Preparation and application of modified chitin nanocrystal loaded gold nanoparticle composite material
Aldehyde-functionalized chitin nanocrystals are used to load gold nanoparticles in-situ, addressing the stability and dispersibility issues of traditional methods, enabling environmentally friendly and stable gold nanoparticle composites for catalysis, water treatment, and antibacterial applications.
Patent Information
- Application Number
- CN202411163400.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-12-03
AI Technical Summary
Existing methods for loading gold nanoparticles using chitin nanocrystals require additional reducing agents, leading to poor loading stability and low dispersibility, which are not environmentally friendly.
A method involving aldehyde-functionalized chitin nanocrystals as templates and dispersants, utilizing the aldehyde groups to in-situ reduce gold nanoparticles without additional reducing agents, resulting in a composite material with good stability and high dispersibility.
The process is green and sustainable, producing gold nanoparticles with small particle size and high stability, suitable for applications in catalysis, water treatment, pharmaceuticals, and antibacterial uses.
Smart Images

Figure CN119056490A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a preparation method and application of a nanocomposite material, and in particular to a preparation method and application of an aldehyde-functionalized chitosan nanocrystal-loaded gold nanoparticle composite material. Background Art
[0002] Chitosan is the highest nitrogen-containing resource in the ocean and the second most abundant polysaccharide on Earth after cellulose. Chitosan nanocrystals have the advantages of low density, high specific surface area and good biocompatibility. In particular, they contain numerous functional groups such as hydroxyl, acetylamino and amino groups on the surface, which are easy to functionalize. At the same time, the unique needle-like morphology has a high mechanical modulus and mechanical strength. Therefore, chitosan nanocrystals can be used in many fields, such as the preparation of polymer composite materials, cosmetics production, food additives, food packaging, water treatment, drug delivery and tissue engineering.
[0003] Gold nanoparticles (AuNPs) have large specific surface area, high surface energy and high catalytic activity. They also have unique biocompatibility, small size effect, quantum size effect, surface effect and quantum tunneling effect. Due to their unique properties, gold nanoparticles are widely used in many fields, such as industrial catalysis, biomedicine, bioanalytical chemistry and rapid detection. In order to prevent the aggregation of AuNPs, high molecular polymers or inorganic mesoporous materials are needed as the substrate of AuNPs, as templates and stabilizers to control the monodispersity and stability of AuNPs in solution.
[0004] At present, some studies have used graphene, hydrogel and silica microspheres as carriers to load gold nanoparticles. However, most of the existing loading methods have the defects of poor loading stability and low dispersibility, and usually require the additional addition of reducing agents to reduce metal ions, which runs counter to green environmental protection.
[0005] Based on this, the researchers of this application considered combining chitin nanocrystals with gold nanoparticles, thereby using chitin nanocrystals as carriers to load gold nanoparticles. However, the original chitin nanocrystals, when used, are no different from traditional carriers, and still have defects such as the need to add additional reducing agents. Therefore, how to modify chitin and apply it to in-situ reduction and load gold nanoparticles, thereby avoiding the technical defects of traditional carriers, is the main work of the present invention. Summary of the invention
[0006] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a preparation method and application of a composite material of modified chitosan nanocrystal loaded with gold nanoparticles. The modified chitosan nanocrystal of the present invention is an aldehyde-modified chitosan nanocrystal, the preparation method thereof is simple, the compound structure is controllable, and it is green and sustainable; more importantly, the present invention uses the aldehyde-modified chitosan nanocrystal as a template agent, and also as a dispersant and uses the aldehyde group on its surface as a reducing agent to in-situ reduce and load the gold nanoparticles, and the whole process does not require the addition of an additional reducing agent, is green and environmentally friendly, and the gold nanoparticle loading has good stability and high dispersibility.
[0007] One of the technical solutions of the present invention:
[0008] Provided is a method for preparing a composite material of modified chitin nanocrystals loaded with gold nanoparticles. Aldehyde functionalized chitin nanocrystals are used as templates, dispersants and reducing agents. After reacting with gold ions, uniformly dispersed gold nanoparticles are prepared and loaded, thereby obtaining the composite material of modified chitin nanocrystals loaded with gold nanoparticles.
[0009] Preferably, the preparation of the aforementioned modified chitin nanocrystal-loaded gold nanoparticle composite material is carried out by the following specific method: first, ultrasonically suspending the aldehyde-functionalized chitin nanocrystals in water, then adding NaAuCl4 or HAuCl4 solution, stirring for 3-12 hours, adjusting the pH to 7-13 with sodium hydroxide solution or ammonia water, and then reacting for another 3-12 hours, centrifuging to obtain a crude product, washing with water several times, and freeze-drying to obtain a modified chitin nanocrystal-loaded gold nanoparticle composite material.
[0010] Preferably, in the preparation of the aforementioned modified chitin nanocrystal-loaded gold nanoparticle composite material, in the reaction system, the mass concentration of the aldehyde-functionalized chitin nanocrystals is 0.1-50 g / L, and the concentration of NaAuCl4 or HAuCl4 is 0.1-10 mmol / L.
[0011] Preferably, in the preparation of the aforementioned modified chitin nanocrystal-loaded gold nanoparticle composite material, the particle size of the gold nanoparticles is 0.1-100 nm.
[0012] Preferably, in the preparation of the aforementioned modified chitosan nanocrystal-loaded gold nanoparticle composite material, the preparation method of the aldehyde-functionalized chitosan nanocrystal is as follows:
[0013] (1) anchoring an initiator α-bromoisobutyryl bromide on the surface of chitin nanocrystals through an esterification reaction to obtain bromine-containing chitin nanocrystals;
[0014] (2) using lignin-based aromatic aldehyde as raw material and methacryloyl chloride or acryloyl chloride to construct a lignin-based aromatic aldehyde monomer containing a double bond through an acylation reaction;
[0015] (3) Brominated chitosan nanocrystals and lignin-based aromatic aldehyde monomers containing double bonds are mixed, and polymers are grown on the brominated chitosan nanocrystals by SI-ARGETATRP to obtain aldehyde-functionalized chitosan nanocrystals.
[0016] Preferably, in the preparation of the aforementioned modified chitin nanocrystal-loaded gold nanoparticle composite material, the method of step (1) is specifically as follows:
[0017] Under ice bath ultrasonic conditions, chitosan nanocrystals are dispersed in an organic solvent to form a dispersed chitosan nanocrystal suspension, and then 4-dimethylaminopyridine and triethylamine are added under stirring, and then an organic solvent mixture of α-bromoisobutyryl bromide is added; then the mixture is reacted at 25-70° C. for 3-24 hours under stirring conditions; the resulting suspension is centrifuged to obtain a crude product, and the crude product is repeatedly washed in acetone, dichloromethane, anhydrous ethanol and water in sequence, and then dispersed in water, and freeze-dried to obtain bromine-containing chitosan nanocrystals; wherein the mass concentration of chitosan nanocrystals in the chitosan nanocrystal suspension is 1-50 g / L, and the reaction molar ratio of chitosan nanocrystals to α-bromoisobutyryl bromide is 1:5-1:20; the reaction molar ratio of 4-dimethylaminopyridine to α-bromoisobutyryl bromide is 1:1-5:1; and the reaction molar ratio of triethylamine to α-bromoisobutyryl bromide is 1:1-5:1.
[0018] Preferably, in the preparation of the aforementioned modified chitin nanocrystal-loaded gold nanoparticle composite material, the method of step (2) is specifically as follows:
[0019] Lignin-based aromatic aldehyde is used as a raw material, dissolved in an organic solvent, an acid-binding agent pyridine is added, and a mixed organic solvent solution of methacryloyl chloride or acryloyl chloride is added under an ice bath, and the mixture is refluxed for 1-5 hours; after the reaction is completed, insoluble matter is filtered out, dichloromethane is removed by rotary evaporation, ethyl acetate is added, and then a saturated NaCl aqueous solution, a saturated NaHCO3 aqueous solution and deionized water are used for washing 3-5 times in sequence; anhydrous sodium sulfate is used to dry the organic layer for 10-15 hours, sodium sulfate is finally filtered out, and ethyl acetate is removed by rotary evaporation to obtain an oily, light yellow liquid crude product; finally, the crude product is recrystallized through an ethanol-water system, and dried to obtain a lignin-based aromatic aldehyde monomer containing a double bond; wherein the lignin-based aromatic aldehyde is vanillin, syringaldehyde or p-hydroxybenzaldehyde; the reaction molar ratio of pyridine to the lignin-based aromatic aldehyde is 1:1-5:1; the reaction molar ratio of methacryloyl chloride to the lignin-based aromatic aldehyde is 1:1-5:1.
[0020] Preferably, in the preparation of the aforementioned modified chitin nanocrystal-loaded gold nanoparticle composite material, the method of step (3) is specifically as follows:
[0021] The brominated chitosan nanocrystals prepared in step (1) are ultrasonically dispersed in an organic solvent, and then added to the organic solvent mixed solution of the lignin-based aromatic aldehyde monomer prepared in step (2), and then the catalyst copper bromide, the ligand N,N,N',N',N'-pentamethyldiethylenetriamine, the sacrificial initiator ethyl 2-bromoisobutyrate and the reducing agent ascorbic acid are added in sequence, and stirred for 1-10 minutes; and then subjected to three freezing-vacuuming-nitrogen filling cycles, the reaction is carried out in an oil bath at 30-80° C. for 3-24 hours to perform surface SI-ARGET ATRP polymerization, nitrogen protection during the reaction process, repeated washing with acetone, ethanol and deionized water after the reaction, freeze-drying to obtain aldehyde-functionalized chitin nanocrystals; wherein, in the reaction system, the mass concentration of brominated chitin nanocrystals is 0.05-5g / L, and the mass molar ratio of brominated chitin nanocrystals, lignin-based aromatic aldehyde monomers, catalysts, ligands, sacrificial initiators and reducing agents is 300mg:30-200mmol:0.05-0.2mmol:0.5-2mmol:0.5-2mmol:0.5-2mmol.
[0022] The second technical solution of the present invention:
[0023] Provided is a modified chitin nanocrystal-loaded gold nanoparticle composite material, which is prepared by the above method.
[0024] The third technical solution of the present invention:
[0025] Provided is an application of the modified chitin nanocrystal-loaded gold nanoparticle composite material in the fields of catalysis, water treatment, pharmaceuticals and antibacterial.
[0026] Beneficial effects of the present invention:
[0027] 1. The preparation method of the aldehyde-modified chitosan nanocrystals of the present invention is simple, the compound structure is controllable, and it is green and sustainable.
[0028] 2. The present invention utilizes aldehyde-modified chitosan nanocrystals as carriers and dispersants, and utilizes the reducing property of the aldehyde groups on its surface to in-situ reduce gold ions to obtain a composite material of modified chitosan nanocrystals loaded with gold nanoparticles. The entire synthesis process is green and environmentally friendly, and no additional reducing agent is required, which is in line with the development trend of green chemistry.
[0029] 3. The gold nanoparticles of the aldehyde-functionalized chitosan nanocrystal-loaded gold nanoparticle composite material prepared by the present invention have small particle size, good dispersibility, and high stability, and can be widely promoted and applied in the fields of catalysis, water treatment, pharmaceuticals and antibacterial. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 The figure is a flow chart of the process steps of the present invention.
[0031] Figure 2 The infrared spectrum of the modified chitin nanocrystal-loaded gold nanoparticle composite material (Au@ChNCs-PVMA) and other intermediate products of the present invention. -1 The new C=O stretching vibration appeared at 1760 cm -1 、1701cm -1 and 1500cm -1 The characteristic peaks of ester group, aldehyde group and benzene ring in PVMA chain appeared at the 400 nm position, which confirmed the successful preparation of ChNCs-PVMA. From the changes in the infrared spectra of ChNCs-PVMA and Au@ChNCs-PVMA before and after the reaction, it can be found that, with amide I as the reference, after the reduction reaction, the absorption peak intensity of aldehyde group weakened, while other peaks remained basically unchanged, which proved that aldehyde group reacted during the reaction and Au 3+ Reduced to AuNPs by aldehyde groups.
[0032] Figure 3 The XRD spectra of the modified chitin nanocrystal-loaded gold nanoparticle composite material and other intermediate products of the present invention. With the modification of the surface of chitin nanocrystal ChNCs, the crystallinity gradually decreases, because the surface grafting modification of ChNCs will reduce the crystallinity of ChNCs. From the modified chitin nanocrystal-loaded gold nanoparticle composite material Au@ChNCs-PVMA, it can be seen that there are sharp diffraction peaks at 2θ=38.2°, 44.4°, 64.7° and 77.8°, which correspond to the (111), (200), (220) and (311) lattice planes of face-centered cubic (FCC) AuNPs, respectively. This shows that AuNPs are successfully loaded and the aldehyde-functionalized chitin nanocrystal ChNCs-PVMA structure maintains its original structure.
[0033] Figure 4 The TEM spectrum of the modified chitin nanocrystal-loaded gold nanoparticle composite material of the present invention shows that the AuNPs anchored by ChNCs-PVMA are evenly dispersed, almost without aggregation, and the average particle size distribution is about 5 nm.
[0034] Figure 5The figure is a time-dependent UV-visible spectrum of hydrogenation of 4-nitrophenol (4-NP) catalyzed by the modified chitin nanocrystal-supported gold nanoparticle composite material of the present invention. The UV-visible absorption peak at 400nm in the figure is the characteristic peak of 4-NP. As the reaction time increases, the absorption peak gradually weakens, and a new characteristic absorption peak belonging to the product 4-aminophenol (4-AP) appears at 300nm. Under the catalysis of the Au@ChNCs-PVMA catalyst containing 0.6μmol AuNPs, the catalytic hydrogenation reaction of 4-NP only takes 12min, indicating that the Au@ChNCs-PVMA catalyst has excellent catalytic activity.
[0035] Figure 6 The figure is a time-dependent UV-visible spectrum of hydrogenation of azo dyes catalyzed by the modified chitin nanocrystal-supported gold nanoparticle composite material of the present invention. Under the condition of 0.4 μmol AuNPs Au@ChNCs-PVMA catalyst, the characteristic absorption peaks of methyl orange (MO, 465 nm), Congo red (CR, 486 nm) and chrome black T (EBT, 552 nm) gradually decrease with the reaction time, and a new characteristic absorption peak appears at 250 nm, indicating the formation of aromatic amines, further illustrating the successful degradation of azo dyes. The complete degradation times are 280 s, 350 s and 420 s, respectively, indicating that the catalyst Au@ChNCs-PVMA has a good catalytic effect in catalyzing the degradation of azo dyes.
[0036] Figure 7 The figure is the time-dependent UV-visible spectrum of the modified chitin nanocrystal-supported gold nanoparticle composite material catalyzing the hydrogenation of non-azo dyes. After adding 0.6 μmol AuNPs to the Au@ChNCs-PVMA catalyst, it takes 4 min, 7 min and 30 min to degrade methylene blue, rhodamine B and phenol red, respectively, indicating that Au@ChNCs-PVMA can also show good catalytic activity in catalyzing the degradation of non-azo dyes. DETAILED DESCRIPTION
[0037] The present invention will be further described below in conjunction with the embodiments, but they are not intended to limit the present invention.
[0038] Embodiments of the present invention
[0039] Unless otherwise specified, the experimental methods used in the following examples are conventional methods.
[0040] Unless otherwise specified, the reagents and materials used in the following examples can be obtained from commercial sources.
[0041] Embodiment 1 of the present invention:
[0042] Step 1: Preparation of aldehyde-functionalized chitin nanocrystals
[0043] Step 1-1: ChNCs (2.50 g) were added to a glass bottle containing 250 mL of DMF (N, N-dimethylaminoformamide) and stirred for 2 h to ensure that DMF first effectively penetrated and diffused, and then ultrasonicated for 2 h under ice bath protection; DMAP (4-dimethylaminopyridine) (15.35 g, 123.40 mmol) and TEA (triethylamine) (25.90 mL, 185.00 mmol) were added thereto under stirring, and then magnetic stirring was continued for about The mixture was stirred for 10 minutes, and then BiBB (α-bromoisobutyryl bromide, 15.55 mL, 123.30 mmol) dissolved in 50 mL DMF was added dropwise. The whole process was protected in an ice bath. After the addition was completed, the mixture was placed in a 70 °C oil bath for reaction for 24 hours. After the reaction was completed, the mixture was centrifuged at 8000 rpm for 15 minutes, and repeatedly washed with acetone, dichloromethane, anhydrous ethanol and water until the supernatant was colorless, and then dispersed in water and freeze-dried to obtain brominated chitin nanocrystals (ChNCs-Br).
[0044] Step 1-2: Weigh vanillin (30.40 g, 200.00 mmol) and place it in a 1000 mL three-necked flask, add 500 mL of dichloromethane solvent, and dissolve it by stirring with a magnetic bar until it is clear, continue to add the acid binding agent pyridine (24.23 mL, 300.00 mmol) and stir for 10 min, then use a constant pressure dropping funnel to dropwise add methacryloyl chloride (29.00 mL, 200.00 mmol) dissolved in 50 mL of dichloromethane under ice bath conditions, after the addition is complete, heat to 38 ° C and reflux for 3 h; after the reaction is completed The insoluble matter was removed by filtration, and then the dichloromethane was removed by rotary evaporation, 500 mL of ethyl acetate was added, and then washed with saturated NaCl aqueous solution, saturated NaHCO3 aqueous solution and deionized water for 4 times in sequence; the organic layer was dried with anhydrous sodium sulfate for 12 hours; the sodium sulfate was removed by filtration, and the solvent ethyl acetate was removed to obtain an oily, light yellow liquid; the crude product was dissolved in 300 mL of ethanol, the ethanol-insoluble solids were removed by filtration, and recrystallization was performed twice through an ethanol-water system. After drying, a lignin-based aromatic aldehyde monomer (methacrylic acid vanillin ester) containing a double bond was finally obtained.
[0045] Step 1-3: 300 mg of brominated chitin nanocrystals (ChNCs-Br) were ultrasonically dispersed in 30 mL of DMF, and then vanillin methacrylate (9.8 g, 44.5 mmol) dissolved in 30 mL of DMF was added dropwise, followed by the catalyst copper bromide (CuBr2) (20.1 mg, 0.089 mmol), the ligand N,N,N',N',N'-pentamethyldiethylenetriamine (PMDETA) (188 μL, 0.89 mmol), the sacrificial initiator 2-bromoisobutylene Ethyl bicarbonate (EBiB) (133 μL, 0.89 mmol) and reducing agent ascorbic acid (AsAc) (0.16 mg, 0.89 mmol) were added and stirred for 5 min; after three cycles of (freezing-vacuuming-nitrogen filling), the mixture was transferred to a 60 °C oil bath for reaction for 3 h; the reaction was protected by nitrogen. After the reaction, the mixture was repeatedly centrifuged and washed with acetone, ethanol and deionized water for two days to ensure that the free self-polymers and components involved in the ATRP initiation procedure were completely removed. After washing, the mixture was freeze-dried to obtain aldehyde-functionalized chitin nanocrystals ChNCs-PVMA.
[0046] Step 2: Add 150 mg of aldehyde-functionalized chitin nanocrystals (ChNCs-PVMA) to 40 ml of water, then add 10 ml of NaAuCl4 aqueous solution (3 mmol / L), stir for 12 hours, adjust the pH to 11 with 0.1 mol / L NaOH solution under ice bath conditions, and then react at room temperature for 12 hours. After the reaction is completed, wash with water and centrifuge three times, and finally freeze-dry to obtain aldehyde-functionalized chitin nanocrystals loaded with gold nanoparticles composite materials (Au@ChNCs-PVMA).
[0047] Embodiment 2 of the present invention:
[0048] In step 2 of Example 1, the concentration of the NaAuCl4 aqueous solution was adjusted to 6 mmol / L, and other conditions remained unchanged.
[0049] Embodiment 3 of the present invention:
[0050] In step 2 of Example 1, the concentration of the NaAuCl4 aqueous solution was adjusted to 9 mmol / L, and other conditions remained unchanged.
[0051] Embodiment 4 of the present invention:
[0052] The modified chitin nanocrystal-loaded gold nanoparticle composite material of the present invention is used to catalyze the reduction reaction of 4-nitrophenol to prepare 4-aminophenol. The experimental steps are as follows:
[0053] 1) Prepare a 0.5 mM 4-nitrophenol aqueous solution;
[0054] 2) preparing a 0.1 M sodium borohydride aqueous solution;
[0055] 3) Take 25 ml of sodium borohydride aqueous solution and 5 ml of 4-nitrophenol solution in a beaker, add the catalyst ChNCs-PVMA@AuNPs containing 0.6 μmol AuNPs, react at room temperature, and monitor the reaction process using a UV-visible spectrophotometer.
[0056] Embodiment 5 of the present invention:
[0057] The modified chitin nanocrystal-loaded gold nanoparticle composite material of the present invention is used to catalyze the hydrogenation of azo dyes. The experimental steps are as follows:
[0058] 5 mL of azo dyes (MO (0.5 mM), CR (1.5 mM) and EBT (0.5 mM)) and 25 mL of fresh NaBH4 solution (0.1 M) were mixed. Then, the catalyst ChNCs-PVMA@AuNPs containing 0.4 μmol AuNPs was added to start the catalytic reaction. The UV-visible spectrum recorded the changes of the mixture over time to track the progress of the reaction.
[0059] Embodiment 6 of the present invention:
[0060] The modified chitin nanocrystal-loaded gold nanoparticle composite material of the present invention is used to catalyze the hydrogenation of non-azo dyes. The experimental steps are as follows:
[0061] 5 mL of non-azo dyes (methylene blue (0.3 mM), rhodamine B (0.5 mM), and phenol red (0.3 mM)) and 25 mL of fresh NaBH4 solution (0.1 M) were mixed. Then, the catalyst ChNCs-PVMA@AuNPs containing 0.6 μmol AuNPs was added to start the catalytic reaction. UV-visible spectroscopy was used to record the changes of the mixture over time to track the progress of the reaction.
[0062] Embodiment 7 of the present invention:
[0063] The preparation method of the modified chitosan nanocrystal-loaded gold nanoparticle composite material is as follows: first, ultrasonically suspend the aldehyde-functionalized chitosan nanocrystals in water, then add NaAuCl4 solution, stir for 3 hours, adjust the pH to 7 with sodium hydroxide solution, and then react for 12 hours, centrifuge to obtain a crude product, wash it with water for 3 times, and freeze-dry it to obtain the modified chitosan nanocrystal-loaded gold nanoparticle composite material; in the reaction system, the mass concentration of the aldehyde-functionalized chitosan nanocrystals is 0.1 g / L, and the NaAuCl4 concentration is 0.1 mmol / L.
[0064] Embodiment 8 of the present invention:
[0065] The preparation method of the modified chitin nanocrystal-loaded gold nanoparticle composite material is as follows: first, ultrasonically suspend the aldehyde-functionalized chitin nanocrystals in water, then add HAuCl4 solution, stir for 12 hours, adjust the pH to 13 with ammonia water, and then react for 3 hours, centrifuge to obtain a crude product, wash it with water 5 times, and freeze-dry it to obtain the modified chitin nanocrystal-loaded gold nanoparticle composite material; in the reaction system, the mass concentration of the aldehyde-functionalized chitin nanocrystals is 50 g / L, and the concentration of HAuCl4 is 10 mmol / L.
[0066] Embodiment 9 of the present invention:
[0067] Under ice bath ultrasonic conditions, chitosan nanocrystals are dispersed in an organic solvent to form a dispersed chitosan nanocrystal suspension, and then 4-dimethylaminopyridine and triethylamine are added under stirring, and then an organic solvent mixture of α-bromoisobutyryl bromide is added; then the mixture is reacted at 25° C. for 24 hours under stirring conditions; the resulting suspension is centrifuged to obtain a crude product, and the crude product is repeatedly washed in acetone, dichloromethane, anhydrous ethanol and water in sequence, and then dispersed in water, and freeze-dried to obtain brominated chitosan nanocrystals; wherein the mass concentration of chitosan nanocrystals in the chitosan nanocrystal suspension is 1 g / L, and the reaction molar ratio of chitosan nanocrystals to α-bromoisobutyryl bromide is 1:5; the reaction molar ratio of 4-dimethylaminopyridine to α-bromoisobutyryl bromide is 1:1; and the reaction molar ratio of triethylamine to α-bromoisobutyryl bromide is 1:1.
[0068] Lignin-based aromatic aldehyde is used as a raw material, dissolved in an organic solvent, an acid-binding agent pyridine is added, and an organic solvent mixed solution of acryloyl chloride is added under an ice bath, and the mixture is refluxed for 1 hour; after the reaction is completed, insoluble matter is filtered out, dichloromethane is removed by rotary evaporation, ethyl acetate is added, and then a saturated NaCl aqueous solution, a saturated NaHCO3 aqueous solution and deionized water are used to wash the mixture three times in sequence; the organic layer is then dried with anhydrous sodium sulfate for 10 hours, sodium sulfate is finally filtered out, and ethyl acetate is removed by rotary evaporation to obtain an oily, light yellow liquid crude product; the crude product is finally recrystallized through an ethanol-water system, and dried to obtain a lignin-based aromatic aldehyde monomer containing a double bond; wherein the lignin-based aromatic aldehyde is vanillin; the reaction molar ratio of pyridine to the lignin-based aromatic aldehyde is 1:1; the reaction molar ratio of acryloyl chloride to the lignin-based aromatic aldehyde is 1:1.
[0069] The brominated chitosan nanocrystals prepared in step (1) are ultrasonically dispersed in an organic solvent, and then added to the organic solvent mixed solution of the lignin-based aromatic aldehyde monomer prepared in step (2), and then the catalyst copper bromide, the ligand N,N,N',N',N'-pentamethyldiethylenetriamine, the sacrificial initiator ethyl 2-bromoisobutyrate and the reducing agent ascorbic acid are added in sequence, and stirred for 1 minute; and then subjected to three freezing-vacuuming-nitrogen filling cycles, the reaction is carried out in a 30° C. oil bath for 24 hours to perform surface SI-ARGET ATRP polymerization, nitrogen protection during the reaction process, repeated washing with acetone, ethanol and deionized water after the reaction, and freeze-drying to obtain aldehyde-functionalized chitin nanocrystals; wherein, in the reaction system, the mass concentration of brominated chitin nanocrystals is 0.05 g / L, and the mass molar ratio of brominated chitin nanocrystals, lignin-based aromatic aldehyde monomers, catalysts, ligands, sacrificial initiators and reducing agents is 300 mg: 30 mmol: 0.05 mmol: 0.5 mmol: 0.5 mmol: 0.5 mmol.
[0070] Embodiment 10 of the present invention:
[0071] Under ice bath ultrasonic conditions, chitosan nanocrystals are dispersed in an organic solvent to form a dispersed chitosan nanocrystal suspension, and then 4-dimethylaminopyridine and triethylamine are added under stirring, and then an organic solvent mixture of α-bromoisobutyryl bromide is added; then the mixture is reacted at 70° C. for 3 hours under stirring conditions; the resulting suspension is centrifuged to obtain a crude product, and the crude product is repeatedly washed in acetone, dichloromethane, anhydrous ethanol and water in sequence, and then dispersed in water, and freeze-dried to obtain brominated chitosan nanocrystals; wherein the mass concentration of chitosan nanocrystals in the chitosan nanocrystal suspension is 50 g / L, and the reaction molar ratio of chitosan nanocrystals to α-bromoisobutyryl bromide is 1:20; the reaction molar ratio of 4-dimethylaminopyridine to α-bromoisobutyryl bromide is 5:1; and the reaction molar ratio of triethylamine to α-bromoisobutyryl bromide is 5:1.
[0072] Lignin-based aromatic aldehyde is used as a raw material, dissolved in an organic solvent, an acid-binding agent pyridine is added, and an organic solvent mixed solution of methacryloyl chloride is added under an ice bath, and the mixture is refluxed for 5 hours; after the reaction is completed, the insoluble matter is filtered out, dichloromethane is removed by rotary evaporation, ethyl acetate is added, and then a saturated NaCl aqueous solution, a saturated NaHCO3 aqueous solution and deionized water are used to wash the mixture 5 times in sequence; the organic layer is then dried with anhydrous sodium sulfate for 15 hours, the sodium sulfate is finally filtered out, and the ethyl acetate is removed by rotary evaporation to obtain an oily, light yellow liquid crude product; the crude product is finally recrystallized through an ethanol-water system, and dried to obtain a lignin-based aromatic aldehyde monomer containing a double bond; wherein the lignin-based aromatic aldehyde is p-hydroxybenzaldehyde; the reaction molar ratio of pyridine to the lignin-based aromatic aldehyde is 5:1; the reaction molar ratio of methacryloyl chloride to the lignin-based aromatic aldehyde is 5:1.
[0073] The bromine-containing chitosan nanocrystals prepared in step (1) are ultrasonically dispersed in an organic solvent, and then added to the organic solvent mixed solution of the lignin-based aromatic aldehyde monomer prepared in step (2), and then the catalyst copper bromide, the ligand N,N,N',N',N'-pentamethyldiethylenetriamine, the sacrificial initiator 2-ethyl bromoisobutyrate and the reducing agent ascorbic acid are added in sequence, and stirred for 1-10 minutes; and then subjected to three freezing-vacuuming-nitrogen filling cycles, reacted in an 80° C. oil bath for 3 hours to perform surface SI-ARGET ATRP polymerization, with nitrogen protection during the reaction process, and after the reaction is completed, repeatedly washed with acetone, ethanol and deionized water, and freeze-dried to obtain aldehyde-functionalized chitosan nanocrystals; wherein, in the reaction system, the mass concentration of the bromine-containing chitosan nanocrystals is 5 g / L, and the mass molar ratio of the bromine-containing chitosan nanocrystals, the lignin-based aromatic aldehyde monomer, the catalyst, the ligand, the sacrificial initiator and the reducing agent is 300 mg: 200 mmol: 0.2 mmol: 2 mmol: 2 mmol: 2 mmol.
[0074] The above is only a preferred specific implementation of the invention, but the protection scope of the invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical solutions and inventive concepts of the invention within the technical scope disclosed by the invention, which should be included in the protection scope of the invention.
Claims
1. Preparation of a composite material of modified chitin nanocrystals loaded with gold nanoparticles, Features: The method uses aldehyde-functionalized chitin nanocrystals as templates, dispersants and reducing agents, and after reacting with gold ions, prepares and loads uniformly dispersed gold nanoparticles, thereby obtaining a modified chitin nanocrystal-loaded gold nanoparticle composite material.
2. The preparation of the modified chitin nanocrystal-loaded gold nanoparticle composite material according to claim 1, It is characterized in that The specific method is: firstly, aldehyde functionalized chitin nanocrystals are ultrasonically suspended in water, and then NaAuCl is added. 4 or HAuCl 4 The solution is stirred for 3-12 hours, and the pH is adjusted to 7-13 with sodium hydroxide solution or ammonia water. Then, after reacting for another 3-12 hours, the crude product is obtained by centrifugation, washed with water several times, and freeze-dried to obtain a modified chitin nanocrystal-loaded gold nanoparticle composite material.
3. The preparation of the modified chitin nanocrystal-loaded gold nanoparticle composite material according to claim 2, Features: In the reaction system, the mass concentration of aldehyde functionalized chitin nanocrystals is 0.1-50 g / L, NaAuCl 4 or HAuCl 4 The concentration is 0.1-10mmol / L.
4. The preparation of the modified chitin nanocrystal-loaded gold nanoparticle composite material according to claim 1 or 2, Features: The particle size of the gold nanoparticles is 0.1-100 nm.
5. The preparation of the modified chitin nanocrystal-loaded gold nanoparticle composite material according to claim 1, It is characterized in that The preparation method of the aldehyde functionalized chitin nanocrystals is as follows: (1) anchoring an initiator α-bromoisobutyryl bromide on the surface of chitin nanocrystals through an esterification reaction to obtain bromine-containing chitin nanocrystals; (2) using lignin-based aromatic aldehyde as raw material and methacryloyl chloride or acryloyl chloride to construct a lignin-based aromatic aldehyde monomer containing a double bond through an acylation reaction; (3) Brominated chitosan nanocrystals and lignin-based aromatic aldehyde monomers containing double bonds are mixed, and polymers are grown on the brominated chitosan nanocrystals by SI-ARGET ATRP to obtain aldehyde-functionalized chitosan nanocrystals.
6. The preparation of the modified chitin nanocrystal-loaded gold nanoparticle composite material according to claim 5, It is characterized in that The method of step (1) is specifically as follows: Under ice bath ultrasonic conditions, chitosan nanocrystals are dispersed in an organic solvent to form a dispersed chitosan nanocrystal suspension, and then 4-dimethylaminopyridine and triethylamine are added under stirring, and then an organic solvent mixture of α-bromoisobutyryl bromide is added; then the mixture is reacted at 25-70° C. for 3-24 hours under stirring conditions; the resulting suspension is centrifuged to obtain a crude product, and the crude product is repeatedly washed in acetone, dichloromethane, anhydrous ethanol and water in sequence, and then dispersed in water, and freeze-dried to obtain bromine-containing chitosan nanocrystals; wherein the mass concentration of chitosan nanocrystals in the chitosan nanocrystal suspension is 1-50 g / L, and the reaction molar ratio of chitosan nanocrystals to α-bromoisobutyryl bromide is 1:5-1:20; the reaction molar ratio of 4-dimethylaminopyridine to α-bromoisobutyryl bromide is 1:1-5:1; and the reaction molar ratio of triethylamine to α-bromoisobutyryl bromide is 1:1-5:
1.
7. The preparation of the modified chitin nanocrystal-loaded gold nanoparticle composite material according to claim 5, It is characterized in that The method of step (2) is specifically as follows: Take lignin-based aromatic aldehyde as raw material, dissolve it in an organic solvent, add acid-binding agent pyridine, add methacryloyl chloride or acryloyl chloride mixed organic solvent solution under ice bath, and reflux reaction for 1-5h; after the reaction, filter to remove insoluble matter, remove dichloromethane by rotary evaporation, add ethyl acetate, and then use saturated NaCl aqueous solution, saturated NaHCO 3 The aqueous solution and deionized water are washed 3-5 times respectively; the organic layer is dried with anhydrous sodium sulfate for 10-15 hours, the sodium sulfate is filtered out, and the ethyl acetate is removed by rotary evaporation to obtain an oily, light yellow liquid crude product; the crude product is recrystallized through an ethanol-water system, and dried to obtain a lignin-based aromatic aldehyde monomer containing a double bond; wherein the lignin-based aromatic aldehyde is vanillin, syringaldehyde or p-hydroxybenzaldehyde; the reaction molar ratio of pyridine to lignin-based aromatic aldehyde is 1:1-5:1; the reaction molar ratio of methacryloyl chloride to lignin-based aromatic aldehyde is 1:1-5:
1.
8. The preparation of the modified chitin nanocrystal-loaded gold nanoparticle composite material according to claim 5, It is characterized in that The method of step (3) is specifically as follows: The brominated chitosan nanocrystals prepared in step (1) are ultrasonically dispersed in an organic solvent, and then added to the organic solvent mixed solution of the lignin-based aromatic aldehyde monomer prepared in step (2), and then the catalyst copper bromide, the ligand N,N,N',N',N'-pentamethyldiethylenetriamine, the sacrificial initiator ethyl 2-bromoisobutyrate and the reducing agent ascorbic acid are added in sequence, and stirred for 1-10 minutes; and then subjected to three freezing-vacuuming-nitrogen filling cycles, reacted in an oil bath at 30-80° C. for 3-24 hours to perform surface SI-ARGETATRP polymerization, The reaction process is protected by nitrogen. After the reaction is completed, the mixture is repeatedly washed with acetone, ethanol and deionized water, and freeze-dried to obtain aldehyde-functionalized chitin nanocrystals. In the reaction system, the mass concentration of brominated chitin nanocrystals is 0.05-5 g / L, and the mass molar ratio of brominated chitin nanocrystals, lignin-based aromatic aldehyde monomers, catalysts, ligands, sacrificial initiators and reducing agents is 300 mg: 30-200 mmol: 0.05-0.2 mmol: 0.5-2 mmol: 0.5-2 mmol: 0.5-2 mmol.
9. A modified chitin nanocrystal-loaded gold nanoparticle composite material, Features: It is prepared by the method according to any one of claims 1 to 8.
10. Use of the modified chitin nanocrystal-loaded gold nanoparticle composite material according to claim 9 in the fields of catalysis, water treatment, pharmaceuticals and antibacterial.