
[0019] On the other hand, the present invention provides a transparent front plate. Furthermore, the transparent front plate is prepared by using the above preparation method.
[0020] On the other hand, the present invention provides a photovoltaic module, characterized in that it includes a halogen-free flame-retardant transparent front panel prepared by the preparation method described in any one of claims 1 to 7, a first POE layer, a solar cell, a second POE layer, and a halogen-free flame-retardant photovoltaic back panel.
[0021] Beneficial effects:
[0022] The present invention introduces ceramic silicone rubber methyl vinyl silicone rubber into the PMMA matrix, which can form a hard ceramic-like hard shell during high-temperature burning to prevent the flame from spreading further. The introduction of glass fiber can promote the formation of the ceramic hard shell of methyl vinyl silicone rubber, and can achieve a good flame retardant effect when combined with a colorless and transparent phosphorus-based flame retardant. Compared with traditional technologies, the present invention does not use halogen flame retardants, and the smoke and toxicity generated during the combustion process are very small, which can reduce pollution to the environment and harm to the human body; in addition, the preparation process of the present invention is simple, the cost is low, and it can be mass-produced, and it can be widely used in the field of photovoltaic building integration. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 A schematic diagram of a method for preparing a transparent photovoltaic front panel in an embodiment of the present invention. DETAILED DESCRIPTION
[0024] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with embodiments.
[0025] like Figure 1 As shown, the method of this embodiment includes the following steps:
[0026] S1, placing the dried PMMA, methyl vinyl silicone rubber, modified glass fiber, halogen-free flame retardant, cross-linking accelerator, antioxidant and anti-ultraviolet additive in an internal mixer, mixing them evenly, and then extruding and granulating them by single screw extruder to obtain PMMA halogen-free flame retardant special material;
[0027] S2, placing the PMMA halogen-free flame-retardant special material obtained in S1 in an extrusion casting machine for casting to obtain a halogen-free flame-retardant photovoltaic substrate;
[0028] S3. The halogen-free flame-retardant photovoltaic substrate obtained in S2 is placed under an electron accelerator for irradiation cross-linking to obtain a halogen-free flame-retardant transparent front plate.
[0029] Furthermore, the mass ratio of PMMA:methyl vinyl silicone rubber:modified glass fiber in S1 is in the following range: 30-40:1-5:10-20.
[0030] Preferably, 30 to 40 parts of polymethyl methacrylate (PMMA), 10 to 20 parts of glass fiber, 15 to 20 parts of halogen-free flame retardant, 1 to 5 parts of methyl vinyl silicone rubber, 5 to 10 parts of crosslinking accelerator, and 1 to 5 parts of antioxidant and anti-ultraviolet additives.
[0031] Furthermore, the halogen-free flame retardant in S1 includes any one or more of the following combinations: 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, resorcinol bis(diphenyl phosphate), hexaphenoxy cyclophosphazene, resorcinol bis[di(2,6-dimethylphenyl) phosphate], and the addition ratio is 15 to 20 wt% of PMMA.
[0032] Further, the cross-linking accelerator includes any one or more of the following combinations: trimethylolpropane trimethacrylate, trimethylolpropane triacrylate, pentaerythritol triacrylate, and the cross-linking accelerator is added in an amount of 0.2wt% to 10wt% of PMMA;
[0033] Further, the antioxidant includes any one or more of the following combinations: the antioxidant includes any one of the following: one or more of tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] pentaerythritol ester, tris(2,4-di-tert-butylphenyl) phosphite, dilauryl thiodipropionate, N,N'-bis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl]hydrazine, and β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, and the added ratio is 0.1wt% to 3wt% of PMMA.
[0034] Furthermore, the anti-ultraviolet auxiliary agent includes any one or more of the following combinations: bisphenol A disalicylate, cyanuric chloride polymer, p-tert-octylphenyl salicylate, bis-2,2,6,6-tetramethylpiperidinol sebacate, 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, 2-hydroxy-4-octyloxybenzophenone, 2-hydroxy-4-methoxybenzophenone, one or more thereof, and the addition ratio is 0.1wt% to 2wt% of PMMA.
[0035] Furthermore, the temperature of the internal mixer in S1 is 185-195°C, the internal mixing time is 20-25 min, and the temperature of the single screw extrusion granulation is 190-210°C;
[0036] The temperature of the extrusion casting machine in S3 is 231-250°C.
[0037] Furthermore, the modified glass fiber in S2 is a glass fiber treated with a silane coupling agent, and the silane coupling agent includes any one or a mixture of the following: γ-aminopropyltriethoxysilane, γ-(2,3-epoxypropoxy)propyltrimethoxysilane, and γ-methacryloxypropyl.
[0038] Furthermore, the dose of the electron beam irradiation in S4 is 100-150 kGy, and the irradiation atmosphere includes: nitrogen, vacuum, and air atmosphere.
[0039] On the other hand, the present invention provides a transparent front plate. Furthermore, the transparent front plate is prepared by using the above preparation method.
[0040] On the other hand, the present invention provides a photovoltaic module, characterized in that it includes a halogen-free flame-retardant transparent front panel prepared by the preparation method described in any one of claims 1 to 7, a first POE layer, a solar cell, a second POE layer, and a halogen-free flame-retardant photovoltaic back panel.
[0041] It should be noted that the manufacturing method of the halogen-free flame-retardant photovoltaic backsheet can be the same as that of the front sheet.
[0042] Beneficial effects:
[0043] The present invention introduces ceramic silicone rubber methyl vinyl silicone rubber into the PMMA matrix, which can form a hard ceramic-like hard shell during high-temperature burning to prevent the flame from spreading further. The introduction of glass fiber can promote the formation of the ceramic hard shell of methyl vinyl silicone rubber, and can achieve a good flame retardant effect when combined with a colorless and transparent phosphorus-based flame retardant. Compared with traditional technologies, the present invention does not use halogen flame retardants, and the smoke and toxicity generated during the combustion process are very small, which can reduce pollution to the environment and harm to the human body; in addition, the preparation process of the present invention is simple, the cost is low, and it can be mass-produced, and it can be widely used in the field of photovoltaic building integration.
[0044] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with embodiments.
[0045] Embodiment 1:
[0046] A transparent front plate is prepared by the following steps:
[0047] (1) Dry polymethyl methacrylate resin (PMMA), methyl vinyl silicone rubber, glass fiber modified by γ-(2,3-epoxypropyloxy)propyltrimethoxysilane coupling agent, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO), trimethylolpropane trimethacrylate, pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], 2-hydroxy-4-octyloxybenzophenone and (2,2,6,6-tetramethylpiperidinyl) are placed in an internal mixer and mixed evenly, and then single-screw extrusion granulation is performed to obtain PMMA halogen-free flame retardant special material; wherein polymethyl methacrylate: methyl vinyl silicone rubber: modified glass fiber are of high quality. The weight ratio is 40:5:20, trimethylolpropane trimethacrylate is 10wt% of PMMA resin; the addition ratio of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO) is 20wt% of PMMA resin; pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, 2-hydroxy-4-methoxybenzophenone and bis-2,2,6,6-tetramethylpiperidinol sebacate are 0.2wt%, 0.2wt% and 0.3wt% of polymethyl methacrylate (PMMA) respectively, the mixing temperature is 190°C, the mixing time is 25min, and the temperature of single-screw extrusion granulation is 190-210°C.
[0048] (2) placing the PMMA halogen-free flame-retardant special material obtained in step (1) in an extrusion casting machine for casting to obtain a halogen-free flame-retardant photovoltaic substrate, wherein the temperature of the casting extruder is 231 to 250° C.;
[0049] (3) The halogen-free flame-retardant photovoltaic substrate obtained in step (3) is placed under an electron accelerator for irradiation, the irradiation dose is 150 kGy, and the irradiation atmosphere is nitrogen.
[0050] Embodiment 2:
[0051] A transparent front plate is prepared by the following steps:
[0052] (1) Drying polymethyl methacrylate resin (PMMA), methyl vinyl silicone rubber, glass fiber modified by γ-aminopropyl triethoxysilane coupling agent, resorcinol bis(diphenyl phosphate) (RDP), trimethylolpropane triacrylate, pentaerythritol tetra[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate], 2-hydroxy-4-octyloxybenzophenone and (2,2,6,6-tetramethylpiperidinyl) are placed in an internal mixer and mixed evenly, and then single-screw extrusion granulation is performed to obtain PMMA halogen-free flame retardant special material; wherein polymethyl methacrylate: methyl vinyl silicone rubber: modified glass fiber The mass ratio of trimethylolpropane triacrylate is 35:5:15, trimethylolpropane triacrylate is 5wt% of PMMA resin; the addition ratio of resorcinol bis(diphenyl phosphate) (RDP) is 20wt% of PMMA resin; tri(2,4-di-tert-butylphenyl) phosphite, 2-hydroxy-4-octyloxybenzophenone and bis-2,2,6,6-tetramethylpiperidinol sebacate are 0.1wt%, 0.1wt% and 0.3wt% of polymethyl methacrylate (PMMA) respectively, the mixing temperature is 185°C, the mixing time is 30min, and the temperature of single-screw extrusion granulation is 190-210°C.
[0053] (2) placing the PMMA halogen-free flame-retardant special material obtained in step (1) in an extrusion casting machine for casting to obtain a halogen-free flame-retardant photovoltaic substrate, wherein the temperature of the casting extruder is 231 to 250° C.;
[0054] (3) The halogen-free flame-retardant photovoltaic substrate obtained in step (3) is placed under an electron accelerator for irradiation, the irradiation dose is 100 kGy, and the irradiation atmosphere is air.
[0055] Embodiment 3:
[0056] A transparent front plate is prepared by the following steps:
[0057] (1) Dry polymethyl methacrylate resin (PMMA), methyl vinyl silicone rubber, glass fiber modified by γ-(2,3-epoxypropoxy)propyltrimethoxysilane coupling agent, hexaphenoxy cyclophosphazene (HPCTP), trimethylolpropane trimethacrylate, β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionic acid n-octadecyl ester, 2-hydroxy-4-octyloxybenzophenone and (2,2,6,6-tetramethylpiperidinyl) are placed in an internal mixer and mixed evenly, and then single-screw extrusion granulation is performed to obtain PMMA halogen-free flame retardant special material; wherein polymethyl methacrylate: methyl vinyl silicone rubber: modified The mass ratio of the polymethyl methacrylate is 40:5:20, the trimethylolpropane trimethacrylate is 8wt% of the PMMA resin; the addition ratio of hexaphenoxy cyclophosphazene (HPCTP) is 20wt% of the PMMA resin; the β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, 2-hydroxy-4-octyloxybenzophenone and bisphenol A disalicylate are 1.5wt%, 1.5wt% and 2wt% of the polymethyl methacrylate (PMMA) respectively, the mixing temperature is 190°C, the mixing time is 25min, and the temperature of the single-screw extrusion granulation is 190-210°C.
[0058] (2) placing the PMMA halogen-free flame-retardant special material obtained in step (1) in an extrusion casting machine for casting to obtain a halogen-free flame-retardant photovoltaic substrate, wherein the temperature of the casting extruder is 231 to 250° C.;
[0059] (3) The halogen-free flame-retardant photovoltaic substrate obtained in step (3) is placed under an electron accelerator for irradiation, the irradiation dose is 150 kGy, and the irradiation atmosphere is nitrogen.
[0060] Embodiment 4:
[0061] A transparent front plate is prepared by the following steps:
[0062] (1) Drying polymethyl methacrylate resin (PMMA), methyl vinyl silicone rubber, glass fiber modified by γ-methacryloxypropyl silane coupling agent, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO), trimethylolpropane trimethacrylate, pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, 2-hydroxy-4-octyloxybenzophenone and 2-(2'-hydroxy-5'-methylphenyl)benzotriazole sebacate are placed in an internal mixer and mixed evenly, and then single-screw extrusion granulation is performed to obtain PMMA halogen-free flame retardant special material; wherein polymethyl methacrylate: methyl vinyl silicone rubber: modified glass fiber The mass ratio is 40:5:20, trimethylolpropane trimethacrylate is 10wt% of PMMA resin; the addition ratio of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO) is 20wt% of PMMA resin; pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, 2-hydroxy-4-octyloxybenzophenone and 2-(2'-hydroxy-5'-methylphenyl)benzotriazole sebacate are 2wt%, 2wt% and 3wt% of polymethyl methacrylate (PMMA), respectively, the mixing temperature is 190°C, the mixing time is 20min, and the temperature of single-screw extrusion granulation is 190-210°C.
[0063] (2) placing the PMMA halogen-free flame-retardant special material obtained in step (1) in an extrusion casting machine for casting to obtain a halogen-free flame-retardant photovoltaic substrate, wherein the temperature of the casting extruder is 231 to 250° C.;
[0064] (3) The halogen-free flame-retardant photovoltaic substrate obtained in step (3) is placed under an electron accelerator for irradiation, the irradiation dose is 125 kGy, and the irradiation atmosphere is nitrogen.
[0065] Embodiment 5:
[0066] A transparent front plate is prepared by the following steps:
[0067] (1) Dry polymethyl methacrylate resin (PMMA), methyl vinyl silicone rubber, glass fiber modified by γ-(2,3-epoxypropyloxy)propyltrimethoxysilane coupling agent, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO) and hexaphenoxy cyclophosphazene (HPCTP), trimethylolpropane trimethacrylate, pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], 2-hydroxy-4-octyloxybenzophenone and p-tert-octylphenyl salicylate are placed in an internal mixer and mixed evenly, and then single-screw extrusion granulation is performed to obtain PMMA halogen-free flame retardant special material; wherein polymethyl methacrylate: methyl vinyl silicone rubber: modified glass fiber The mass ratio is 40:5:20, trimethylolpropane trimethacrylate is 10wt% of PMMA resin; the addition ratios of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO) and hexaphenoxy cyclophosphazene (HPCTP) are 10wt% and 10wt% of PMMA resin respectively; pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, 2-hydroxy-4-octyloxybenzophenone and p-tert-octylphenyl salicylate are 2wt%, 2wt% and 3wt% of polymethyl methacrylate (PMMA) respectively, the banburying temperature is 195°C, the banburying time is 25min, and the temperature of single-screw extrusion granulation is 190-210°C.
[0068] (2) placing the PMMA halogen-free flame-retardant special material obtained in step (1) in an extrusion casting machine for casting to obtain a halogen-free flame-retardant photovoltaic substrate, wherein the temperature of the casting extruder is 231 to 250° C.;
[0069] (3) The halogen-free flame-retardant photovoltaic substrate obtained in step (3) is placed under an electron accelerator for irradiation, the irradiation dose is 150 kGy, and the irradiation atmosphere is nitrogen.
[0070] Embodiment 6:
[0071] A transparent front plate is prepared by the following steps:
[0072] (1) Dry polymethyl methacrylate resin (PMMA), methyl vinyl silicone rubber, glass fiber modified by γ-(2,3-epoxypropoxy)propyltrimethoxysilane coupling agent, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO) and resorcinol bis(diphenyl phosphate) (RDP), trimethylolpropane trimethacrylate, pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, 2-hydroxy-4-octyloxybenzophenone and 2-(2'-hydroxy-5'-methylphenyl)benzotriazole are placed in an internal mixer and mixed evenly, and then single-screw extrusion granulation is performed to obtain PMMA halogen-free flame retardant special material; wherein polymethyl methacrylate: methyl vinyl silicone rubber: modified glass fiber The mass ratio is 40:5:20, trimethylolpropane trimethacrylate is 10wt% of PMMA resin; the addition ratios of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO) and resorcinol bis(diphenyl phosphate) (RDP) are 15wt% and 5wt% of PMMA resin respectively; pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, 2-hydroxy-4-octyloxybenzophenone and 2-(2'-hydroxy-5'-methylphenyl)benzotriazole are 2wt%, 2wt% and 3wt% of polymethyl methacrylate (PMMA) respectively, the banburying temperature is 190°C, the banburying time is 25min, and the temperature of single-screw extrusion granulation is 190-210°C.
[0073] (2) placing the PMMA halogen-free flame-retardant special material obtained in step (1) in an extrusion casting machine for casting to obtain a halogen-free flame-retardant photovoltaic substrate, wherein the temperature of the casting extruder is 231 to 250° C.;
[0074] (3) The halogen-free flame-retardant photovoltaic substrate obtained in step (3) is placed under an electron accelerator for irradiation, the irradiation dose is 150 kGy, and the irradiation atmosphere is air.
[0075] Comparative Example 1 is a conventional PVDF / PET / FFC front plate purchased on the market.
[0076] The test standards for the adhesion and vertical burning experiments with EVA for the embodiments and comparative examples are as follows:
[0077] Adhesion with EVA: The test method is peel strength test. Use a knife to cut a 1cm wide strip between the back panel and the EVA, and make sure to cut through it. Use a tensile testing machine to pull the peeling layer in a 180° direction at a speed of 100mm / min. Take points when the material is peeled off at a uniform speed and take the minimum value. The peel strength between the EVA and the back panel is determined to be 40N / cm to be qualified.
[0078] Vertical combustion test: Use a rectangular cutter to prepare a sample with a thickness of 125±5mm×13.0±0.5mm×0.5mm, and use a vertical combustion test machine to test according to the UL-94:2017 standard. Record the afterflame time t1 after leaving the flame for the first time, the afterflame time t2 after leaving the flame for the second time, and the afterflame time t3. Each group of samples includes at least 5 samples, and the samples are judged according to the UL-94 flame grade judgment standard. It should be noted that ±5mm means that the error is not greater than 5mm.
[0079] Front panel transmittance test: Tested in accordance with IEC-62805-2 test standard.
[0080] The results of the solar cell front panel and EVA adhesion test, light transmittance, and UL-94 vertical burning test are shown in Table 1:
[0081] Table 1
[0082]
[0083] It can be seen from Table 1 that the solar cell front panels prepared in the examples all pass the UL-94 standard, have good adhesion to the EVA film and have a light transmittance of ≥85%.
[0084] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a transparent front plate, characterized in that: The following steps are involved: S1, placing the dried PMMA, methyl vinyl silicone rubber, modified glass fiber, halogen-free flame retardant, cross-linking accelerator, antioxidant and anti-ultraviolet additive in an internal mixer, mixing them evenly, and then extruding and granulating them by single screw extruder to obtain PMMA halogen-free flame retardant special material; S2, placing the PMMA halogen-free flame-retardant special material obtained in S1 in an extrusion casting machine for casting to obtain a halogen-free flame-retardant photovoltaic substrate; S3. The halogen-free flame-retardant photovoltaic substrate obtained in S2 is placed under an electron accelerator for irradiation cross-linking to obtain a halogen-free flame-retardant transparent front plate.
2. The method for preparing a transparent front plate according to claim 1, characterized in that: The mass ratio of PMMA:methyl vinyl silicone rubber:modified glass fiber in S1 is in the following range: 30-40:1-5:10-20.
3. The method for preparing a transparent front plate according to claim 1, characterized in that: The halogen-free flame retardant in S1 includes any one or more of the following combinations: 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, resorcinol bis(diphenyl phosphate), hexaphenoxy cyclophosphazene, resorcinol bis[di(2,6-dimethylphenyl) phosphate], and the addition ratio of the halogen-free flame retardant is 15-20wt% of PMMA.
4. The method for preparing a transparent front plate according to claim 1, characterized in that: The cross-linking accelerator comprises any one or more of the following combinations: trimethylolpropane trimethacrylate, trimethylolpropane triacrylate, pentaerythritol triacrylate, and the cross-linking accelerator is added in an amount of 0.2wt% to 10wt% of PMMA; The antioxidant comprises any one or more of the following combinations: pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, tris(2,4-di-tert-butylphenyl) phosphite, dilauryl thiodipropionate, N,N'-bis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl]hydrazine, and n-octadecanol β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate. The antioxidant is added in an amount of 0.1wt% to 3wt% of PMMA.
5. The method for preparing a transparent front plate according to claim 1, characterized in that: The anti-ultraviolet auxiliary agent includes any one or more of the following in any combination: bisphenol A disalicylate, cyanuric chloride polymer, p-tert-octylphenyl salicylate, bis-2,2,6,6-tetramethylpiperidinol sebacate, 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, 2-hydroxy-4-octyloxybenzophenone, 2-hydroxy-4-methoxybenzophenone, and the addition ratio of the anti-ultraviolet auxiliary agent is 0.1wt% to 2wt% of PMMA.
6. The method for preparing a transparent front plate according to claim 1, characterized in that: The temperature of the internal mixer in S1 is 185-195°C, the internal mixing time is 20-25 min, the temperature of the single screw extrusion granulation is 190-210°C; the temperature of the extrusion casting machine in S3 is 231-250°C.
7. The method for preparing a halogen-free flame-retardant transparent front plate according to claim 1, characterized in that: The modified glass fiber in S2 is a glass fiber treated with a silane coupling agent, and the silane coupling agent includes any one or a mixture of the following: γ-aminopropyltriethoxysilane, γ-(2,3-epoxypropoxy)propyltrimethoxysilane, and γ-methacryloxypropyl.
8. The method for preparing a halogen-free flame-retardant transparent front plate according to claim 1, characterized in that: The dose of electron beam irradiation in S4 is 100-150 kGy, and the irradiation atmosphere includes: nitrogen, vacuum, and air atmosphere.
9. A transparent front plate, characterized in that: The transparent front plate is prepared by using the preparation method described in any one of claims 1 to 8.
10. A photovoltaic module, characterized in that: The photovoltaic module comprises, in order along the light incident direction, a transparent front plate prepared by the preparation method according to any one of claims 1 to 8, a first POE layer, a solar cell sheet, a second POE layer, and a halogen-free flame-retardant photovoltaic back plate.
Citation Information
Patent Citations
Transparent gasoline resistant PMMA alloy material and preparation method thereof
CN110358239A
PMMA / glass fiber composite material, preparation method and application thereof
CN112063088A
Thermoplastic composite material for photovoltaic front plate
CN116656108A
Methacrylic resin composition and molded body
WO2017200032A1
Methacrylic resin, methacrylic resin composition, and molded body
WO2019088025A1