Continuous casting method for steel
By controlling the water density and temperature gradient through strong cooling and light pressure in a specific zone within a continuous casting machine, the problem of center segregation in steel castings is solved, improving the quality of the steel, especially its performance in pipeline materials.
Patent Information
- Application Number
- CN202380030669.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-28
- Filing Date
- 2023-03-23
- Publication Date
- 2024-11-29
AI Technical Summary
Existing technologies are insufficient to effectively reduce center segregation in steel castings, leading to a decline in steel quality, especially when used in pipeline materials, which fail to meet high-quality requirements.
Strong cooling and light pressing are performed in specific zones within the continuous casting machine. By controlling the water density and temperature gradient, the cooling and pressing process of the casting is optimized, reducing center segregation.
It significantly reduces center segregation and internal cracks in the casting, improves steel quality, and meets the requirements of high-quality pipeline materials.
Smart Images

Figure CN119053396A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a continuous casting method for steel, and more particularly to a continuous casting method for steel which is effective in reducing center segregation generated in a cast piece. Background Art
[0002] Generally, it is known that during the solidification process of steel, solute elements such as carbon, phosphorus, sulfur, and manganese are concentrated on the unsolidified liquid phase side by redistribution during solidification, resulting in micro segregation between dendrite trees.
[0003] In addition, when steel is cast using a continuous casting machine, the solidifying continuous casting slab (hereinafter also referred to as "slab") sometimes forms a gap or generates negative pressure in the thickness center of the slab due to solidification shrinkage or thermal shrinkage, bulging of the solidified shell generated between the rollers of the continuous casting machine, etc. Therefore, the molten steel is attracted to the thickness center of the slab. However, since there is not enough molten steel in the unsolidified layer at the end of solidification, the molten steel between the dendrite trees where the solute elements are concentrated is attracted to the thickness center and moves to solidify there. The concentration of the solute element at the segregation point in the thickness center of the slab formed in this way becomes an exceptionally high value compared to the initial concentration of the molten steel. This phenomenon is generally called "macrosegregation" and is also called "center segregation" according to its location.
[0004] The above-mentioned center segregation of the cast piece will significantly reduce the quality of steel materials, such as the quality of pipelines for transporting crude oil or natural gas. Such reduction in the quality of steel materials is caused, for example, by the following reasons: hydrogen that has penetrated into the steel due to corrosion reactions diffuses around manganese sulfide (MnS), niobium carbide (NbC), etc. generated in the center segregation part and gathers, generating cracks caused by its internal pressure. In addition, such a center segregation part is hardened due to the high concentration of solute elements, so the above-mentioned cracks further propagate to the surroundings and expand. This crack is called hydrogen induced cracking (HIC). Therefore, reducing the center segregation in the center of the thickness of the cast piece is extremely important for improving the quality of steel products.
[0005] In the past, many technologies for reducing and harmlessly treating the center segregation of the cast piece between the continuous casting process and the rolling process have been proposed. For example, in Patent Documents 1 and 2, a technology is proposed in which a cast piece having an unsolidified layer in the final stage of solidification is gradually pressed down by a reduction amount corresponding to the sum of the solidification shrinkage and the thermal shrinkage using a cast piece support roller in a continuous casting machine while casting. This technology is called a light reduction method. In such a light reduction method, when the cast piece is pulled out using a plurality of pairs of cast piece support rollers arranged in the casting direction, the cast piece is gradually pressed down by a reduction amount corresponding to the sum of the solidification shrinkage and the thermal shrinkage, so that the volume of the unsolidified layer is reduced, thereby preventing the formation of voids and negative pressure portions in the center of the cast piece. By adopting such a mechanism (light reduction method), the thickened molten steel between the dendrite trees is prevented from being attracted from between the dendrite trees to the thickness center of the cast piece, thereby reducing the center segregation generated in the cast piece.
[0006] In addition, it is known that there is a close relationship between the morphology of the dendrite structure in the center of the thickness and the center segregation. For example, Patent Document 3 proposes the following technology: by setting the specific water amount at a specific position in the casting direction of the secondary cooling zone of the continuous casting machine to 0.5L / kg-steel or more, the refinement and equiaxed crystallization of the solidification structure are promoted to reduce the center segregation. In addition, Patent Document 4 proposes the following technology: by appropriately adjusting the pressing conditions and cooling conditions, the dendrite primary arm spacing in the center of the thickness of the casting is set to 1.6mm or less to reduce the center segregation.
[0007] On the other hand, although the purpose of the technology is to prevent surface cracks of the cast piece, Patent Document 5 proposes a technology for heating the surface of the cast piece as a method for controlling the temperature of the cast piece in the continuous casting machine. In the technology proposed in Patent Document 5, the surface layer of the cast piece is heated at an average rate of more than 30°C / min in the correction zone of the continuous casting machine, thereby preventing surface cracks during the correction of the cast piece.
[0008] Prior art literature
[0009] Patent Literature
[0010] Patent Document 1: (Japanese) Patent Publication No. 08-132203
[0011] Patent Document 2: (Japanese) Patent Publication No. 08-192256
[0012] Patent Document 3: (Japanese) Patent Publication No. 08-224650
[0013] Patent Document 4: (Japanese) Patent Publication No. 2016-28827
[0014] Patent Document 5: (Japanese) Patent Publication No. 2008-100249 Summary of the invention
[0015] Technical problem to be solved by the invention
[0016] In the inventions described in Patent Documents 1 and 2, the center segregation can be reduced by adopting the soft reduction method. However, these technologies are insufficient as methods for reducing the center segregation to the quality level required for steel pipes such as line pipes in recent years.
[0017] In addition, in the inventions described in Patent Documents 3 and 4, in addition to the soft reduction method, the secondary cooling conditions are adjusted to refine the solidification structure and reduce the center segregation. However, the level of segregation reduction required for steel pipes such as pipelines is increasing year by year, and it is still insufficient to reduce the segregation degree to the level required in the future. In order to further reduce the segregation, for example, continuous casting of steel under the optimal soft reduction conditions can be considered, but in the methods of Patent Documents 3 and 4, it is difficult to reduce the center segregation beyond the current level.
[0018] In addition, the slab heating device of Patent Document 5 is limited in installation space within the continuous casting machine. Therefore, although it can be used as a local heating method, it cannot control the entire slab to a uniform temperature.
[0019] The present invention is a method developed in view of the above-mentioned problems existing in the prior art, and its object is to propose a new steel continuous casting method that can effectively reduce the center segregation generated in the cast piece.
[0020] Means for solving problems
[0021] Therefore, the inventors conducted in-depth research to solve the above problems in the prior art. As a result, it was found that in the cooling process of the cast piece in the continuous casting of steel, if the cast piece is cooled at a preferred water density in a specific section, the center segregation in the cast piece can be greatly reduced, thereby developing the present invention.
[0022] The present invention has been accomplished based on the above findings, and its main structure is as follows.
[0023] A continuous casting method for steel, characterized in that, along the casting strip drawing direction in a continuous casting machine, when the range from a starting point to an end point is set as a first section, the water density per unit casting strip surface area in the first section is 50L / (m 2 ×min) and above 2000L / (m 2The casting is cooled within a range of 0.100 × min or less, the starting point being a starting point where the average value of the solid phase ratio along the thickness direction at the final solidification portion in the width direction of the casting is 0.8 or less, and the end point being an end point where the average value of the solid phase ratio along the thickness direction at the final solidification portion in the width direction of the casting is greater than the solid phase ratio at the starting point and is 1.0 or less.
[0024] The present invention described above may more preferably adopt the following embodiments.
[0025] (1) When the average solid phase ratio in the width direction at the end point is 1.0 or less and the section located downstream of the first section is defined as the second section, the water density per unit surface area of the slab in the second section is 50 L / (m 2 ×min) and above 300L / (m 2 ×min) or less to cool the casting;
[0026] (2) at least during the period from the end of the first section to the passage through the second section, the casting is performed while maintaining the surface temperature of the cast piece at a nucleate boiling state of 200° C. or less, so that the temperature gradient near the center of the thickness of the cast piece at the end of solidification is 1.7 to 3.5 K / mm;
[0027] (3) The first section and the second section are arranged in an area limited to a horizontal section or a vertical section in the continuous casting machine;
[0028] (4) in the first and second intervals, applying light pressure to press down the long side of the casting at a speed of 0.3 to 2.0 mm / min;
[0029] (5) The long side of the slab is bulged by a total bulging amount of 2 to 20 mm by gradually increasing the roll opening of the plurality of pairs of slab support rolls toward the downstream side in the casting direction, and then the roll opening of the plurality of pairs of slab support rolls is gradually reduced toward the downstream side in the casting direction to lightly press down the slab.
[0030] Effects of the Invention
[0031] By adopting the continuous casting method of steel of the present invention having the above-mentioned essential structure, the continuous cast piece can be effectively cooled, and the center segregation and internal cracks expected to occur in the continuously cast piece can be reduced. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 This is a schematic diagram showing an example of a continuous casting machine effective for carrying out the continuous casting method of steel according to the present invention.
[0033] Figure 2 It is a diagram for explaining the final solidification position in the width direction of the slab.
[0034] Figure 3 It is a cross-sectional view of the casting cut along a plane perpendicular to the drawing direction of the casting.
[0035] Figure 4 This is a graph showing the relationship between the temperature gradient near the center of the slab thickness in Experiment 1 and the number of segregated grains.
[0036] Figure 5 This is a graph showing the relationship between the water density in Experiment 2 and the temperature gradient near the center of the slab thickness.
[0037] Figure 6 This is a graph showing the relationship between the water density and the temperature drop time in Experiment 3.
[0038] Figure 7 This is a graph showing the relationship between the average value of the solid phase ratio at the start of strong cooling in Experiment 4 and the temperature gradient near the center of the slab thickness.
[0039] Figure 8 This is a graph showing the influence of the reduction rate on the segregation degree during strong cooling and soft reduction. DETAILED DESCRIPTION
[0040] Hereinafter, preferred embodiments of the present invention will be described with reference to the accompanying drawings. However, the scope of the present invention is not limited to the examples shown in the drawings.
[0041] Figure 1 This is a schematic diagram showing an example of a continuous casting machine effective for carrying out the continuous casting method of steel according to the present invention. Figure 1 The illustrated continuous casting machine 11 is an example of a vertical curved type continuous casting machine. It should be noted that in the present invention, a curved type or a completely vertical type continuous casting machine may be used instead of the vertical curved type.
[0042] Figure 1 The continuous casting machine 11 shown in the figure includes a casting mold 13, a tundish 14, a plurality of pairs of cast piece support rollers 16, a plurality of spray nozzles 17, etc. As shown in the figure, the cast piece 18 is drawn along the cast piece drawing direction D1. In addition, in the figure, the tundish 14 side along the cast piece drawing direction D1 is described as the upstream side, and the front side where the cast piece 18 is drawn is described as the downstream side.
[0043] The tundish 14 is disposed above the mold 13 and is used to supply the molten steel 12 to the mold 13. The molten steel 12 supplied from the ladle (not shown) is stored in the tundish 14. Therefore, a sliding nozzle (not shown) for adjusting the flow rate of the molten steel 12 is provided at the bottom of the tundish 14, and an immersion nozzle 15 is provided on the lower surface of the sliding nozzle.
[0044] The continuous casting mold 13 is provided below the tundish 14, and molten steel 12 is poured into the mold 13 from the tundish 14 via the immersion nozzle 15. The poured molten steel 12 is cooled in the mold 13 (primary cooling), thereby forming a shell shape of the cast piece 18.
[0045] like Figure 1 As shown in the figure, a plurality of pairs of cast sheet support rollers 16 are arranged to support the cast sheet 18 from both sides along the cast sheet drawing direction D1. The cast sheet support rollers 16 composed of a plurality of pairs are composed of a plurality of pairs of support rollers composed of, for example, a support roller pair, a guide roller pair, and a pinch roller pair. In addition, as shown in the figure, a plurality of pairs of cast sheet support rollers 16 are assembled to form a section 20.
[0046] A plurality of spray nozzles 17 are disposed between the adjacent slab support rolls 16 along the slab drawing direction D1. These spray nozzles 17 are nozzles for spraying cooling water toward the slab 18 to perform secondary cooling on the slab 18. As the spray nozzles 17, a water spray nozzle (single-fluid spray nozzle), an air mist spray nozzle (two-fluid spray nozzle), or the like can be used.
[0047] The cast piece 18 is cooled while being drawn along the cast piece drawing direction D1 by the cooling water (secondary cooling water) sprayed from the plurality of spray nozzles 17. Figure 1 In FIG. 1 , the unsolidified portion 18a of the molten steel in the casting 18 is indicated by oblique lines. Figure 1 In the figure, reference numeral 18b indicates a solidification completion position where the unsolidified portion 18a disappears and solidification is completed.
[0048] The downstream portion of the continuous casting machine 11 is a light reduction zone 19 for lightly reducing the cast piece 18. The light reduction zone 19 is provided with a plurality of sections 20a and 20b consisting of a plurality of pairs of cast piece support rollers 16. The plurality of cast piece support rollers 16 of the light reduction zone 19 are arranged so that the roller interval in the thickness direction of the cast piece 18 of each roller pair gradually narrows toward the cast piece drawing direction D1, thereby lightly reducing the cast piece 18 passing through the light reduction zone 19. It should be noted that Figure 1 Reference numeral 22 in the figure denotes a lower correction position arranged in the region of the lightly pressed belt 19 .
[0049] The downstream portion of the continuous casting machine 11 also forms a horizontal belt area A1 for conveying the cast piece 18 in the horizontal direction. Figure 1 In the diagram, among the zones formed by the slab support rolls 16, the zone existing in the horizontal zone region A1 is denoted by reference numeral 20a, and the zone located upstream of the horizontal zone region A1 is denoted by reference numeral 20b.
[0050] A plurality of conveying rollers 21 are provided downstream of the horizontal zone A1 for conveying the completely solidified slab 18. Above the conveying rollers 21, a slab cutter (not shown) is provided for cutting the slab 18 into a predetermined length.
[0051] In the present invention, for the interval along the casting sheet drawing direction D1 of the above-mentioned continuous casting machine 11, the interval from the starting point to the end point is determined as the first interval, the above-mentioned starting point is the starting point where the average value of the solid phase ratio along the thickness direction at the final solidification part in the width direction with the lowest solid phase ratio in the width direction of the casting sheet is less than 0.8, especially within the range of greater than 0.1 and less than 0.8, and the above-mentioned end point is the end point where the average value of the solid phase ratio along the thickness direction of the final solidification part in the width direction with the lowest solid phase ratio in the width direction of the casting sheet is greater than the average value of the solid phase ratio at the above-mentioned starting point and is less than 1.0.
[0052] Here, the solid phase ratio is an index showing the progress of solidification, and is represented in the range of 0 to 1.0. A solid phase ratio of 0 (zero) indicates no solidification, and a solid phase ratio of 1.0 indicates complete solidification.
[0053] In the present invention, the section continuous with the first section is referred to as the second section, and the second section refers to a section in which the surface temperature state (nucleate boiling state) after cooling in the first section is supplemented until the center solid fraction becomes 1.0.
[0054] In the continuous casting method of steel of the present invention, in the first section, the casting is cooled by spraying water from the water spray nozzle, and at this time, the water density per unit surface area of the casting is set to 50L / (m 2 ×min) and above 2000L / (m 2 By cooling in this way, the temperature gradient in the center of the thickness of the slab is greatly increased, which can refine the solidification structure in the center of the thickness of the slab and effectively reduce the center segregation. Here, in the first interval, the water density per unit surface area of the slab is 50L / (m 2 ×min) and above 2000L / (m 2 ×min) or less, the cast slab is cooled by cooling water, which is called "intensive cooling".
[0055] Below, use Figure 2 as well as Figure 3 The thickness direction of the width-direction final solidification portion in the slab width direction where the solid phase ratio is the lowest will be described.
[0056] Figure 2 This is a diagram when the position of the final solidified portion in the width direction where the solid phase ratio is the lowest in the width direction of the slab is defined as C1. Figure 2FIG. 1 is a top view of the cast piece 18 in a state where the upper surface and the lower surface of the cast piece 18 are supported by the cast piece support rolls 16. Figure 2 In the figure, the direction of "back ←→ front" corresponds to the slab drawing direction D1, and the direction of "right ←→ left" corresponds to the width direction D2 of the slab 18. The position C1 of the width-direction final solidification portion having the lowest solid phase ratio in the slab width direction is located near the center of the slab 18 in the width direction along the slab drawing direction D1.
[0057] Figure 3 1 is a cross-sectional view of the cast piece 18 cut along a plane perpendicular to the cast piece drawing direction D1. Figure 3 In the figure, the direction of "left ←→ right" corresponds to the width direction D2 of the casting 18, and the direction of "up ←→ down" corresponds to the thickness direction D3 of the casting 18. The position C2 in the thickness direction of the width direction final solidification part with the lowest solid phase ratio in the width direction of the casting is parallel to the thickness direction D3 at C1 in the cross section of the casting 18. Figure 3 Indicated by dotted line.
[0058] In the following description, the heat transfer coefficient for cooling the surface of the cast piece by water spray is calculated using a regression equation, and other physical properties related to steel are calculated using the physical property values corresponding to each temperature according to the data sheet. At temperatures for which there are no data, values calculated by proportional calculation using the data at temperatures before and after that temperature are used.
[0059] In the following description, the heat transfer coefficient on the surface of the cast piece using water spray is, for example, the value recorded in Publication 2 (Masashi Mitsuka, Iron and Steel, Vol. 91, 2005, pp. 685-693, The Iron and Steel Institute of Japan), Publication 3 (Toshio Teshima et al., Iron and Steel, Vol. 74, 1988, pp. 1282-1289, The Iron and Steel Institute of Japan), etc.
[0060] In the present invention, under the above premise, the cross-sectional temperature distribution of the cast piece is obtained by performing the unsteady heat transfer solidification analysis.
[0061] Furthermore, the solid fraction at a position arbitrarily selected in the thickness direction of the cross section of the cast piece can be calculated using the temperature at the arbitrarily selected position, the solidus temperature of the molten steel, and the liquidus temperature of the molten steel, and the temperature at the arbitrarily selected position is determined using the cross-sectional temperature distribution of the cast piece. In addition, when the temperature at the position is below the solidus temperature of the molten steel, the solid fraction is 1.0, and when the temperature at the position is above the liquidus temperature of the molten steel, the solid fraction is 0. In addition, when the temperature at the position is higher than the solidus temperature of the molten steel and lower than the liquidus temperature of the molten steel, the solid fraction is a value greater than 0 and less than 1.0, and is determined by the temperature at the position.
[0062] Then, based on the solid phase ratios at various positions in the slab thickness direction thus calculated, the average value of the solid phase ratios along the thickness direction is determined.
[0063] As described above, in the continuous casting method of steel according to the present invention, in the first section, the water density per unit surface area of the cast piece is set to 50 L / (m 2 ×min) and above 2000L / (m 2 Furthermore, in order to more efficiently obtain the effect of reducing segregation, it is more preferable to set the water density per unit surface area of the slab in the first interval to 300 L / (m 2 In addition, according to the inventors' knowledge, it is known that in the first interval, the water density per unit surface area of the cast piece is 2000 L / (m 2 ×min) and make it 1000L / (m 2 ×min), the temperature gradient and the number of segregated particles at the end of solidification are not significantly different. In addition, if the water density is reduced, the cost can be reduced by reducing the necessary water volume. Therefore, 1000L / (m 2 ×min) or less.
[0064] It should be noted that, regarding the cooling in the first interval, if the cast piece is cooled at the above-mentioned water density suitable for the present invention, the effect of the present invention can be obtained, but from the viewpoint of effectively obtaining the effect of the present invention by extending the distance for cooling at this water density, the difference in the average solid phase ratio between the starting point and the end point is preferably greater than 0.2, and more preferably greater than 0.4.
[0065] Next, the starting point of the first section is preferably located at either a horizontal belt that conveys the cast piece in the horizontal direction in the continuous casting machine, or a curved belt that is located upstream of the horizontal belt. For example, the first section is preferably set to be within the region A1 of the horizontal belt that conveys the cast piece in the horizontal direction in the continuous casting machine. The reason is that if strong cooling is performed in the region of the horizontal belt, the cooling can be performed uniformly to suppress the influence of thermal stress, and therefore, it is possible to make it more difficult for internal cracks of the cast piece to occur.
[0066] On the other hand, even when the starting point of the first interval is set as a bending band, the effect of the present invention can be obtained. Although there may be undesirable situations such as temperature drop that cannot be corrected or cracking due to surface stress, even when the starting point of the first interval is set to a position within the bending band, it is within the allowable range of the present invention.
[0067] Next, for cooling in the second interval, the water density per unit surface area of the cast piece is smaller than the water density per unit surface area of the cast piece in the first interval, and the flow rate is set to be able to keep the surface temperature of the cast piece below 200°C. The reason is that if the cooling is performed with the same water density as in the first interval, the equipment will become expensive. However, by doing so, the equipment investment cost can be suppressed, and the same effect as the case of strong cooling only in the first interval can be obtained. In addition, the effect of suppressing rapid heat recovery and preventing internal cracks in the cast piece caused by heat recovery can be obtained.
[0068] In addition, from the viewpoint of obtaining the above-mentioned effect, in the second section, the water density per unit surface area of the cast piece is preferably set to 50 L / (m 2 ×min) and above 300L / (m 2 The cast slab was cooled by water spray within a range of 0.5-10 min or less.
[0069] The surface temperature of the casting refers to the temperature at the center of the width of the outermost surface of the casting in the cross-sectional temperature distribution of the casting obtained by the above-mentioned unsteady heat transfer solidification analysis. It should be noted that the surface temperature in the present invention uses this calculated value, but the surface temperature of the casting can also be actually measured. In the case of actually measuring the surface temperature, for example, a radiation thermometer or a thermocouple is used to measure the temperature of the outermost surface of the casting as the surface temperature.
[0070] Furthermore, for materials with severe center segregation, it is preferred to gently reduce the long sides of the slab at a reduction rate of 0.3 to 2.0 mm / min in the first and second intervals. The reason for this is that the absorption of thickened molten steel due to solidification shrinkage can be suppressed. In the present invention, by combining strong cooling and gentle reduction, center segregation can be further reduced.
[0071] In addition, if the roll opening of multiple pairs of slab support rolls is gradually increased toward the downstream side within a range not including the correction point (starting after the upper correction and ending before the lower correction, and the opening is made flat at the correction point and is not reduced as much as possible) so that the long side of the slab is bulged with a total bulging amount of 2 to 20 mm, and then the roll opening of multiple pairs of slab support rolls is gradually reduced toward the downstream side in the casting direction and lightly pressed down to a total amount that will not be pressed down due to thermal shrinkage of the short side, it is foreseeable that the efficiency will be further improved.
[0072] Hereinafter, an experiment was conducted on the requirements for reducing the center segregation, that is, the implementation conditions for reducing the center segregation.
[0073] In this experiment, we used Figure 1The vertical bending type continuous casting machine shown is used to cast medium carbon aluminum killed steel. The length of the continuous casting machine is 49m, the thickness of the casting is 250mm, the width of the casting is 2100mm, and the secondary cooling uses air mist spray except for the first and second zones. The range of secondary cooling is from just below the mold to the outlet of the continuous casting machine. The chemical composition concentration of the medium carbon aluminum killed steel uses a substance with carbon (C) of 0.20 mass%, silicon (Si) of 0.25 mass%, manganese (Mn) of 1.1 mass%, phosphorus (P) of 0.01 mass%, and sulfur (S) of 0.002 mass%.
[0074] In addition, in this experiment, the temperature gradient near the solidification completion position and the thickness center of the casting at the end of solidification is defined as follows. In addition, the number of segregated particles, internal crack length and pores of the casting are measured as follows, and are used for the evaluation of segregation degree, internal cracks and pores, respectively. Here, "pores" refer to the closed space remaining between dendrites during solidification, and the molten steel with segregated components shrinks in volume during solidification, thereby appearing as voids in the casting.
[0075] <Solidification completion position>
[0076] The solidification completion position of the cast piece was calculated by non-steady-state heat transfer solidification analysis.
[0077] <Temperature gradient near the center of the slab thickness at the end of solidification>
[0078] The temperature gradient near the thickness center of the slab at the final stage of solidification was calculated using the above-mentioned non-steady heat transfer solidification analysis.
[0079] In this analysis, in the cross section of the slab located 1 m upstream from the position where solidification is completed along the direction D1 in which the slab is pulled out, the average temperature of the area within the range of 1 mm in the thickness direction and 10 mm in the width direction from the center position of the slab is calculated. Next, in the cross section of the slab located 1 m upstream from the position where solidification is completed along the direction D1 in which the slab is pulled out, the average temperature of the area within the range of ±1 mm in the thickness direction and 10 mm in the width direction with the position 10 mm in the thickness direction from the center position of the slab as the center is calculated. The value obtained by dividing the difference between the two average temperatures by 10 mm is taken as the temperature gradient (K / mm) near the thickness center of the slab at the end of solidification.
[0080] <Number of segregated particles>
[0081] The number of segregated particles was measured by the following method and used for evaluation of segregation.
[0082] In the cross section of the cast piece perpendicular to the casting piece drawing direction D1, a cast piece sample with a width of 15 mm and a length including a central segregation part in the center and three key points (points where the solidification shells on the short side and the long side grow and meet) from the center of the width to one side is collected. The cross section of the collected cast piece sample perpendicular to the casting piece drawing direction D1 is ground, and the surface is corroded by, for example, a saturated aqueous solution of picric acid to reveal a segregation band, and the range from the center of the segregation band to the casting piece thickness ±7.5 mm is taken as the central segregation part. After the cast piece sample of the segregation band near the center of the thickness (near the solidification completion part) is divided into small pieces in the casting piece width direction, the manganese (Mn) concentration of the cast piece sample is analyzed on the entire surface using an electron probe microanalyzer (Electron Probe Micro Analyzer: EPMA) with an electron beam diameter of 100 μm. Then, the distribution of manganese (Mn) segregation degree is obtained, and the part connected to the area with a Mn segregation degree of 1.33 or more is taken as one segregation particle. The number of segregated grains was counted, and the value obtained by dividing the number of segregated grains by the length of the sample in the width direction of the cast piece was taken as the number of segregated grains (pieces / mm). Here, the Mn segregation degree refers to the value obtained by dividing the Mn concentration of the segregated part by the Mn concentration at a position 10 mm away from the thickness center.
[0083] <Internal crack length of cast slab>
[0084] The internal crack length of the cast piece was measured by the following method for evaluation of the internal cracks.
[0085] In the cast slab after casting, the cross section of the cast slab perpendicular to the casting slab drawing direction D1 is observed, and the length of the internal crack along the thickness direction of the cast slab is measured. The maximum length of the internal crack in the observed cross section is taken as the internal crack length (mm). In the case where no internal crack can be confirmed, the internal crack length is 0.
[0086] <Pore determination>
[0087] After milling the cross section perpendicular to the casting drawing direction D1 of the fully solidified casting, after hydrochloric acid etching, a macro print was collected and the porosity was confirmed by visual sensory inspection. The case where no porosity was confirmed was judged as good (○), and the case where slight porosity that did not affect the quality of the product was confirmed was judged as acceptable (△).
[0088] The inventors conducted the following experiments to examine conditions for reducing center segregation.
[0089] [Experiment 1]
[0090] In this experiment, the temperature gradient and the number of segregated grains near the center of the thickness of the slab at the end of solidification of the slab were calculated or measured by the above-mentioned method, and the relationship between them was examined. Figure 4 A graph is shown plotting the results. Figure 4 The results shown show that if the temperature gradient (K / mm) near the center of the thickness of the cast piece at the end of solidification is increased, the number of segregated particles decreases, and there is a tendency to reduce center segregation. The temperature gradient near the center of the thickness of the cast piece at the end of solidification is 1.7 to 3.5, and more preferably 2.0 to 3.5. The reason for reducing center segregation is believed to be that by increasing the temperature gradient, the solidification structure in the center of the thickness of the cast piece can be refined.
[0091] [Experiment 2]
[0092] In this experiment, when the cast slab is subjected to secondary cooling using a continuous casting machine, the water density per unit surface area of the cast slab in the water spray is changed to produce the cast slab, and the relationship between the water density and the temperature gradient near the thickness center of the cast slab at the end of solidification is studied. In addition, the optimal range of water density is also studied in order to achieve a temperature gradient in the thickness center of the cast slab that can reduce center segregation. Figure 5 A graph plotting the results is shown.
[0093] According to the Figure 5 The results show that the water density per unit surface area of the casting is 50L / (m 2 ×min) or more, the temperature gradient in the center of the thickness of the cast slab increases significantly. That is, according to the results of Experiment 1, it can be seen that by setting the water density per unit surface area of the cast slab to 50 L / (m 2 ×min) or more, the center segregation can be greatly reduced. In addition, even if the water density per unit surface area of the cast piece is greater than 1000L / (m 2 ×min), the temperature gradient in the center of the thickness of the slab will not increase.
[0094] Therefore, although the first and second intervals are somewhat different, in order to effectively increase the temperature gradient in the center of the thickness of the cast piece, the water density per unit surface area of the cast piece is set to 2000 L / (m 2 ×min) or less, preferably 1000L / (m 2 ×min) or less. In addition, the lower limit is 50L / (m 2 ×min) or more, more preferably 300L / (m 2 ×min) or above.
[0095] [Experiment 3]
[0096] In this experiment, the effect of cooling the slab was studied. According to the insights of the inventors, the effect of cooling the slab is greatly affected by the surface temperature of the slab. It is believed that this is because the boiling state of the cooling water changes according to the surface temperature of the slab. If the surface temperature of the slab drops sufficiently, the boiling state of the surface layer becomes nucleate boiling, and stable cooling can be achieved. Therefore, when the slab is secondary cooled using a continuous casting machine, the conditions of the water density per unit surface area of the slab in the water spray are changed, and the time (temperature drop time) taken for the surface temperature of the slab to drop from 800°C to 300°C is calculated, and the effect of the water density on the temperature drop time is investigated. Figure 6 A graph plotting these results is shown.
[0097] According to the Figure 6 The results show that the water density per unit surface area of the casting is 50L / (m 2 The temperature drop time from 800°C to 300°C for the surface temperature of the cast piece is less than 200 seconds. Therefore, the water density per unit surface area of the cast piece is preferably 50 L / (m 2 In addition, the water density per unit surface area of the casting is greater than 2000L / (m 2 ×min), there is no significant change in the fall time.
[0098] Therefore, it can be seen that from the viewpoint of efficient cooling, the water density per unit surface area of the slab in the first section is preferably 2000 L / (m 2 ×min) or less.
[0099] [Experiment 4]
[0100] Next, the inventors also investigated the starting position of strong cooling that can effectively increase the temperature gradient in the center of the thickness of the cast piece. Using a continuous casting machine, the conditions of the average value of the solid phase ratio along the thickness direction of the cast piece at the beginning of strong cooling were changed to cool the cast piece, and the relationship between the average value of the solid phase ratio at the beginning of strong cooling and the temperature gradient near the thickness center of the cast piece at the end of solidification was studied. The thickness of the cast piece was 250 mm, and the water density per unit surface area of the cast piece under strong cooling was 300 L / (m 2 ×min), and the strong cooling continues until the casting is completely solidified. The relationship between the average solid phase ratio at the beginning of the strong cooling and the temperature gradient near the thickness center of the casting at the end of solidification is: Figure 7 A graph plotting the results is shown.
[0101] according to Figure 7The results shown show that there is a tendency that the smaller the average value of the solid phase ratio at the beginning of strong cooling is, the larger the temperature gradient in the center of the casting sheet is. However, there is no significant change in the temperature gradient when the average value of the solid phase ratio at the beginning of strong cooling is 0.26 and the temperature gradient when the average value of the solid phase ratio at the beginning of strong cooling is 0.43, the average value of the solid phase ratio is 0.8, and the temperature gradient in the center of the casting sheet is more than 1.7. Therefore, it can be seen that in order to give full play to the effect of the present invention, and to make the equipment of strong cooling more compact and improve the efficiency of equipment investment and operation, the average value of the solid phase ratio at the beginning of strong cooling is 0.4 or more. In addition, when the average value of the solid phase ratio at the beginning of strong cooling is greater than 0.9, the temperature gradient will not become larger.
[0102] Example
[0103] Hereinafter, examples performed to verify the effects of the present invention will be described.
[0104] use Figure 1 The vertical bending type continuous casting machine shown is used to cast medium carbon aluminum killed steel. The length of the continuous casting machine is 49m, the thickness of the casting is 250mm, the width of the casting is 2100mm, and the secondary cooling uses air mist spray except for the first and second zones. The range of secondary cooling is from just below the mold to the outlet of the continuous casting machine. The chemical composition concentration of the medium carbon aluminum killed steel uses a substance with carbon (C) of 0.20 mass%, silicon (Si) of 0.25 mass%, manganese (Mn) of 1.1 mass%, phosphorus (P) of 0.01 mass%, and sulfur (S) of 0.002 mass%.
[0105] [Example 1]
[0106] In this embodiment, the solid phase ratio at the starting point, the solid phase ratio at the end point, the water density per unit surface area of the cast piece (L / (m 2 ×min)), the outlet surface temperature of the first section (°C), the solid phase ratio at the starting point of the "second section", the solid phase ratio at the end point, the water density per unit surface area of the cast piece (L / (m 2 ×min)), the maximum surface temperature in the second interval (°C), and the conditions shown in Table 1 were given for investigation.
[0107] As for the results, the temperature gradient (K / mm) at the end of solidification, the light pressing conditions (pressing speed: 0.3-2.0 m / min), and the total amount of bulging (mm) were studied, and they are summarized in Table 1. At the same time, as an evaluation of the segregation degree, the number of segregated particles (pieces / mm) was studied, and as an evaluation of the internal cracks, the internal crack length (mm) was studied, and they are summarized in Table 1. It should be noted that in these tables, the examples that meet the conditions of the present invention are represented as invention examples, and the examples that do not meet the conditions of the present invention are represented as comparative examples. In the following table, regarding the evaluation of the segregation degree, the number of segregated particles is 1.3 pieces / mm or less, which is good and marked as "◎", more than 1.3 pieces / mm and less than 3.5 pieces / mm is acceptable and marked as "○", and more than 3.5 pieces / mm is unacceptable and evaluated with "×". Regarding the evaluation of internal cracks, an internal crack length of 1.0 mm or less was evaluated as good and marked with "◎", a crack length of more than 1.0 mm and less than 10 mm was evaluated as acceptable and marked with "○", and a crack length of more than 10 mm was evaluated as unacceptable and marked with "×".
[0108] No. 1 to 7 and No. 10 to 14 are all examples of operations performed within the scope suitable for the present invention in the conditions required for the operation in the first interval. As a result, the evaluation of the degree of segregation and the evaluation of internal cracks are both good. On the other hand, No. 8 shown as a comparative example is an example of water density deviation in the first interval, and No. 9 is an example of solid phase ratio deviation at the starting point. In No. 8 with low water density, the nucleate boiling state cannot be maintained, and the evaluation of the number of segregated particles and the evaluation of internal cracks are also poor. In addition, in No. 9 with deviated solid phase ratio, the temperature gradient in the center of the casting becomes smaller, and the evaluation of the number of segregated particles is poor.
[0109] [Table 1]
[0110]
[0111] [Example 2]
[0112] This example is about the conditions required for the treatment of the second section in the present invention (water density per unit surface area of the cast piece (L / (m 2×min)), the maximum surface temperature (℃) in the second interval was studied. That is, in this example, the conditions required in the second interval were studied on the basis of the conditions required in the first interval of [Example 1] mentioned above. The conditions and results are summarized in Table 2. Each evaluation was carried out in the same way as [Example 1]. It can be seen from Table 2 that No. 20 to 26 meet the conditions of the present invention. On the other hand, for No. 27 and 28, the water density per unit surface area of the casting required in the second interval is insufficient. Therefore, although No. 27 and 28 meet the conditions of the present invention required in the first interval, the evaluation of segregation degree and the evaluation of internal cracks are slightly worse than those of No. 20 to 26.
[0113] [Table 2]
[0114]
[0115] [Example 3]
[0116] In this embodiment, regarding the temperature gradient (K / mm) at the center of the thickness of the casting at the end of solidification, the pressing speed (m / min) as a light pressing condition, and the total amount of bulging (mm), the conditions required for the first and second intervals mentioned above were studied for examples suitable for the present invention. The conditions and results are summarized in Table 3. Each evaluation was carried out in the same way as [Example 1]. It can be seen from Table 3 that No. 30 to 37 are all suitable as examples of the invention, and the evaluation of segregation and internal cracks are generally good. However, for No. 38 and 39, due to the insufficient water density in the second interval, the temperature gradient (K / mm) near the center of the thickness of the casting at the end of solidification becomes smaller, and the maximum surface temperature in the second interval also becomes higher (>200°C). Therefore, it can be seen that No. 38 and 39 cannot obtain the same effect as No. 30 to 37.
[0117] [Table 3]
[0118]
[0119] According to the results of these examples, it is confirmed that in the present invention, the water density per unit surface area of the cast piece in at least the first interval is set within a predetermined range, and the water density per unit surface area of the cast piece in the second interval is also controlled as needed, so that the continuous casting cast piece can be effectively cooled. In addition, it is more preferably considered that the temperature gradient near the center of the cast piece thickness at the end of solidification and the soft reduction conditions in the first and second intervals are more effective.
[0120] [Example 4]
[0121] In this embodiment, the cooling condition required in the first interval is set to a stronger cooling range, and the cooling condition required in the second interval is set to 180 L / (m 2 ×min), the total bulging amount was set to a constant. In addition, the effect of the pressing speed (m / min) as a light pressing condition was studied. The conditions and results are summarized in Table 4. Figure 8 It shows the relationship between the pressing speed and the segregation degree during light pressing. Each evaluation is performed in the same manner as in [Example 1]. In addition, regarding the determination of pores, the case where no pores are confirmed is determined to be good (○), and the case where slight pores that have no effect on the quality of the product are confirmed is determined to be acceptable (△). It can be seen from Table 4 that No. 41 to 45, 48 to 52 are all suitable as examples of the invention, and the evaluation of the segregation degree and the evaluation of the pore determination are generally good. However, for No. 40 and 47, since the pressing speed as a condition for light pressing is too small, the number of segregated particles is greater than that of No. 41 to 45, 48 to 52, and slight pores are visible. On the other hand, for No. 46 and 53, since the pressing speed as a condition for light pressing is too large, the number of segregated particles is greater than that of No. 41 to 45, 48 to 52. It should be noted that no internal cracks were generated under the conditions of Table 4. According to the results, if Figure 8 As shown, by setting the cooling conditions in the first section to a stronger cooling range and setting the reduction rate as a soft reduction condition to 0.3 to 2.0 m / min, a cast slab excellent in evaluation of segregation degree and internal crack and porosity determination can be produced.
[0122] The reasons are considered to be as follows. By applying ultra-strong cooling of the cast piece in the unsolidified area, the temperature gradient increases, and the refinement of the dendrites can be achieved. In order to further improve the center segregation, it is preferred to combine light reduction. However, if the light reduction is too weak, that is, the reduction rate is too small, the flow accompanying the solidification shrinkage cannot be suppressed and positive segregation occurs. In addition, due to solidification shrinkage, pores may be generated. On the contrary, if the light reduction is too strong, that is, the reduction rate is too fast, the reduction is too much, the thickened molten steel flows back, and an inverted V segregation occurs, and the segregation worsens.
[0123] [Table 4]
[0124]
[0125] In this manual, the volume unit "L" is 10 -3 m 3 “x to y” indicating a numerical range means greater than or equal to x and less than or equal to y, including the boundary values.
[0126] Description of Reference Numerals
[0127] 11Continuous casting machine
[0128] 12 Molten Steel
[0129] 13. Casting
[0130] 14 Tundish
[0131] 15 Immersion Nozzles
[0132] 16 Casting Slab Support Roller
[0133] 17 Spray Nozzles
[0134] 18 Casting
[0135] 18a Unsolidified part in the casting
[0136] 18b Solidification completion position
[0137] 19 Gently press down the belt
[0138] 20 sectors
[0139] Segment 20a
[0140] Segment 20b
[0141] 21 conveyor roller
Claims
1. A method for continuous casting of steel, characterized in that: When the range from the starting point to the end point along the casting strip drawing direction in the continuous casting machine is defined as a first section, the water density per unit casting strip surface area in the first section is 50 to 2000 L / (m 2 × min), the starting point is a starting point where the average value of the solid phase ratio along the thickness direction at the final solidification portion in the width direction of the casting is less than 0.8, and the end point is an end point where the average value of the solid phase ratio along the thickness direction at the final solidification portion in the width direction of the casting is greater than the solid phase ratio at the starting point and is less than 1.
0.
2. The method for continuous casting of steel according to claim 1, When the second section is a section where the average solid phase ratio in the width direction at the end point is 1.0 or less and is located downstream of the first section, the water density per unit surface area of the slab in the second section is 50 to 300 L / (m 2 The casting was cooled in the range of 0.10 × min.
3. The method for continuous casting of steel according to claim 1 or 2, At least during the period from the end of the first section to the second section, casting is performed while maintaining the surface temperature of the cast piece at a nucleate boiling state below 200°C, so that the temperature gradient near the center of the cast piece thickness at the end of solidification is 1.7 to 3.5 K / mm.
4. The method for continuous casting of steel according to any one of claims 1 to 3, The first section and the second section are arranged in an area defined in a horizontal section or a vertical section in the continuous casting machine.
5. The method for continuous casting of steel according to any one of claims 1 to 4, In the first section and the second section, light reduction is applied to reduce the long sides of the cast piece at a reduction rate of 0.3 to 2.0 mm / min.
6. The method for continuous casting of steel according to any one of claims 1 to 5, By gradually increasing the roller opening of multiple pairs of slab support rollers toward the downstream side in the casting direction, the long side of the slab is bulged with a total bulging amount of 2 to 20 mm. Thereafter, the roller opening of multiple pairs of slab support rollers is gradually reduced toward the downstream side in the casting direction to lightly press down the slab.