Preparation method of nonmetal catalyst for catalyzing and depolymerizing biomass

By introducing N and S heteroatoms into catalyst preparation to construct active centers, an efficient graded porous carbon catalyst is formed, which solves the problems of non-renewable and high cost of existing catalyst resources, and realizes high conversion rate lignin depolymerization, and utilizes agriculture Helin and grassland waste reduces manufacturing costs.

CN119056478APending Publication Date: 2024-12-03GUANGXI TEACHERS EDUCATION UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411174883.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing catalysts used for the directional catalytic depolymerization of lignin have problems such as non-renewable resource, high cost and low substrate conversion, especially the large carbon emissions during the preparation and utilization of precious metals and transition metal catalysts.

Method used

A non-metallic catalyst preparation method is adopted to form a graded porous carbon catalyst by heating the biomass powder with calcium chloride and specific catalysts (such as thiourea, activated carbon, carbon nanotubes, etc.) at high temperature, and introduce N and S hybrids. Atoms build active centers to improve the active site and adsorption capacity of the catalyst.

Benefits of technology

It has achieved efficient catalytic disposal of lignin, improved the conversion rate of lignin, renewable catalyst resources, low manufacturing cost, and can effectively utilize agricultural and forestry and grassland waste, significantly improving the adsorption capacity of carbon-based catalytic materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119056478A_ABST
    Figure CN119056478A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a renewable non-metal catalyst for catalyzing and depolymerizing biomass, which is low in cost and high in lignin conversion rate, and belongs to the technical field of non-metal catalysts. The method comprises the following steps: step 1, taking biomass, washing, drying, cooling to room temperature, and crushing and grinding into biomass powder for later use; 2, adding a proper amount of biomass powder, calcium chloride and a catalyst into deionized water, and stirring to obtain a mixed precursor; 3, carrying out rotary evaporation on the mixed precursor, transferring the mixed precursor into a container after moisture is completely evaporated, and drying the mixed precursor; 4, the dried product is contained in a nickel crucible and placed in a tubular furnace, shielding gas is introduced, heating is conducted, and a non-metal catalyst crude product is obtained; and step five, after cooling the non-metal catalyst crude product, soaking the non-metal catalyst crude product in diluted hydrochloric acid, continuously stirring, then carrying out suction filtration on the mixed solution, cleaning the solid subjected to suction filtration with deionized water until the solid is neutral, and drying in vacuum to obtain the non-metal catalyst.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of non-metallic catalyst preparation, and in particular relates to a method for preparing a non-metallic catalyst for catalytic depolymerization of biomass. Background Art

[0002] With the development of economy, the demand for fossil energy is increasing day by day, but fossil energy is non-renewable and its reserves are gradually decreasing, so it is urgent to find renewable energy to replace it. Biomass energy is one of the alternative energy sources. Biomass energy belongs to renewable carbon resources and has the characteristics of large output, wide source and low pollution.

[0003] Lignin is a biological macromolecule with a three-dimensional structure formed by free radical coupling reactions of various lignin precursors. It mainly has three basic structural units, namely guaiacyl (G type), syringyl (S type) and p-hydroxyphenyl (H type). Among them, coniferous wood lignin is mainly G type, broadleaf wood lignin is mainly G type and S type, and in addition to G and S type lignin, grass plant lignin also contains H type lignin, which is a biomass resource containing benzene ring monomers. Directed catalytic depolymerization of it can obtain low molecular weight aromatic compounds, which are expected to replace fossil resources through biorefining.

[0004] At present, the catalysts for the directional catalytic depolymerization of lignin mainly focus on precious metals, transition metals, rare earth metals and their compounds, etc. These catalysts have the problems of non-renewable resources, high cost, and large carbon emissions during preparation and utilization. In order to overcome the problems of non-renewable resources, high cost, and low substrate conversion rate for preparing catalysts, the present application provides a method for catalytic depolymerization of lignin with renewable catalyst resources, low cost, and high lignin conversion rate. Summary of the invention

[0005] To achieve the above objectives, the present invention adopts the following technical solutions:

[0006] A method for preparing a non-metallic catalyst for catalytic depolymerization of biomass comprises the following steps:

[0007] Step 1: Take some biomass, wash it, dry it, cool it to room temperature, and then grind it into biomass powder for later use;

[0008] Step 2: Add appropriate amount of biomass powder, calcium chloride and catalyst into deionized water and stir to obtain a mixed precursor;

[0009] Step 3: Rotate the mixed precursor to evaporate, transfer to a container after the water is completely evaporated, and dry;

[0010] Step 4: Put the dried product into a nickel crucible and place it in a tube furnace, fill it with protective gas, and heat it to obtain a crude non-metallic catalyst product;

[0011] Step 5: After the crude non-metallic catalyst product is cooled, the crude non-metallic catalyst product is immersed in dilute hydrochloric acid and stirred continuously, and then the mixed solution is filtered, and the filtered solid is washed with deionized water until the solid is neutral, and then placed in a vacuum dry to obtain a non-metallic catalyst.

[0012] As a further improvement of the technical solution, the catalyst is any one of thiourea, activated carbon, carbon nanotubes, urea, thioacetamide, sodium sulfide, hierarchical porous carbon material, C3N4

[0013] As a further improvement of the technical solution, the catalyst is thiourea.

[0014] As a further improvement of the technical solution, the weight ratio of biomass powder: calcium chloride: catalyst is 1:2:0-2.

[0015] As a further improvement of the technical solution, the weight ratio of material powder: calcium chloride: catalyst is 1:2:2.

[0016] As a further improvement of the technical solution, in step four, the dried product is heated to 100°C-900°C.

[0017] As a further improvement of the technical solution, in step four, the dried product is heated to 800°C.

[0018] As a further improvement of the technical solution, in step four, the protective gas filled is nitrogen.

[0019] The present application also provides a non-metal catalyst for catalyzing the depolymerization of biomass, and the catalyst is prepared by the above preparation method.

[0020] The present application also provides a method for using a non-metal catalyst for catalytic depolymerization of biomass, which comprises adding lignin and the non-metal catalyst into a solvent and stirring the solvent.

[0021] As a further improvement of the technical solution, the solvent is any one of methanol, isopropanol and ethanol.

[0022] As a further improvement of the technical solution, the solvent is methanol.

[0023] As a further improvement of the technical solution, the temperature during the stirring process is 120°C-160°C, the air pressure is 0.8MPa-1.2MPa; and the pressurized gas is oxygen.

[0024] As a further improvement of the technical solution, the temperature during the stirring process is 140° C. and the air pressure is 1.0 MPa.

[0025] Compared with the prior art, the present invention has the following beneficial effects:

[0026] The non-metallic catalyst preparation method for catalytic depolymerization of biomass of the present application introduces heteroatoms such as N and S to construct the non-metallic catalyst active center during the preparation process, thereby obtaining a hierarchical porous carbon catalyst (NSHPC) that can efficiently catalyze the depolymerization of lignin, realizes the introduction of specific energy groups (N, S), increases the active sites, accurately improves the microstructure of carbon atoms, and effectively improves the adsorption capacity of carbon-based catalytic materials for lignin molecules; in the preparation process, various agricultural wastes, various forestry and grassland wastes, and various crop processing residues can be used as raw materials, the catalyst resources are renewable, and the manufacturing cost is low. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is the gas chromatography-mass spectrometry (GC-MC) of the product after lignin depolymerization;

[0028] Figure 2 NSHPC Mapping analysis diagram and EDS analysis of a non-metallic catalyst for catalytic depolymerization of biomass according to the present invention;

[0029] Figure 3 XPS spectrum analysis of the non-metallic catalyst NSHPC provided by the present invention (A. NSHPC full spectrum, BC 1s, CO 1s, DN 1s, E. S2p). DETAILED DESCRIPTION

[0030] The present invention is further described below by way of examples, but the present invention is not limited to the scope of the examples described. The experimental methods for specific adjustments not specified in the following examples are selected according to the product specifications. Based on the described embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Unless otherwise defined, the technical terms or scientific terms used herein should be the common meanings understood by people with ordinary skills in the field to which the present invention belongs.

[0031] Embodiment 1:

[0032] A method for preparing a non-metallic catalyst for catalytic depolymerization of biomass comprises the following steps:

[0033] Step 1: Take some biomass, wash it, dry it at 80°C for 12 hours, cool it to room temperature and slice it, then put it into a video grinder for crushing, take it out and continue to grind it into biomass powder, put it in a vacuum bag for standby use; the biomass can be various agricultural wastes such as shells, stalks, stems, various forestry and grass wastes such as sawdust, branches, hay, and various crop processing residues such as sugarcane bagasse, rice husks, peanut shells, etc. In this embodiment, the biomass is sugarcane bagasse;

[0034] Step 2: Add appropriate amounts of biomass powder, calcium chloride, and catalyst to deionized water and stir to obtain a mixed precursor; the catalyst is any one of thiourea, activated carbon, carbon nanotubes, urea, thioacetamide, and sodium sulfide. In this embodiment, the catalyst is thiourea; the weight ratio of biomass powder: calcium chloride: catalyst is 1:2:2; in this embodiment, the weight of bagasse is 5g, the weight of calcium chloride is 10g, the weight of catalyst is 10g, and the weight of deionized water is 100ml;

[0035] Step 3: Rotate the mixed precursor to evaporate completely, transfer it to a container, and dry it at 85°C for 12 hours;

[0036] Step 4: Put the dried product into a nickel crucible and place it in a tube furnace, fill it with protective gas, use nitrogen as the protective gas, heat it to 800° C. at a heating rate of 5° C. / min, and keep it for 2 hours to obtain a crude non-metallic catalyst product;

[0037] Step 5: After the crude non-metallic catalyst product is cooled, the crude non-metallic catalyst product is immersed in 1.0 mol / L dilute hydrochloric acid and stirred continuously for 6 hours, then the mixed solution is filtered, the filtered solid is washed with deionized water until the solid is neutral, and then dried in a vacuum at 60°C to obtain the non-metallic catalyst.

[0038] Embodiment 2:

[0039] Compared with Example 1, the difference is that the catalyst is activated carbon.

[0040] Embodiment 3:

[0041] Compared with Example 1, the difference is that the catalyst is carbon nanotubes.

[0042] Embodiment 4:

[0043] Compared with Example 1, the difference is that the catalyst is urea.

[0044] Embodiment 5:

[0045] Compared with Example 1, the difference is that the catalyst is thioacetamide.

[0046] Embodiment 6:

[0047] Compared with Example 1, the difference is that the catalyst is sodium sulfide.

[0048] Embodiment 7:

[0049] Compared with Example 1, the difference is that the catalyst is C3N4.

[0050] Embodiment 8:

[0051] Compared with Example 1, the difference is that the catalyst is a hierarchical porous carbon material HPC without adding a dopant.

[0052] Embodiment 9:

[0053] Compared with Example 1, the difference is that the catalyst is C3N5 / C (bagasse carbon source).

[0054] Embodiment 10:

[0055] Compared with Example 1, the difference is that the weight ratio of biomass powder: calcium chloride: catalyst is 1:2:0, that is, no catalyst is added.

[0056] Embodiment 11:

[0057] Compared with Example 1, the difference is that the weight ratio of biomass powder: calcium chloride: catalyst is 1:2:1.

[0058] Embodiment 12:

[0059] Compared with Example 1, the difference is that the weight ratio of biomass powder: calcium chloride: catalyst is 1:2:1.5.

[0060] Embodiment 13:

[0061] Compared with Example 1, the difference is that in step 4, the dried product is heated to 100°C.

[0062] Embodiment 14:

[0063] Compared with Example 1, the difference is that in step 4, the dried product is heated to 900°C.

[0064] Embodiment 15:

[0065] A method for using a non-metallic catalyst for catalytic depolymerization of biomass

[0066] Add an appropriate amount of lignin and a catalyst for catalytic depolymerization of biomass into the solvent, and stir at a rate of 200 r / min for 4 hours at 140° C. and an air pressure of 1.0 MPa to cause a degradation reaction, wherein the solvent is any one of methanol, isopropanol, and ethanol; in this embodiment, the solvent is methanol, the volume of the solvent is 15 ml, the weight of lignin (the type of lignin is pp-one) is 100 mg, the weight of the catalyst is 20 mg, and the pressurized gas is oxygen.

[0067] Embodiment 16:

[0068] Compared with Example 15, the difference is that the temperature during the stirring process is 120° C. and the air pressure is 0.8 MPa.

[0069] Embodiment 17:

[0070] Compared with Example 15, the difference is that the temperature during the stirring process is 160° C. and the air pressure is 1.2 MPa.

[0071] Embodiment 18:

[0072] Determination of depolymerization products of lignin using non-metallic catalysts for catalytic depolymerization of biomass

[0073] After the degradation reaction is completed, the depolymerization products are analyzed in a targeted and quantitative manner by gas chromatography-mass spectrometry. Figure 1 The following is the gas chromatography-mass spectrometry diagram of the depolymerization product. Figure 1 It can be seen that the depolymerization products are phenol, methyl benzoylformate, benzoic acid, and methyl benzoate.

[0074] Embodiment 19:

[0075] Structural analysis of the non-metallic catalyst for catalytic depolymerization of biomass prepared in Example 1

[0076] like Figure 2 As shown in the figure, in order to thoroughly explore the distribution characteristics and content of each element at the local TEM scale, a 250-nanometer-scale NSHPC area and a 100-nanometer-precision TEM area were specially selected for high-precision mapping tests and EDS component analysis. The mapping test intuitively revealed that the electron distribution of carbon (C) in NSHPC was extremely uniform, and the subsequent EDS data further confirmed that C dominated both in terms of mass percentage and atomic percentage, followed by oxygen (O), nitrogen (N) and sulfur (S). Further comparison of the mapping images of O, N, and S elements before and after loading shows that the atomic distribution of these elements is significantly non-uniform and tends to concentrate in the central area.

[0077] like Figure 3 As shown in the figure, in order to analyze the fine distribution of each element in NSHPC more deeply, we used photoelectron spectroscopy (XPS) for characterization, and used Avantage software to perform fine peak fitting and spectrum drawing on XPS data. The XPS full spectrum scan clearly shows that NSHPC has characteristic peaks of corresponding elements at specific binding energy positions (284.8eV C1s, 400.3eV O1s, 532.5eV N1s and 169.7eV S2p). Specifically for the analysis of the chemical state of the elements, Figure 3 (C) shows the detailed peak fitting results of O1s, revealing that although there is no lattice oxygen in NSHPC, adsorbed oxygen appears in the form of a characteristic peak of binding energy of 532.5 eV. Figure 3 (D) conducted an in-depth analysis of N1s and subdivided it into four forms: pyridinic nitrogen (398.4eV), pyrrolic nitrogen (400.0eV), graphitic nitrogen (401.2eV) and oxidized nitrogen (403.0eV). Among them, the atomic ratio of pyridinic nitrogen and pyrrolic nitrogen is much higher than that of graphitic nitrogen and oxidized nitrogen, indicating that these two nitrogen forms dominate in NSHPC. They significantly enhance the adsorption affinity of NSHPC to the target substrate by donating electrons to the π-conjugated system of the graphitic carbon layer. Finally, Figure 3 (E) presents the complex peak fitting spectrum of S2p. Due to the spin-orbit coupling effect, the S2p energy level is split into 2p3 / 2 and 2p1 / 2 doublets, forming paired spin split peaks. The analytical results show that the S element mainly exists in the form of thiophene sulfur (CSC, 2p3 / 2 of about 164eV and 2p1 / 2 of 165eV) and sulfonic acid sulfur (C-SOx-C, x=2~4, 2p3 / 2 of about 169eV and 2p1 / 2 of 170eV), and sulfonic acid sulfur is the main binding state, and the atomic percentage of its 2p3 / 2 state is about twice that of the 2p1 / 2 state.

[0078] Embodiment 20:

[0079] According to the usage scheme of Example 15, the non-metallic catalysts for catalytic depolymerization of biomass prepared in Examples 1 to 9 were used to depolymerize lignin respectively, and blank group 1 was added as a control, that is, no non-metallic catalyst was added during the depolymerization of lignin, and the rest was depolymerized according to normal steps, and the yield of the depolymerization product and the overall conversion rate were calculated.

[0080] The quantitative analysis of the model molecular compound was performed by the LC-100 liquid chromatograph equipped by Wufeng Company. The liquid chromatograph was equipped with a UV xenon lamp detector, a 5μm C18 (250X4.6mm) chromatographic column, a column box temperature of 35°C, a mobile phase of acetonitrile: water = 6:4, and a flow rate of 1.0ml / min. The results are shown in Table 1.

[0081] The specific calculation formulas for product yield (%) and conversion rate (%) are as follows:

[0082] Conversion rate = (the amount of substrate substance remaining after the reaction / the amount of substrate substance before the reaction) x 100%.

[0083] Product yield = (molar amount of product / total molar amount of substrate) × 100%.

[0084] Table 1 Comparison of the performance of different carbon-based catalysts in catalytic depolymerization of lignin

[0085]

[0086] As can be seen from Table 1, without adding any catalyst (row 1), the conversion rate of the substrate is only 13.2%, which indicates that under these conditions, the stability of the substrate is relatively high.

[0087] When activated carbon and carbon nanotube materials (rows 2-3) were used as catalysts, the conversion rate was slightly improved, reaching 31.9% and 36.2%, respectively. This shows that these materials have a certain catalytic effect on the reaction, but it is not significant. When the commonly used nitrogen-carbon doped material C3N4 (row 4) and C3N5 prepared using sugarcane bagasse as a carbon source (row 5) were used as catalysts, the conversion rate was significantly improved, reaching 46.0% and 26.0%, respectively. These results are similar to those of commonly used carbon materials, indicating that these homemade catalysts have good catalytic performance.

[0088] When considering hierarchical porous carbon materials as catalysts, the conversion rate of the hierarchical porous carbon material HPC (row 6) without adding dopants is improved to a certain extent, reaching 33.1%.

[0089] When single-element doped hierarchical porous carbon materials are used, the conversion rate of hierarchical porous carbon doped with urea as the N source (row 7) is significantly increased to 85.3%, indicating that the doping of N element has a significant effect on the catalytic performance of hierarchical porous carbon.

[0090] When thioacetamide and sodium sulfide were used as the S source to dope the graded porous carbon (rows 8 and 9), the conversion rate continued to increase slightly, reaching 64.5% and 67.1%, respectively.

[0091] When N and S co-doped carbon materials are used as catalysts, the conversion rate is significantly improved. When thiourea is used as a dopant to jointly provide N and S sources (row 10), the depolymerization efficiency reaches 98.7%, nearly 100%, and is improved compared to the graded porous carbon doped with single N and S elements (rows 7-9). This indicates that the N and S elements have a synergistic effect in jointly improving the substrate conversion rate of the system. This may be because the S element further optimizes the active sites and reaction pathways of the catalyst.

[0092] In summary, the co-doping of N and S elements has a significant effect on improving the catalytic performance of graded porous carbon materials; the non-metallic catalyst preparation method for catalytic depolymerization of biomass of the present application introduces heteroatoms such as N and S to construct non-metallic catalyst active centers during the preparation process, thereby obtaining a graded porous carbon catalyst (NSHPC) that can efficiently catalyze the depolymerization of lignin, realizes the introduction of specific energy groups (N, S), increases active sites, accurately improves the microstructure of carbon atoms, and effectively improves the adsorption capacity of carbon-based catalytic materials for lignin molecules; various agricultural wastes, various forestry and grassland wastes, and various crop processing residues can be used as raw materials in the preparation process, the catalyst resources are renewable, and the manufacturing cost is low.

[0093] Embodiment 21:

[0094] According to the usage scheme of Example 15, the non-metallic catalysts for catalytic depolymerization of biomass prepared in Examples 1 to 9 were used to depolymerize lignin respectively, and a blank group 2 was added as a control, that is, no non-metallic catalyst was added during the depolymerization of lignin, and the rest was depolymerized according to normal steps, and the yield of the depolymerization product and the overall conversion rate were calculated.

[0095] The quantitative analysis of the model molecular compound was performed by the LC-100 liquid chromatograph equipped by Wufeng Company. The liquid chromatograph was equipped with a UV xenon lamp detector, a 5μm C18 (250X4.6mm) chromatographic column, a column box temperature of 35°C, a mobile phase of acetonitrile: water = 6:4, and a flow rate of 1.0ml / min. The results are shown in Table 2.

[0096] The specific calculation formulas for product yield (%) and conversion rate (%) are as follows:

[0097] Conversion rate = (the amount of substrate substance remaining after the reaction / the amount of substrate substance before the reaction) x 100%.

[0098] Product yield = (molar amount of product / total molar amount of substrate) × 100%.

[0099] Table 2 Comparison of the results of depolymerization of lignin by catalysts at different weight ratios

[0100]

[0101] It can be seen from Table 2 that under the same reaction conditions, the N and S doped hierarchical porous carbon materials prepared with different thiourea doping amounts as catalysts have a certain correlation with the conversion rate. When the weight ratio of biomass powder: calcium chloride: thiourea is 1:2:0, the conversion rate of lignin is 40.88%, which is 26.27% higher than that of blank group 2. As the weight ratio of biomass powder: calcium chloride: thiourea continues to increase, the conversion rate of lignin also gradually increases. When the weight ratio of biomass powder: calcium chloride: thiourea is 1:2:2, the conversion rate of lignin also reaches the highest value, as high as 98.7%. It can be seen that when the thiourea doping amount is 1:2:2, the prepared non-metallic catalyst has a high conversion rate for the depolymerization process of the system.

[0102] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the present invention.

Claims

1. A method for preparing a non-metallic catalyst for catalytic depolymerization of biomass, characterized in that: The following steps are involved: Step 1: Take some biomass, wash it, dry it, cool it to room temperature, and then grind it into biomass powder for later use; Step 2: Add appropriate amount of biomass powder, calcium chloride and catalyst into deionized water and stir to obtain a mixed precursor; Step 3: Rotate the mixed precursor to evaporate, transfer to a container after the water is completely evaporated, and dry; Step 4: Put the dried product into a nickel crucible and place it in a tube furnace, fill it with protective gas, and heat it to obtain a crude non-metallic catalyst product; Step 5: After the crude non-metallic catalyst product is cooled, the crude non-metallic catalyst product is immersed in dilute hydrochloric acid and stirred continuously, and then the mixed solution is filtered, and the filtered solid is washed with deionized water until the solid is neutral, and then placed in a vacuum dry to obtain a non-metallic catalyst.

2. The method for preparing a non-metallic catalyst for catalytic depolymerization of biomass according to claim 1, characterized in that: The catalyst is any one of thiourea, activated carbon, carbon nanotubes, urea, thioacetamide, sodium sulfide, hierarchical porous carbon material, and C3N4.

3. The method for preparing a non-metallic catalyst for catalytic depolymerization of biomass according to claim 2, characterized in that: The catalyst is thiourea.

4. The method for preparing a non-metallic catalyst for catalytic depolymerization of biomass according to claim 1, characterized in that: The weight ratio of biomass powder: calcium chloride: catalyst is 1:2:0-2.

5. The method for preparing a non-metallic catalyst for catalytic depolymerization of biomass according to claim 4, characterized in that: The weight ratio of biomass powder: calcium chloride: catalyst is 1:2:

2.

6. The method for preparing a non-metallic catalyst for catalytic depolymerization of biomass according to claim 1, characterized in that: In step 4, the dried product is heated to 100°C-900°C.

7. A non-metal catalyst for catalytic depolymerization of biomass, prepared by the method for preparing a non-metal catalyst for catalytic depolymerization of biomass according to any one of claims 1 to 6.

8. The method for using a non-metallic catalyst for catalytic depolymerization of biomass according to claim 7, characterized in that: Lignin and the non-metal catalyst according to claim 9 are added to a solvent and stirred.

9. The method for using the non-metallic catalyst for catalytic depolymerization of biomass according to claim 8, characterized in that: The temperature during the stirring process is 120°C-160°C, and the air pressure is 0.8MPa-1.2MPa.

10. The method for using the non-metallic catalyst for catalytic depolymerization of biomass according to claim 9, characterized in that: The temperature during stirring was 140°C and the air pressure was 1.0 MPa.