Polyimide material CMP method for hybrid bonding and semiconductor wafer

By using the hybrid bonding CMP method of polyimide materials on semiconductor integrated circuits, the removal rate and thickness of the polyimide layer are controlled, and the problems of surface roughness and bonding interface quality are solved, and better bonding is achieved Strength and device stability improve chip performance.

CN119057651APending Publication Date: 2024-12-03BEIJING SEMICORE MICROELECTRONICS EQUIPMENT CO LTD

Patent Information

Application Number
CN202411237530.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-04
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The surface roughness and bonding interface quality of existing semiconductor integrated circuits lead to unreliable bonding and gap problems. The CMP process parameters and consumables are complex and difficult to effectively control.

Method used

Using a hybrid bonding CMP method of polyimide material, the removal rate and thickness of the polyimide layer are controlled on the first and second polishing discs, using a hard polishing pad and Al2O3 abrasive, combined with white light endpoint detection and motor Current end point detection achieves surface roughness <0.5nm and lower material height difference <5nm.

Benefits of technology

The bonding interface state and bonding strength are improved, making the device more stable and reliable, improving the chip's data transmission speed and reducing power consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119057651A_ABST
    Figure CN119057651A_ABST
Patent Text Reader

Abstract

The invention is applicable to the technical field of semiconductor material processing, and provides a polyimide material CMP (chemical mechanical polishing) method for hybrid bonding and a semiconductor wafer, and the method comprises the following steps: removing PI (polyimide) of a wafer on a first polishing disk, and controlling the residual thickness of a PI layer to be within # imgabs0 #; wherein the rate of removing the PI layer on the first polishing disc is # imgabs 1 #, and the remaining PI layer is removed on the second polishing disc until a lower layer material of the PI layer is exposed; wherein the rate of removing the remaining PI layer on the second polishing disk is that # imgabs2 # two polishing disks select a hard polishing pad and a polishing solution of an Al2O3 abrasive material, and the particle diameter of the Al2O3 abrasive material is 100-150 nm. According to the invention, a better bonding interface state can be obtained, the bonding strength is higher, the device is more stable and reliable, and the surface roughness of the wafer is less than 0.5 nm.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of semiconductor material processing, and in particular, relates to a polyimide material CMP method for hybrid bonding and a semiconductor wafer. Background Art

[0002] The technology iteration of semiconductor integrated circuits has been developing along Moore's Law until now, and has almost reached the physical limit. In order to further improve the performance of integrated circuits, on the one hand, new technologies such as Fin FET (Fin Field-Effect Transistor) and GAA (Gate-All-Around) for plane size miniaturization are being explored, and on the other hand, integrated circuit chips or systems are being stacked in three-dimensional space.

[0003] Before the introduction of the Chemical Mechanical Polishing (CMP) process, high-temperature heating reflux and dry / wet etching were used to obtain a relatively flat surface. However, due to the height difference and poor surface quality caused by the underlying structure, problems such as gaps or loose bonding would occur during bonding.

[0004] The CMP process is a complex dynamic process, which is closely related to many factors such as the consumables used and their physical and chemical properties, such as the combination of polishing pads and polishing liquids, the distribution of polishing liquids on polishing pads, process parameter settings such as pressure, the rotation speed of the grinding head and grinding disc, and the flow rate of polishing liquid. Different consumable combinations and different process parameters will produce completely different grinding results. How to influence the wafer-level bonding results and indicators through the combination of consumables and the setting of process parameters is a key issue. Summary of the invention

[0005] In order to overcome the problems existing in the related art, the embodiments of the present application provide a polyimide material CMP method and a semiconductor wafer for hybrid bonding, which can obtain a better bonding interface state, greater bonding strength, more stable and reliable devices, and make the surface roughness of the wafer <0.5nm.

[0006] This application is implemented through the following technical solutions:

[0007] In a first aspect, an embodiment of the present application provides a polyimide material CMP method for hybrid bonding, comprising:

[0008] The polyimide layer of the wafer is removed on the first polishing plate, and the remaining thickness of the polyimide layer is controlled within a preset thickness range; wherein the rate of removing the polyimide layer on the first polishing plate is The preset thickness range is

[0009] The remaining polyimide layer is removed on the second polishing disc until the underlying material of the polyimide layer is exposed; wherein the rate of removing the remaining polyimide layer on the second polishing disc is The first polishing disc and the second polishing disc use a hard polishing pad and a polishing liquid of Al2O3 abrasive, and the particle diameter of the Al2O3 abrasive is 100-150nm.

[0010] In one embodiment, the flow rate of the polishing liquid is 250-300 ml / min.

[0011] In one embodiment, the first polishing plate corresponds to a first polishing head; the second polishing plate corresponds to a second polishing head;

[0012] The pressure of the first polishing head and the second polishing head are both 3-5Psi, the rotation speed is both 75-90r / min, and the swing amplitude is both 6mm.

[0013] In one embodiment, the first polishing disc and the second polishing disc are both diamond polishing discs; the pressure of the first polishing disc and the second polishing disc is 5-6 lbf, and the rotation speed is 75-90 r / min.

[0014] In one embodiment, controlling the remaining thickness of the polyimide layer to be within a preset thickness range includes:

[0015] White light endpoint detection is used to control the remaining thickness of the polyimide layer to be within a preset thickness range.

[0016] In one embodiment, the wavelength of white light used in white light endpoint detection is 400-900 nm.

[0017] In one embodiment, removing the remaining polyimide layer on the second polishing pad until the underlying material of the polyimide layer is exposed comprises:

[0018] The remaining polyimide layer is removed on the second polishing disc, and the removal thickness of the remaining polyimide layer is controlled by using the motor current endpoint detection until the lower layer material of the polyimide layer is exposed.

[0019] In one embodiment, the thickness of the polyimide layer is 1-3 um.

[0020] In one embodiment, the lower layer material of the polyimide layer is Cu, oxide or SiN.

[0021] In a second aspect, an embodiment of the present application provides a semiconductor wafer obtained by applying the polyimide material CMP method for hybrid bonding as in the first aspect.

[0022] Compared with the related art, the embodiments of the present application have the following beneficial effects:

[0023] The embodiments of the present application achieve a lower surface roughness of <0.5nm and a smaller height difference between PI and the underlying material of <5nm through the combination of consumables and the setting of process parameters, so as to obtain a better bonding interface state, a greater bonding strength, and a more stable and reliable device.

[0024] The beneficial effects of the second aspect mentioned above refer to the beneficial effects of the CMP method for hybrid bonding of polyimide materials in the first aspect, which will not be described in detail here.

[0025] It is to be understood that the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the present specification. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the embodiments or related technical descriptions will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0027] Figure 1 This is a schematic diagram of a wafer surface obtained by heating and reflowing a PI material provided in an embodiment of the present application and then etching it;

[0028] Figure 2 It is a schematic flow chart of a CMP method for a polyimide material for hybrid bonding provided in one embodiment of the present application;

[0029] Figure 3 is a schematic cross-sectional view of a wafer before polishing provided in an embodiment of the present application;

[0030] Figure 4 is a schematic cross-sectional view of a wafer polished on a first polishing disk according to an embodiment of the present application;

[0031] Figure 5 is a schematic cross-sectional view of a wafer polished on a second polishing plate provided in an embodiment of the present application;

[0032] Figure 6 is the surface roughness of different material layers provided in an embodiment of the present application;

[0033] Figure 7 This is a schematic diagram of two protruding wafers before bonding provided by an embodiment of the present application;

[0034] Figure 8 This is a schematic diagram of two concave wafers before bonding provided in an embodiment of the present application. DETAILED DESCRIPTION

[0035] In the following description, specific details such as specific system structures and technologies are provided for the purpose of illustration rather than limitation, so as to provide a thorough understanding of the embodiments of the present application. However, it should be clear to those skilled in the art that the present application may also be implemented in other embodiments without these specific details. In other cases, detailed descriptions of well-known systems, devices, circuits, and semiconductor wafers are omitted to prevent unnecessary details from obstructing the description of the present application.

[0036] It should be understood that when used in the present specification and the appended claims, the term "comprising" indicates the presence of described features, wholes, steps, operations, elements and / or components, but does not exclude the presence or addition of one or more other features, wholes, steps, operations, elements, components and / or combinations thereof.

[0037] It should also be understood that the term “and / or” used in the specification and appended claims refers to any and all possible combinations of one or more of the associated listed items, and includes these combinations.

[0038] In addition, in the description of the present application specification and the appended claims, the terms "first", "second", "third", etc. are only used to distinguish the descriptions and cannot be understood as indicating or implying relative importance.

[0039] References to "one embodiment" or "some embodiments" etc. described in the specification of this application mean that one or more embodiments of the present application include specific features, structures or characteristics described in conjunction with the embodiment. Therefore, the statements "in one embodiment", "in some embodiments", "in some other embodiments", "in some other embodiments", etc. that appear in different places in this specification do not necessarily refer to the same embodiment, but mean "one or more but not all embodiments", unless otherwise specifically emphasized in other ways. The terms "including", "comprising", "having" and their variations all mean "including but not limited to", unless otherwise specifically emphasized in other ways.

[0040] In order to enable those skilled in the art to better understand the scheme of the present invention, the technical scheme in the embodiments of the present application will be clearly and completely described below in conjunction with the accompanying drawings and specific implementation methods. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0041] If polyimide (PI) material is heated and reflowed and then etched, a relatively flat wafer surface can be obtained, but the PI thickness has problems such as uneven thickness and uneven surface heights. Figure 1 shown.

[0042] This application uses PI material as a CMP planarization process for hybrid bonding surfaces in chip stacking technology. The CMP planarization process allows the wafer surface to obtain a surface state suitable for hybrid bonding, which is a very important aspect that affects the wafer bonding results and device reliability.

[0043] The present invention selects specific polishing liquid, polishing pad and other consumables, controls the removal rate of PI material and the entire polishing process to perform process control, and ultimately achieves a higher polishing rate, better surface quality, and higher hybrid bond synthesis success rate and reliability.

[0044] Figure 2 1 is a schematic flow chart of a CMP method for a polyimide material for hybrid bonding provided in one embodiment of the present application. Figure 3 is a schematic diagram of the wafer cross section before polishing. Figure 4 is a schematic diagram of the cross section of a wafer polished on the first polishing plate. Figure 5 is a schematic diagram of the cross section of the wafer polished on the second polishing plate; refer to Figures 2 to 5 The details of the CMP method of the polyimide material for hybrid bonding are as follows:

[0045] Step 101, removing the polyimide layer of the wafer on a first polishing plate, and controlling the remaining thickness of the polyimide layer to be within a preset thickness range; wherein the rate of removing the polyimide layer on the first polishing plate is The preset thickness range is

[0046] Exemplarily, a thicker PI layer is removed in large quantities on the first polishing pad, such as Figure 3 to Figure 4 shown.

[0047] Step 102, removing the remaining polyimide layer on the second polishing disc until the underlying material of the polyimide layer is exposed; wherein the rate of removing the remaining polyimide layer on the second polishing disc is The first polishing disc and the second polishing disc use a hard polishing pad and a polishing liquid of Al2O3 abrasive, and the particle diameter of the Al2O3 abrasive is 100-150nm.

[0048] The lower layer material of the polyimide layer is generally Cu. The lower layer here refers to the polyimide layer that is actually partially located between the Cu materials compared to the unpolished polyimide layer.

[0049] Exemplarily, a small amount of the remaining PI layer is removed on the second polishing plate, such as Figure 4 to Figure 5 As shown, the thickness of the PI layer removed on the second polishing disk is less than the thickness of the PI layer removed on the first polishing disk, thereby achieving the purpose of removing a large amount first and then a small amount.

[0050] This embodiment controls the height difference and surface roughness of different materials by controlling the rate and uniformity of the removed material PI, achieving the ideal surface state for wafer-level bonding. The surface roughness <0.5nm is achieved. Figure 6 As shown in the figure, the average roughness Ra and root mean square roughness Rq of the PI layer and the Cu layer are both less than 0.5nm. At the same time, a smaller height difference between the PI and the underlying material is achieved, which is less than 5nm, to obtain a better bonding interface state, a greater bonding strength, and a more stable and reliable device.

[0051] In one embodiment, the flow rate of the polishing liquid is 250-300 ml / min.

[0052] In one embodiment, the first polishing disc corresponds to a first polishing head; the second polishing disc corresponds to a second polishing head; the pressure of the first polishing head and the second polishing head are both 3-5Psi, the rotation speed is both 75-90r / min; the swing amplitude is both 6mm.

[0053] In one embodiment, the first polishing disc and the second polishing disc are both diamond polishing discs; the pressure of the first polishing disc and the second polishing disc is 5-6 lbf (pound force), and the rotation speed is 75-90 r / min.

[0054] In one embodiment, controlling the remaining thickness of the polyimide layer to be within a preset thickness range includes:

[0055] White light endpoint detection is used to control the remaining thickness of the polyimide layer to be within a preset thickness range.

[0056] Among them, white light assists in controlling the thickness of the PI layer based on the different reflectivities of different materials. Generally, metals have high reflectivity, while non-metallic reflectivity is much lower. When approaching the polishing endpoint, the surface material of the wafer will change, and the reflectivity will change. This control method is real-time and can adjust the time and other parameters of the polishing process according to the actual thickness of the PI layer. The wavelength of white light used in white light endpoint detection is 400-900nm.

[0057] Exemplarily, removing the remaining polyimide layer on the second polishing pad until the underlying material of the polyimide layer is exposed includes:

[0058] The remaining polyimide layer is removed on the second polishing disc, and the removal thickness of the remaining polyimide layer is controlled by using the motor current endpoint detection until the lower layer material of the polyimide layer is exposed.

[0059] Among them, the machine of motor current endpoint detection will give the second polishing plate a current to make it rotate, and generally CMP will set a fixed speed. To maintain this speed, the machine must continue to give the second polishing plate a fixed current; when the wafer contacts the surface of the polishing pad, the friction force will cause the machine to increase the current to keep the polishing plate at this fixed speed; however, when approaching the polishing end point EPD, the change of the material being polished on the wafer will cause the change of friction, and the current supplied by the machine will also change at this time; the method of using this current value change as the CMP polishing end point detection EPD capture is called motor current endpoint detection.

[0060] The above-mentioned use of white light endpoint detection and motor current endpoint detection to assist in controlling the total polishing time to control the remaining thickness of the polyimide layer can uniformly control the height difference between the PI layer on the wafer surface and the underlying material to be less than 5nm. The height difference between the PI layer and the underlying material has two forms: concave and convex.

[0061] If Figure 1 When bonding the wafers obtained by etching, due to the uneven height difference of different materials, gaps will occur during bonding or the bonding will be unreliable. In addition, if the interface roughness is between 1nm and 2nm, the depression will be large, which cannot meet the requirements of subsequent bonding and the bonding success rate is low. Figure 7 and Figure 8 As shown, the height difference between the PI layer on the wafer surface and the underlying material is uniformly controlled so that the height difference between materials of different qualities is uniform. Combined with the above-mentioned better roughness, an ideal surface state for wafer-level bonding is achieved.

[0062] In one embodiment, the thickness of the polyimide layer is 1-3 um.

[0063] In one embodiment, the lower layer material of the polyimide layer is Cu, oxide or SiN.

[0064] The polyimide material CMP method for hybrid bonding proposed in the present invention achieves a lower surface roughness of <0.5nm and a smaller height difference between PI and the underlying material of <5nm through the matching of consumables and the setting of process parameters, so as to obtain a better bonding interface state, a greater bonding strength, a more stable and reliable device, and a faster data transmission speed and lower power consumption of the prepared chip.

[0065] An embodiment of the present application provides a semiconductor wafer obtained by using the polyimide material CMP method for hybrid bonding as in the above embodiment.

[0066] It should be understood that the execution order of the above processes should be determined by their functions and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present application.

[0067] It should be noted that the information interaction, execution process and other contents between the above-mentioned devices are based on the same concept as the method embodiment of the present application. Their specific functions and technical effects can be found in the method embodiment part and will not be repeated here.

[0068] The technicians in the relevant field can clearly understand that for the convenience and simplicity of description, only the division of the above-mentioned functional units and modules is used as an example for illustration. In practical applications, the above-mentioned function allocation can be completed by different functional units and modules as needed, that is, the internal structure of the device can be divided into different functional units or modules to complete all or part of the functions described above. The functional units and modules in the embodiment can be integrated in a processing unit, or each unit can exist physically separately, or two or more units can be integrated in one unit. The above-mentioned integrated unit can be implemented in the form of hardware or in the form of software functional units. In addition, the specific names of the functional units and modules are only for the convenience of distinguishing each other, and are not used to limit the scope of protection of this application. The specific working process of the units and modules in the above-mentioned system can refer to the corresponding process in the aforementioned method embodiment, which will not be repeated here.

[0069] The above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. These modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present application, and should all be included in the protection scope of the present application.

Claims

1. A CMP method for polyimide materials for hybrid bonding, characterized in that: include: The polyimide layer of the wafer is removed on a first polishing disk, and the remaining thickness of the polyimide layer is controlled to be within a preset thickness range; wherein the rate of removing the polyimide layer on the first polishing disk is The preset thickness range is The remaining polyimide layer is removed on the second polishing disc until the underlying material of the polyimide layer is exposed; wherein the rate of removing the remaining polyimide layer on the second polishing disc is The first polishing disc and the second polishing disc use a hard polishing pad and a polishing liquid containing Al2O3 abrasives, and the particle diameter of the Al2O3 abrasives is 100-150nm.

2. The polyimide material CMP method for hybrid bonding according to claim 1, characterized in that: The flow rate of the polishing liquid is 250-300 ml / min.

3. The polyimide material CMP method for hybrid bonding according to claim 1, characterized in that: The first polishing disc corresponds to a first polishing head; the second polishing disc corresponds to a second polishing head; The pressure of the first polishing head and the second polishing head are both 3-5Psi, the rotation speed is both 75-90r / min, and the swing amplitude is both 6mm.

4. The polyimide material CMP method for hybrid bonding according to claim 1, characterized in that: The first polishing disc and the second polishing disc are both diamond polishing discs; the pressure of the first polishing disc and the second polishing disc is 5-6 lbf, and the rotation speed is 75-90 r / min.

5. The polyimide material CMP method for hybrid bonding according to claim 1, characterized in that: The controlling the remaining thickness of the polyimide layer to be within a preset thickness range comprises: White light endpoint detection is used to control the remaining thickness of the polyimide layer to be within a preset thickness range.

6. The polyimide material CMP method for hybrid bonding according to claim 5, characterized in that: The wavelength of white light used in the white light endpoint detection is 400-900 nm.

7. The polyimide material CMP method for hybrid bonding according to claim 1, characterized in that: The step of removing the remaining polyimide layer on the second polishing pad until the underlying material of the polyimide layer is exposed comprises: The remaining polyimide layer is removed on the second polishing disc, and the removal thickness of the remaining polyimide layer is controlled by using motor current endpoint detection until the lower layer material of the polyimide layer is exposed.

8. The polyimide material CMP method for hybrid bonding according to claim 7, characterized in that: The thickness of the polyimide layer is 1-3 um.

9. A CMP method for polyimide materials for hybrid bonding, characterized in that: The lower layer material of the polyimide layer is Cu, oxide or SiN.

10. A semiconductor wafer, characterized in that: The method is obtained by using the CMP method of the polyimide material for hybrid bonding as claimed in any one of claims 1 to 9.

Citation Information

Patent Citations

  • Blended bonding achieving method

    CN103474366A

  • Polyimide layer removal method and manufacturing method of semiconductor device

    CN108321085A

  • Wafer level mixed bonding method

    CN109671619A

  • Wafer acquisition method and failure analysis method of semiconductor device

    CN111883453A

  • Polishing solution, polishing solution set, polishing method, and defect suppressing method

    CN113661563A

Cited By

  • Chemical mechanical polishing solution for removing polyimide film

    CN120842993A

  • Final polishing method for wafer, and polished wafer

    WO2026138261A1