PA66 modified material with good temperature resistance and preparation method thereof

By adding modified wollastonite powder and other raw materials to PA66 material, the problem of insufficient temperature resistance of PA66 material is solved, and the material's high temperature resistance and aging resistance are achieved, which is suitable for the processing and application of mechanical components such as gears.

CN119039779APending Publication Date: 2024-11-29ANHUI ZHONGHAN POLYMER TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411248787.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-06
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The insufficient temperature resistance of PA66 materials limits its development in the field of mechanical engineering, especially in harsh environments.

Method used

By adding modified wollastonite powder, wear-resistant agent and compatibility agent, a PA66 modified material was prepared. The modified wollastonite powder formed covalent bonds through esterification reaction, reducing surface energy, improving dispersion, and The hindered amine structure provides light stability and antioxidant effects, improving the material's temperature resistance and anti-aging properties.

Benefits of technology

The excellent temperature resistance and aging resistance of PA66 modified materials are achieved, with high mechanical strength, dimensional stability and chemical stability, while simplifying the preparation process and reducing water absorption and production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005031656650000021
    Figure BDA0005031656650000021
  • Figure BDA0005031656650000031
    Figure BDA0005031656650000031
  • Figure BDA0005031656650000091
    Figure BDA0005031656650000091
Patent Text Reader

Abstract

The invention discloses a PA66 modified material with good temperature resistance and a preparation method thereof, and belongs to the technical field of high polymer materials. The PA66 modified material with good temperature resistance comprises the following raw materials in percentage by weight: 70-84% of PA66 resin, 10-15% of modified wollastonite powder, 2-4% of a wear-resistant agent, 3-10% of a compatilizer, 0.1-1% of an antioxidant and 0.1-1% of a lubricant. The PA66 modified material prepared by taking PA66 as a matrix and adding the modified wollastonite powder containing the hindered amine structure, the wear-resistant agent, the compatilizer and other raw materials has excellent and stable temperature resistance and aging resistance, meanwhile, has relatively high dimensional stability and good chemical stability and mechanical strength, in addition, the preparation process is simple, the cost is low, and the PA66 modified material is suitable for industrial production. The water absorption rate and the production cost are reduced, and the composite material can be widely applied to the aspects of gears, bearings, sealing elements, automobile industry spare and accessory parts, medical instruments, mechanical parts and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of polymer materials, and in particular, relates to a PA66 modified material with good temperature resistance and a preparation method thereof. Background Art

[0002] Nylon 66 (PA66) is an important engineering plastic with excellent physical properties and chemical stability. It is widely used in gears, bearings, fan blades, automotive parts, electronics, aerospace, medical equipment, mechanical parts, etc. It is one of the most widely used engineering plastics in the world.

[0003] The market demand for PA66 continues to grow, due to its unique characteristics. It has excellent mechanical properties, wear resistance, self-lubrication, corrosion resistance, etc., can meet various mechanical requirements and can remain stable in harsh environments. However, with the advancement of technology and market demand, the temperature resistance of PA66 has hindered its development in the field of mechanical engineering. Therefore, it is urgent to improve the temperature resistance of PA66 materials. Summary of the invention

[0004] The purpose of the present invention is to overcome the defects of the prior art and provide a PA66 modified material with good temperature resistance and a preparation method thereof.

[0005] The purpose of the present invention can be achieved through the following technical solutions:

[0006] A PA66 modified material with good temperature resistance, comprising the following raw materials in weight percentage: 70-84% of PA66 resin, 10-15% of modified wollastonite powder, 2-4% of wear-resistant agent, 3-10% of compatibilizer, 0.1-1% of antioxidant, and 0.1-1% of lubricant;

[0007] Furthermore, the relative viscosity of the PA66 resin is 2.2-2.7.

[0008] Furthermore, the aspect ratio of the modified wollastonite powder is 20:1.

[0009] Furthermore, the modified wollastonite powder is prepared by the following steps:

[0010] S1. Add 2-chloro-1,3-propanediol, 2-(2,2,6,6-tetramethylpiperidin-4-yl)acetic acid and chloroform into a three-necked flask, stir until completely dissolved, then slowly add concentrated sulfuric acid, stir and heat to 110°C, keep warm for 3 hours, cool to room temperature after the reaction, add sodium bicarbonate solution for neutralization, shake and stand for stratification, take the organic phase, dry it with anhydrous sodium sulfate, filter, and distill the filtrate under reduced pressure to obtain intermediate 1; the amount ratio of 2-chloro-1,3-propanediol, 2-(2,2,6,6-tetramethylpiperidin-4-yl)acetic acid, concentrated sulfuric acid and chloroform is 9.1g:35.5g:2mL:200mL;

[0011] Under concentrated sulfuric acid and heating conditions, the molar ratio of 2-chloro-1,3-propanediol and 2-(2,2,6,6-tetramethylpiperidin-4-yl)acetic acid is controlled to be 1:2.15-2.2, then the -OH of 2-chloro-1,3-propanediol and the -COOH of 2-(2,2,6,6-tetramethylpiperidin-4-yl)acetic acid undergo esterification reaction, and the reaction process is as follows:

[0012]

[0013] S2. Replace the air in a dry three-necked flask with nitrogen at room temperature, then add intermediate 1, KH-540 (3-aminopropyltrimethoxysilane), triethylamine and DMF (N,N-dimethylformamide), stir and dissolve, then heat to 60°C, keep warm for 3 hours, cool to room temperature after the reaction, and distill under reduced pressure to obtain intermediate 2; the amount ratio of intermediate 1, KH-540, triethylamine and DMF is 35.5g:14.1mL:12.5mL:200mL;

[0014] Triethylamine is used as an acid binding agent. Under heating conditions, the molar ratio of intermediate 1 and KH-540 is controlled to be 1:1.05-1.1, and the -Cl of intermediate 1 and the -NH2 of KH-540 undergo a nucleophilic substitution reaction. The reaction process is as follows:

[0015]

[0016] S3. Add the fibrous wollastonite powder dried at 120°C for 2-3h and the mixed solution of intermediate 2 and DMF into a high-speed mixer, stir and mix at 80°C, react for 0.5-2h, and after the reaction is completed, filter, wash with anhydrous ethanol 3 times, wash with deionized water 3 times, and finally dry at 120°C for 2-3h to obtain modified wollastonite powder; the amount of intermediate 2 used is 0.5-2% of the mass of the fibrous wollastonite powder.

[0017] The trimethoxysilane on the intermediate 2 can be hydrolyzed and then condensed to form Si-O-Si and Si-OH; the -OH in Si-OH can form a hydrogen bond with the -OH on the surface of the fibrous wollastonite powder, and then dehydrate and condense to form a covalent bond.

[0018] The chemical interaction between intermediate 2 and fibrous wollastonite powder significantly reduces the surface energy of fibrous wollastonite powder and improves the dispersion of fibrous wollastonite powder in PA66 modified materials. In addition, the surface of modified wollastonite powder contains abundant lipophilic ester groups and heterocycles. Therefore, modified wollastonite powder can be highly dispersed in PA66 modified materials and fully play its role to improve the temperature resistance of PA66 modified materials.

[0019] In addition, there is a hindered amine structure on the surface of the modified wollastonite powder. The hindered amine structure has a high photostability efficiency and achieves light protection effect by capturing free radicals, decomposing hydroperoxides, quenching singlet oxygen and capturing heavy metal ions. The hindered amine structure stabilized on the surface of the modified wollastonite powder through chemical action works synergistically with phosphite antioxidants and hindered phenol antioxidants to give the PA66 modified material excellent anti-aging effect.

[0020] Therefore, under the combined effect of the modified wollastonite powder and the other raw materials, the PA66 modified material of the present invention has excellent and stable temperature resistance and anti-aging effects.

[0021] Furthermore, the anti-wear agent is a mixture of molybdenum disulfide and polytetrafluoroethylene in a mass ratio of 1:1.

[0022] Furthermore, the compatibilizer is MAH-g-PE (maleic anhydride grafted polyethylene).

[0023] Furthermore, the antioxidant includes phosphite antioxidant and hindered phenol antioxidant.

[0024] Furthermore, the phosphite antioxidant is one or both of antioxidant 168 and antioxidant 626.

[0025] Furthermore, the hindered phenol antioxidant is one or both of antioxidant 1010 and antioxidant 1098.

[0026] Furthermore, the lubricant is a compound formed by mixing calcium stearate and erucamide in a mass ratio of 1:2.

[0027] A method for preparing a PA66 modified material with good temperature resistance comprises the following steps:

[0028] (1) Weigh each raw material according to weight percentage;

[0029] (2) Dry the PA66 resin in a vacuum drying oven at 100-110° C. for 3-4 hours to ensure that the moisture content of the PA66 resin after drying is less than 0.08%;

[0030] (3) Add the dried PA66 resin, wollastonite powder, anti-wear agent, compatibilizer, antioxidant and lubricant into a high-speed mixer at a speed of 10-15 Hz, stir for 3-7 minutes, extrude, granulate and dry the mixture using a twin-screw extruder after mixing evenly, and obtain a PA66 modified material.

[0031] Furthermore, the process temperature of the twin-screw extruder in the step (3) is set to 90-150°C in zone 1, 220-230°C in zone 2, 240-250°C in zone 3, 250-260°C in zone 4, 260-270°C in zone 5, 265-275°C in zone 6, 265-275°C in zone 7, 265-275°C in zone 8, 265-275°C in zone 9, 265-275°C in zone 10, 260-270°C in zone 11, 260-270°C in zone 12, and 255-265°C in zone 13, the die head is 260-275°C, and the main engine speed is 300-400rpm.

[0032] Furthermore, in step (3), the drying temperature is 95-105° C. and the drying time is 2-4 hours.

[0033] Beneficial effects of the present invention: The PA66 modified material prepared by using PA66 as a matrix and adding modified wollastonite powder containing a hindered amine structure, a wear-resistant agent, a compatibilizer and other raw materials has excellent and stable temperature resistance and aging resistance, as well as high dimensional stability, good chemical stability and mechanical strength. In addition, the preparation process is simple, the water absorption rate and production cost are reduced, and the PA66 modified material can be further used for processing and application in gears and the like. DETAILED DESCRIPTION

[0034] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0035] Example 1

[0036] Preparation of modified wollastonite powder, the specific steps are as follows:

[0037] S1, 9.1g of 2-chloro-1,3-propanediol, 35.5g of 2-(2,2,6,6-tetramethylpiperidin-4-yl)acetic acid and 200mL of chloroform were added to a 500mL three-necked flask, stirred until completely dissolved, then 2mL of concentrated sulfuric acid was slowly added, stirred and heated to 110°C, and the reaction was kept warm for 3h. After the reaction was completed, it was cooled to room temperature, and sodium bicarbonate solution was added to neutralize it. After shaking, it was allowed to stand for stratification, and the organic phase was dried over anhydrous sodium sulfate, filtered, and the filtrate was distilled under reduced pressure to obtain intermediate 1;

[0038] S2, replace the air in a 500 mL dry three-necked flask with nitrogen at room temperature, then add 35.5 g of intermediate 1, 14.1 mL of KH-540, 12.5 mL of triethylamine and 200 mL of DMF, stir to dissolve, then heat to 60°C, keep warm for 3 h, cool to room temperature after the reaction, and distill under reduced pressure to obtain intermediate 2;

[0039] S3. Add 20 g of fibrous wollastonite powder dried at 120°C for 3 h, 0.4 g of intermediate 2 and 100 mL of DMF into a high mixer, stir and mix at 80°C, and react for 2 h. After the reaction is completed, filter, wash with anhydrous ethanol 3 times, wash with deionized water 3 times, and finally dry at 120°C for 3 h to obtain modified wollastonite powder.

[0040] Example 2

[0041] Preparation of modified wollastonite powder, the specific steps are as follows:

[0042] S1, 9.1g of 2-chloro-1,3-propanediol, 35.5g of 2-(2,2,6,6-tetramethylpiperidin-4-yl)acetic acid and 200mL of chloroform were added to a 500mL three-necked flask, stirred until completely dissolved, then 2mL of concentrated sulfuric acid was slowly added, stirred and heated to 110°C, and the reaction was kept warm for 3h. After the reaction was completed, it was cooled to room temperature, and sodium bicarbonate solution was added to neutralize it. After shaking, it was allowed to stand for stratification, and the organic phase was dried over anhydrous sodium sulfate, filtered, and the filtrate was distilled under reduced pressure to obtain intermediate 1;

[0043] S2, replace the air in a 500 mL dry three-necked flask with nitrogen at room temperature, then add 35.5 g of intermediate 1, 14.1 mL of KH-540, 12.5 mL of triethylamine and 200 mL of DMF, stir to dissolve, then heat to 60°C, keep warm for 3 h, cool to room temperature after the reaction, and distill under reduced pressure to obtain intermediate 2;

[0044] S3. Add 20 g of fibrous wollastonite powder dried at 120°C for 2.5 h, 0.2 g of intermediate 2 and 100 mL of DMF into a high mixer, stir and mix at 80°C, react for 1.5 h. After the reaction is completed, filter, wash with anhydrous ethanol 3 times, wash with deionized water 3 times, and finally dry at 120°C for 2.5 h to obtain modified wollastonite powder.

[0045] Example 3

[0046] Preparation of modified wollastonite powder, the specific steps are as follows:

[0047] S1, 9.1g of 2-chloro-1,3-propanediol, 35.5g of 2-(2,2,6,6-tetramethylpiperidin-4-yl)acetic acid and 200mL of chloroform were added to a 500mL three-necked flask, stirred until completely dissolved, then 2mL of concentrated sulfuric acid was slowly added, stirred and heated to 110°C, and the reaction was kept warm for 3h. After the reaction was completed, it was cooled to room temperature, and sodium bicarbonate solution was added to neutralize it. After shaking, it was allowed to stand for stratification, and the organic phase was dried over anhydrous sodium sulfate, filtered, and the filtrate was distilled under reduced pressure to obtain intermediate 1;

[0048] S2, replace the air in a 500 mL dry three-necked flask with nitrogen at room temperature, then add 35.5 g of intermediate 1, 14.1 mL of KH-540, 12.5 mL of triethylamine and 200 mL of DMF, stir to dissolve, then heat to 60°C, keep warm for 3 h, cool to room temperature after the reaction, and distill under reduced pressure to obtain intermediate 2;

[0049] S3. Add 20 g of fibrous wollastonite powder dried at 120°C for 2-3 h, 0.1 g of intermediate 2 and 100 mL of DMF into a high mixer, stir and mix at 80°C, react for 0.5 h. After the reaction is completed, filter, wash 3 times with anhydrous ethanol, wash 3 times with deionized water, and finally dry at 120°C for 2 h to obtain modified wollastonite powder.

[0050] Embodiment 4 to Embodiment 7

[0051] The raw material formula for preparing PA66 modified materials is shown in Table 1:

[0052] Table 1

[0053] raw material Example 4 Example 5 Example 6 Example 7 PA66 resin / % 81.7 79.7 77.7 76.7 Modified wollastonite powder / % 10 12 14 15 Wear-resistant agent / % 2 2 2 2 Compatibilizer / % 5 5 5 5 Antioxidant / % 0.3 0.3 0.3 0.3 Lubricant / % 1 1 1 1

[0054] PA66 resin is EP1106; modified wollastonite powder is the modified wollastonite powder prepared in Example 1; the anti-wear agent is molybdenum disulfide and polytetrafluoroethylene, with a mass ratio of 1:1; the compatibilizer is MAH-g-PE; the antioxidant is antioxidant 168 and antioxidant 1098, with a mass ratio of 1:2; the lubricant is calcium stearate and erucamide, with a mass ratio of 1:2.

[0055] Preparation of PA66 modified material, the specific steps are as follows:

[0056] (1) Weigh each raw material according to the raw material formula in Table 1;

[0057] (2) Dry the PA66 resin in a vacuum drying oven at 110° C. for 4 h, ensuring that the moisture content of the PA66 resin after drying is less than 0.08%.

[0058] (3) Add the dried PA66 resin, wollastonite powder, wear-resistant agent, compatibilizer, antioxidant and lubricant into a high-speed mixer at a speed of 12 Hz, stir for 6 min, and extrude and granulate the mixture using a twin-screw extruder after uniform mixing, and dry the mixture at 105° C. for 3 h to obtain a PA66 modified material, wherein the process temperature of the twin-screw extruder is set to 90° C. for zone 1, 220° C. for zone 2, 250° C. for zone 3, 260° C. for zone 4, 265° C. for zone 5, 270° C. for zone 6, 270° C. for zone 7, 275° C. for zone 8, 275° C. for zone 9, 275° C. for zone 10, 270° C. for zone 11, 265° C. for zone 12 and 260° C. for zone 13, the die head is 275° C., and the main engine speed is 300 rpm.

[0059] Example 8

[0060] Preparation of PA66 modified material, the specific steps are as follows:

[0061] (1) Weigh the following raw materials by weight: 84% PA66 resin, 10% modified wollastonite powder prepared in Example 2, 2.8% anti-wear agent, 3% compatibilizer, 0.1% antioxidant, and 0.1% lubricant;

[0062] PA66 resin uses EP1106; anti-wear agent uses molybdenum disulfide and polytetrafluoroethylene, with a mass ratio of 1:1; compatibilizer uses MAH-g-PE; antioxidant 626 and antioxidant 1010, with a mass ratio of 1:2; lubricant uses calcium stearate and erucamide, with a mass ratio of 1:2;

[0063] (2) Dry the PA66 resin in a vacuum drying oven at 100° C. for 3.5 h to ensure that the moisture content of the PA66 resin after drying is less than 0.08%.

[0064] (3) Add the dried PA66 resin, wollastonite powder, wear-resistant agent, compatibilizer, antioxidant and lubricant into a high-speed mixer at a speed of 12 Hz, stir for 6 min, extrude and granulate the mixture using a twin-screw extruder after uniform mixing, and dry at 100° C. for 2 h to obtain a PA66 modified material, wherein the process temperature of the twin-screw extruder is set to 150° C. for zone 1, 230° C. for zone 2, 245° C. for zone 3, 255° C. for zone 4, 270° C. for zone 5, 275° C. for zone 6, 275° C. for zone 7, 270° C. for zone 8, 270° C. for zone 9, 270° C. for zone 10, 265° C. for zone 11, 270° C. for zone 12 and 265° C. for zone 13, the die head is 270° C., and the main engine speed is 400 rpm.

[0065] Example 9

[0066] Preparation of PA66 modified material, the specific steps are as follows:

[0067] (1) Weigh the following raw materials by weight: 70% PA66 resin, 14% modified wollastonite powder prepared in Example 3, 4% anti-wear agent, 10% compatibilizer, 1% antioxidant, and 1% lubricant;

[0068] PA66 resin uses EP1106; anti-wear agent uses molybdenum disulfide and polytetrafluoroethylene, with a mass ratio of 1:1; compatibilizer uses MAH-g-PE; antioxidant 168 and antioxidant 1010, with a mass ratio of 1:4; lubricant uses calcium stearate and erucamide, with a mass ratio of 1:2;

[0069] (2) Dry the PA66 resin in a vacuum drying oven at 105° C. for 3 h, ensuring that the moisture content of the PA66 resin after drying is less than 0.08%.

[0070] (3) Add the dried PA66 resin, wollastonite powder, wear-resistant agent, compatibilizer, antioxidant and lubricant into a high-speed mixer at a speed of 12 Hz, stir for 6 min, extrude and granulate the mixture using a twin-screw extruder after uniform mixing, and dry at 95° C. for 4 h to obtain a PA66 modified material, wherein the process temperature of the twin-screw extruder is set to 120° C. for zone 1, 225° C. for zone 2, 240° C. for zone 3, 250° C. for zone 4, 260° C. for zone 5, 265° C. for zone 6, 265° C. for zone 7, 265° C. for zone 8, 265° C. for zone 9, 265° C. for zone 10, 260° C. for zone 11, 260° C. for zone 12 and 255° C. for zone 13, the die head is 260° C., and the main engine speed is 350 rpm.

[0071] Comparative Example 1

[0072] Preparation of PA66 modified material, the specific steps are as follows:

[0073] The remaining steps remained unchanged, except that the modified wollastonite powder in Example 4 was replaced with 9.8% of untreated wollastonite powder and 0.2% of light stabilizer 744 to obtain a PA66 modified material.

[0074] Performance Testing

[0075] The PA66 modified materials prepared in Examples 4-9 were subjected to the following performance tests, and the test results are shown in Table 2 below:

[0076] Table 2

[0077]

[0078] It can be seen from Table 2 that the various properties of the PA66 modified material prepared in Example 1 are better than those in Comparative Example 1; at the same time, it can be seen that the temperature resistance of the PA66 modified material prepared in Example 7 is better than that in other examples, indicating that the addition amount of modified wollastonite powder has a great influence on the mechanical properties and temperature resistance, and should be selected and designed according to the product application in actual operation.

[0079] The PA66 modified materials prepared in Examples 4-9 were dry-heat aged at 110° C. for 150 h, and then tested for tensile strength according to the test method of ISO 527, and for flexural strength according to the test method of ISO 178. The test results are shown in Table 3 below:

[0080] Table 3

[0081]

[0082] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0083] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.

Claims

1. A PA66 modified material with good temperature resistance, It is characterized in that The raw materials include the following weight percentages: PA66 resin 70-84%, modified wollastonite powder 10-15%, anti-wear agent 2-4%, compatibilizer 3-10%, antioxidant 0.1-1%, lubricant 0.1-1%; Wherein, the modified wollastonite powder is prepared by the following steps: S1. Add 2-chloro-1,3-propanediol, 2-(2,2,6,6-tetramethylpiperidin-4-yl)acetic acid and chloroform into a flask and stir, add concentrated sulfuric acid, react at 110° C. for 3 h, cool, neutralize, separate, take the organic phase, dry, filter, and distill the filtrate under reduced pressure to obtain intermediate 1; S2, replace the air in the flask with nitrogen, add intermediate 1, KH-540, triethylamine and DMF, stir and heat to 60°C for 3h, cool and distill under reduced pressure to obtain intermediate 2; S3. Add the dried fibrous wollastonite powder, intermediate 2 and DMF into a high-speed mixer, stir and react at 80° C. for 0.5-2 h, filter, wash and dry to obtain modified wollastonite powder.

2. A PA66 modified material with good temperature resistance according to claim 1, It is characterized in that The amount ratio of 2-chloro-1,3-propanediol, 2-(2,2,6,6-tetramethylpiperidin-4-yl)acetic acid, concentrated sulfuric acid and chloroform in step S1 is 9.1g:35.5g:2mL:200mL; the amount ratio of intermediate 1, KH-540, triethylamine and DMF in step S2 is 35.5g:14.1mL:12.5mL:200mL; the amount of intermediate 2 in step S3 is 0.5-2% of the mass of fibrous wollastonite powder.

3. A PA66 modified material with good temperature resistance according to claim 1, It is characterized in that The relative viscosity of the PA66 resin is 2.2-2.7; the aspect ratio of the modified wollastonite powder is 20:

1.

4. The PA66 modified material with good temperature resistance according to claim 1, It is characterized in that The anti-wear agent is a mixture of molybdenum disulfide and polytetrafluoroethylene in a mass ratio of 1:1; the compatibilizer is MAH-g-PE.

5. The PA66 modified material with good temperature resistance according to claim 1, It is characterized in that The antioxidants include phosphite antioxidants and hindered phenol antioxidants.

6. A PA66 modified material with good temperature resistance according to claim 5, It is characterized in that The phosphite antioxidant is one or both of antioxidant 168 and antioxidant 626; the hindered phenol antioxidant is one or both of antioxidant 1010 and antioxidant 1098.

7. The PA66 modified material with good temperature resistance according to claim 1, It is characterized in that The lubricant is a compound prepared by mixing calcium stearate and erucamide in a mass ratio of 1:

2.

8. The method for preparing a PA66 modified material with good temperature resistance according to claim 1, It is characterized in that The following steps are involved: (1) Weigh each raw material according to weight percentage; (2) drying the PA66 resin to ensure that the moisture content of the PA66 resin after drying is less than 0.08%; (3) Add the dried PA66 resin, wollastonite powder, anti-wear agent, compatibilizer, antioxidant, and lubricant into a high-speed mixer, stir, and after mixing evenly, extrude, granulate, and dry using a twin-screw extruder to obtain a PA66 modified material.

9. The method for preparing a PA66 modified material with good temperature resistance according to claim 8, It is characterized in that In the step (3), the process temperature of the twin-screw extruder is set to 90-150°C for zone 1, 220-230°C for zone 2, 240-250°C for zone 3, 250-260°C for zone 4, 260-270°C for zone 5, 265-275°C for zone 6, 265-275°C for zone 7, 265-275°C for zone 8, 265-275°C for zone 9, 265-275°C for zone 10, 260-270°C for zone 11, 260-270°C for zone 12, and 255-265°C for zone 13, the die head is 260-275°C, and the main engine speed is 300-400rpm.

10. The method for preparing a PA66 modified material with good temperature resistance according to claim 8, It is characterized in that In the step (3), the drying temperature is 95-105° C. and the drying time is 2-4 hours.