Process for recovering and preparing refined tin from tin-containing tungsten slag

Through the processes of dilute acid leaching, ammonia water reaction, concentrated acid leaching, ionic liquid microemulsion extraction and stripping agent reverse extraction, the problem of tin ore resource depletion is solved, and high efficiency recovery of high-purity refined tin is achieved, with a high tin recovery rate of up to tin More than 97%, simplifying the process flow and reducing energy consumption.

CN119040654APending Publication Date: 2024-11-29YONGXING CHANGLONG ENVIRONMENTAL PROTECTION TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411179423.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Tin ore resources are exhausted. How to improve the purity and recovery rate of tin recycling from tin-containing waste and make full use of tin resources.

Method used

Using dilute acid leaching, ammonia water reaction, concentrated acid leaching, ionic liquid microemulsion extraction and stripping agent retrieval, high-purity refined tin is obtained through electrolysis, which eliminates the high-temperature carbon-heat reduction step and reduces the equipment requirements. and energy consumption.

Benefits of technology

The efficient recycling and reuse of tin elements is achieved, the purity of refined tin reaches more than 99.9%, and the tin recovery rate is ≥97%, which simplifies the process flow and reduces the operation complexity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005011662970000031
    Figure BDA0005011662970000031
  • Figure BDA0005011662970000051
    Figure BDA0005011662970000051
  • Figure BDA0005011662970000061
    Figure BDA0005011662970000061
Patent Text Reader

Abstract

The invention relates to the technical field of metal waste recovery, in particular to a process for recovering and preparing refined tin from tin-containing tungsten slag, which comprises the following steps: performing acid leaching on the tin-containing tungsten slag with dilute acid, filtering to obtain primary filter residue, reacting the primary filter residue with ammonia water, filtering again to obtain secondary filter residue, adding concentrated acid into the secondary filter residue, performing acid leaching, and filtering to obtain filtrate; according to the technology, the refined tin can be recycled and prepared from the tin-containing tungsten slag, the purity of the recycled refined tin reaches 99.9% or above, the tin recycling rate is larger than or equal to 97%, the recycling rate of the tin is larger than or equal to 97%, the recycling rate of the tin is larger than or equal to 99%, and the recycling rate of the tin is larger than or equal to 99%. And high-efficiency recycling and reusing of the tin element are realized on the whole.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metal waste recycling, in particular to a process for recovering and preparing refined tin from tin-containing tungsten slag. Background Art

[0002] Tin has become an indispensable material in many industrial fields due to its unique physical and chemical properties. First of all, tin has a low melting point and is easy to process and shape, which makes it extremely flexible in the manufacturing process. At the same time, tin has excellent ductility and plasticity, and can be easily drawn into wires or forged into various shapes to meet diverse production needs. In the electronics industry, as the main component of solder, tin is alloyed with metals such as lead to form solder with good melting point and fluidity, which can ensure the precise connection between electronic components and improve the stability and reliability of electronic products. In the field of food packaging, packaging materials such as tin cans and tin foil can effectively protect food from external pollution and oxidation due to their good sealing and corrosion resistance, and extend the shelf life of food. After tin is alloyed with metals such as copper, lead, and silver, alloy materials with excellent properties can be formed, such as bronze, lead-tin alloy, and tin-silver alloy. These alloy materials are widely used in machinery, chemical industry, construction and other fields, such as manufacturing precision devices such as valves, pipes, bearings, springs, and corrosion-resistant and wear-resistant industrial equipment.

[0003] However, tin is a non-renewable resource with limited global reserves. With the development of science and technology and industry, the increasing demand for tin and the continuous depletion of tin ore resources have become problems that cannot be ignored at home and abroad. Therefore, tin-containing waste has become an important source of tin extraction. How to make full use of these resources and improve the purity and recovery rate of recycled tin has become the current research focus. Summary of the invention

[0004] Purpose of the invention: In view of the above technical problems, the present invention proposes a process for recovering and preparing refined tin from tin-containing tungsten slag.

[0005] The technical solutions adopted are as follows:

[0006] A process for recovering and preparing refined tin from tin-containing tungsten slag:

[0007] The tin-containing tungsten slag is acid-leached with dilute acid and then filtered to obtain a primary filter residue. The primary filter residue is reacted with ammonia water and then filtered again to obtain a secondary filter residue. The secondary filter residue is acid-leached with concentrated acid and then filtered to obtain a filtrate. The filtrate is mixed with an ionic liquid microemulsion for extraction, the ionic liquid microemulsion phase is separated, and then stripping is performed with a stripping agent. Finally, the stripping agent is electrolyzed to obtain refined tin.

[0008] Furthermore, the tin-containing tungsten slag is tailings produced during the smelting process of tungsten ore, wherein the mass content of tin is ≥1.2%.

[0009] Furthermore, the dilute acid is any one or more combinations of dilute nitric acid, dilute hydrochloric acid and dilute sulfuric acid.

[0010] Furthermore, the temperature of the reaction between the primary filter residue and aqueous ammonia is 60-90°C.

[0011] Furthermore, the concentrated acid is any one or more combinations of concentrated nitric acid, concentrated hydrochloric acid and concentrated sulfuric acid.

[0012] Furthermore, the preparation method of the ionic liquid microemulsion is as follows:

[0013] The imidazolium ionic liquid is added to the mixed organic phase of n-heptane and n-butanol, and the mixture is evenly mixed by ultrasonic treatment. Then, deionized water is added dropwise until the aqueous phase just precipitates, and the upper organic phase is the ionic liquid microemulsion.

[0014] Furthermore, the structural formula of the cation in the imidazolium ionic liquid is as follows:

[0015]

[0016] Wherein, L is an alkylene group having ≥6 carbon atoms, and R is an alkyl group having ≥6 carbon atoms.

[0017] Furthermore, the anion in the imidazolium ionic liquid is any one of a bromide ion, a tetrafluoroborate ion, and a hexafluorophosphate ion.

[0018] Furthermore, the stripping agent is any one of sodium chloride solution, potassium bromide solution, thiourea solution, hydrochloric acid solution, and sodium hydroxide solution.

[0019] Furthermore, the volume ratio of the ionic liquid microemulsion phase to the stripping agent is 1:5-10.

[0020] Beneficial effects of the present invention:

[0021] The invention provides a process for recovering and preparing refined tin from tin-containing tungsten slag. First, the tin dioxide in the tin-containing tungsten slag is insoluble in dilute acid. After other valuable metals are recovered by dilute acid leaching, the tin dioxide is enriched in a primary filter residue. Alkaline-soluble impurities such as sodium tungstate are removed by ammonia water. After secondary enrichment, concentrated acid leaching is used to dissolve the tin ions. Then, an ionic liquid microemulsion is used to extract the tin ions and a stripping agent is used to strip the tin ions, thereby separating the tin ions from other impurity ions. Finally, refined tin with high yield and high purity is obtained by electrolysis.

[0022] In the present invention, due to the presence of the linking group, the repulsive force between the hydrophilic groups is weakened, and at the same time, the two alkyl chains in the structure increase the hydrophobic property. The special structure makes it have many unique properties. The prepared ionic liquid microemulsion has better selectivity for tin ions and higher extraction rate.

[0023] Moreover, compared with pyrometallurgy, the process provided by the present invention omits the high-temperature carbon thermal reduction step, has lower equipment requirements, is simpler to operate, and consumes less energy. It can recover and prepare refined tin from tin-containing tungsten slag. The purity of the recovered refined tin is as high as over 99.9%, and the tin recovery rate is ≥97%, thus achieving efficient recovery and reuse of the tin element as a whole. DETAILED DESCRIPTION

[0024] If the specific conditions are not specified in the examples, the experiments were carried out under conventional conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be purchased commercially. The techniques not mentioned in the present invention are all referenced to the prior art. Unless otherwise specified, the following examples and comparative examples are parallel experiments, using the same processing steps and parameters.

[0025] Embodiment 1:

[0026] A process for recovering and preparing refined tin from tin-containing tungsten slag:

[0027] 1 kg of scheelite slag with a tin content of 1.5% was added to 100 L of 1 mol / L dilute sulfuric acid, stirred and acid-leached at 50°C for 5 hours, and then filtered to obtain a primary filter residue. The primary filter residue was fully washed with water and added to 100 L of ammonia water, stirred and reacted at 80°C for 2 hours, and then filtered again to obtain a secondary filter residue. The secondary filter residue was fully washed with water and added to 50 L of concentrated sulfuric acid, stirred and acid-leached at 80°C for 5 hours, and then filtered to collect the filtrate;

[0028] Dissolve 0.5 mol of imidazole in 600 ml of toluene and 600 ml of dimethyl sulfoxide, add 400 g of 50% NaOH aqueous solution, remove water by distillation through a condenser, then add 2.5 mol of 1,6-dibromohexane dropwise, stir at 120°C for 2 h, remove NaBr by hot filtration, remove the solvent under vacuum drying conditions, then dissolve the resulting crude product in 1000 ml of dichloromethane and filter out the residual NaBr, take 0.5 mol of the product and 1.1 mol of 1-bromooctane and dissolve them in 250 ml of isopropanol, stir and reflux at 70°C for 24 h, then remove the isopropanol solvent in vacuo at 60°C, recrystallize with ethyl acetate 3 times, 400 ml each time, to obtain an ionic liquid with the following structural formula (L is (CH2)6, R is n-octyl);

[0029]

[0030] 50g of the above ionic liquid was added to a mixed organic phase of 700ml n-heptane and 300ml n-butanol, and the mixture was evenly mixed by ultrasonic treatment. Deionized water was then added dropwise until the aqueous phase just precipitated. The upper organic phase was taken as the ionic liquid microemulsion. The filtrate was mixed with the ionic liquid microemulsion at a volume ratio of 3:1 for extraction, and the ionic liquid microemulsion phase was separated. Then, 0.1mol / L sodium chloride aqueous solution was used as a stripping agent for stripping. The volume ratio of the ionic liquid microemulsion phase to the stripping agent was 1:5. The tin-containing stripping agent was separated and injected into the electrolytic cell. The anode was a graphite electrode and the cathode was a stainless steel plate. At a current density of 120A / m 2 , electrolysis is carried out at a temperature of 40°C and a stirring speed of 200 rpm, and the cathode precipitate is collected, washed, and dried to obtain refined tin.

[0031] Embodiment 2:

[0032] A process for recovering and preparing refined tin from tin-containing tungsten slag:

[0033] 1 kg of scheelite slag with a tin content of 1.5% was added to 100 L of 1 mol / L dilute sulfuric acid, stirred and acid-leached at 50°C for 5 hours, and then filtered to obtain a primary filter residue. The primary filter residue was fully washed with water and added to 100 L of ammonia water, stirred and reacted at 80°C for 2 hours, and then filtered again to obtain a secondary filter residue. The secondary filter residue was fully washed with water and added to 50 L of concentrated sulfuric acid, stirred and acid-leached at 80°C for 5 hours, and then filtered to collect the filtrate;

[0034] Dissolve 0.5 mol of imidazole in 600 ml of toluene and 600 ml of dimethyl sulfoxide, add 400 g of 50% NaOH aqueous solution, remove water by distillation through a condenser, then add 2.5 mol of 1,6-dibromohexane dropwise, and stir at 120°C for 2 h, remove NaBr by hot filtration, remove the solvent under vacuum drying conditions, then dissolve the resulting crude product in 1000 ml of dichloromethane and filter out residual NaBr, take 0.5 mol of the product and 1.1 mol of 1-bromooctane and dissolve them in 250 ml of isopropanol, stir and reflux at 70°C for 24 h, then remove the isopropanol solvent in vacuo at 60°C, recrystallize with ethyl acetate 3 times with 400 ml each time, and finally carry out anion replacement with the same amount of NaBF4 to obtain an ionic liquid with the following structural formula (L is (CH2)6, R is n-octyl);

[0035]

[0036] 50g of the above ionic liquid was added to a mixed organic phase of 700ml n-heptane and 300ml n-butanol, and the mixture was evenly mixed by ultrasonic treatment. Deionized water was then added dropwise until the aqueous phase just precipitated. The upper organic phase was taken as the ionic liquid microemulsion. The filtrate was mixed with the ionic liquid microemulsion at a volume ratio of 3:1 for extraction, and the ionic liquid microemulsion phase was separated. Then, 0.1mol / L sodium chloride aqueous solution was used as a stripping agent for stripping. The volume ratio of the ionic liquid microemulsion phase to the stripping agent was 1:5. The tin-containing stripping agent was separated and injected into the electrolytic cell. The anode was a graphite electrode and the cathode was a stainless steel plate. At a current density of 120A / m 2 , electrolysis is carried out at a temperature of 40°C and a stirring speed of 200 rpm, and the cathode precipitate is collected, washed, and dried to obtain refined tin.

[0037] Embodiment 3:

[0038] A process for recovering and preparing refined tin from tin-containing tungsten slag:

[0039] 1 kg of scheelite slag with a tin content of 1.5% was added to 100 L of 1 mol / L dilute sulfuric acid, stirred and acid-leached at 50°C for 5 hours, and then filtered to obtain a primary filter residue. The primary filter residue was fully washed with water and added to 100 L of ammonia water, stirred and reacted at 80°C for 2 hours, and then filtered again to obtain a secondary filter residue. The secondary filter residue was fully washed with water and added to 50 L of concentrated sulfuric acid, stirred and acid-leached at 80°C for 5 hours, and then filtered to collect the filtrate;

[0040] Dissolve 0.5 mol of imidazole in 600 ml of toluene and 600 ml of dimethyl sulfoxide, add 400 g of 50% NaOH aqueous solution, remove water by distillation through a condenser, then add 2.5 mol of 1,6-dibromohexane dropwise, and stir at 120°C for 2 h, remove NaBr by hot filtration, remove the solvent under vacuum drying conditions, then dissolve the resulting crude product in 1000 ml of dichloromethane and filter out residual NaBr, take 0.5 mol of the product and 1.1 mol of 1-bromooctane and dissolve them in 250 ml of isopropanol, stir and reflux at 70°C for 24 h, then remove the isopropanol solvent in vacuo at 60°C, recrystallize with ethyl acetate 3 times with 400 ml each time, and finally carry out anion replacement with the same amount of NaPF6 to obtain an ionic liquid with the following structural formula (L is (CH2)6, R is n-octyl);

[0041]

[0042] 50g of the above ionic liquid was added to a mixed organic phase of 700ml n-heptane and 300ml n-butanol, and the mixture was evenly mixed by ultrasonic treatment. Deionized water was then added dropwise until the aqueous phase just precipitated. The upper organic phase was taken as the ionic liquid microemulsion. The filtrate was mixed with the ionic liquid microemulsion at a volume ratio of 3:1 for extraction, and the ionic liquid microemulsion phase was separated. Then, 0.1mol / L sodium chloride aqueous solution was used as a stripping agent for stripping. The volume ratio of the ionic liquid microemulsion phase to the stripping agent was 1:5. The tin-containing stripping agent was separated and injected into the electrolytic cell. The anode was a graphite electrode and the cathode was a stainless steel plate. At a current density of 120A / m 2 , electrolysis is carried out at a temperature of 40°C and a stirring speed of 200 rpm, and the cathode precipitate is collected, washed, and dried to obtain refined tin.

[0043] Comparative Example 1:

[0044] The method is basically the same as Example 1, except that Triton X-100 is used instead of the homemade ionic liquid.

[0045] Comparative Example 2:

[0046] The method is basically the same as Example 1, except that sodium oleate is used instead of the homemade ionic liquid.

[0047] Comparative Example 3:

[0048] The method is substantially the same as Example 1, except that 1-octyl-3-methylimidazolium bromide is used instead of the homemade ionic liquid.

[0049] Performance Testing:

[0050] The purity of the refined tin recovered in Examples 1-3 of the present invention and Comparative Examples 1-3 was tested and the recovery rate was calculated. The results are shown in Table 1 below:

[0051] Table 1:

[0052]

[0053] As can be seen from Table 1 above, the method provided by the present invention can recover and prepare refined tin from tin-containing tungsten slag, the purity of the recovered refined tin is as high as over 99.9%, and the tin recovery rate is ≥97%, which generally achieves efficient recovery and reuse of tin element.

[0054] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A process for recovering refined tin from tin-containing tungsten slag, characterized in that: The tin-containing tungsten slag is acid-leached with dilute acid and then filtered to obtain a primary filter residue. The primary filter residue is reacted with ammonia water and then filtered again to obtain a secondary filter residue. The secondary filter residue is acid-leached with concentrated acid and then filtered to obtain a filtrate. The filtrate is mixed with an ionic liquid microemulsion for extraction, the ionic liquid microemulsion phase is separated, and then stripping is performed with a stripping agent. Finally, the stripping agent is electrolyzed to obtain refined tin.

2. The process for recovering refined tin from tin-containing tungsten slag as claimed in claim 1, characterized in that: The tin-containing tungsten slag is tailings produced during the smelting process of tungsten ore, wherein the mass content of tin is ≥1.2%.

3. The process for recovering refined tin from tin-containing tungsten slag as claimed in claim 1, characterized in that: The dilute acid is any one or more combinations of dilute nitric acid, dilute hydrochloric acid and dilute sulfuric acid.

4. The process for recovering refined tin from tin-containing tungsten slag as claimed in claim 1, characterized in that: The temperature of the reaction between the primary filter residue and aqueous ammonia is 60-90°C.

5. The process for recovering refined tin from tin-containing tungsten slag as claimed in claim 1, characterized in that: The concentrated acid is any one or more combinations of concentrated nitric acid, concentrated hydrochloric acid and concentrated sulfuric acid.

6. The process for recovering refined tin from tin-containing tungsten slag as claimed in claim 1, characterized in that: The preparation method of the ionic liquid microemulsion is as follows: The imidazolium ionic liquid is added to the mixed organic phase of n-heptane and n-butanol, and the mixture is evenly mixed by ultrasonic treatment. Then, deionized water is added dropwise until the aqueous phase just precipitates, and the upper organic phase is the ionic liquid microemulsion.

7. The process for recovering refined tin from tin-containing tungsten slag as claimed in claim 6, characterized in that: The structural formula of the cation in the imidazolium ionic liquid is as follows: Wherein, L is an alkylene group having ≥6 carbon atoms, and R is an alkyl group having ≥6 carbon atoms.

8. The process for recovering refined tin from tin-containing tungsten slag as claimed in claim 6, characterized in that: The anion in the imidazolium ionic liquid is any one of a bromide ion, a tetrafluoroborate ion and a hexafluorophosphate ion.

9. The process for recovering refined tin from tin-containing tungsten slag as claimed in claim 1, characterized in that: The stripping agent is any one of sodium chloride solution, potassium bromide solution, thiourea solution, hydrochloric acid solution and sodium hydroxide solution.

10. The process for recovering refined tin from tin-containing tungsten slag according to claim 1, characterized in that: The volume ratio of the ionic liquid microemulsion phase to the stripping agent is 1:5-10.