Alternating projection optimization method based on ceramic digital light processing technology

The alternating projection optimization method addresses warping deformation in ceramic digital light processing by dividing the projection pattern into outer and inner layers, optimizing printing parameters, and ensuring full shell exposure, thereby improving accuracy and efficiency.

CN119057889APending Publication Date: 2024-12-03TECH & ENG CENT FOR SPACE UTILIZATION CHINESE ACAD OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411445905.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-16
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Existing ceramic digital light processing technologies face challenges in reducing warping deformation and dimensional deviations due to photocuring shrinkage, which are exacerbated by the presence of ceramic powder and require additional materials and processes that increase viscosity and complexity.

Method used

An alternating projection optimization method that involves slicing the model, setting template parameters, and performing morphological and logical operations to divide the projection pattern into outer and inner patterns, ensuring full exposure of the shell and discrete exposure of the inner pattern, with optimized printing parameters to reduce shrinkage stress.

Benefits of technology

Effectively reduces warping deformation, improves part molding accuracy, maintains versatility across different printers, and enhances manufacturing efficiency without additional materials or process steps.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119057889A_ABST
    Figure CN119057889A_ABST
Patent Text Reader

Abstract

The invention discloses an alternative projection optimization method based on a ceramic digital light processing technology, and the method comprises the following steps: carrying out the slicing of a printing model, and obtaining an initial projection pattern; obtaining a template substrate of each layer by setting a function and setting template parameters; obtaining a shell through morphological operation and logical operation, and determining an outer wall and an internal pattern of each layer according to the shell; performing logical operation on the internal pattern of each layer and the template substrate corresponding to each layer to obtain an optimized internal pattern; combining the optimized internal pattern of each layer with the outer wall pattern to obtain an optimized projection pattern; appropriate printing parameters are set according to a printing material, a ceramic printing blank is obtained through layer-by-layer manufacturing, and a ceramic sintering part is obtained through post-treatment steps such as degreasing and sintering. According to the method, the buckling deformation of the printed blank in the ceramic digital light treatment process can be effectively reduced, and the control over the part forming precision is improved; extra materials are not required to be introduced, the steps of burdening and post-treatment are reduced, and the manufacturing efficiency is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of ceramic materials, and in particular to an alternating projection optimization method based on ceramic digital light processing technology. Background Art

[0002] Photocuring technology is a method of manufacturing layer by layer by irradiating photosensitive materials with ultraviolet light. Among them, digital light processing technology is a manufacturing technology based on the principle of photocuring that is widely used in the field of ceramic 3D printing. It is essentially a surface exposure system based on mask projection. Among them, ultraviolet light is transmitted to the printing surface through a patterned mask, and the photosensitive resin in the ceramic printing slurry absorbs ultraviolet light and then cures rapidly. Then the photocuring process is carried out layer by layer to finally form a three-dimensional structure. This method can greatly reduce the printing cycle without being restricted by the complexity of the part shape, which facilitates the rapid manufacturing of fine ceramic parts. Therefore, this technology has become one of the hot spots in the field of ceramic manufacturing, and it has been widely used in aerospace, biomedicine, machinery, electronics, and new energy vehicles.

[0003] During the exposure process of photocuring, the photosensitive resin monomer undergoes a chemical covalent bond transformation, resulting in a decrease in the molecular distance, which is manifested as a volume shrinkage of the material on a macro scale, resulting in dimensional deviations of ceramic printed parts. Photocuring shrinkage has always been a serious problem that restricts photocuring ceramics. At present, research institutions at home and abroad are trying to suppress warping deformation by optimizing the material system. The paper "A comprehensive evaluation of vat-photopolymerization resins and alumina slurries for ceramic stereolithography" proposes to conduct research on different photosensitive resin configurations, and obtain a mixed resin with the best comprehensive performance by blending the preferred monomers. However, the blending of resin monomers will increase the process of slurry preparation and post-processing. The paper "Research on Photosensitive Resin Systems for Photocuring 3D Printing Ceramic Components" proposes to introduce low-shrinkage prepolymers to achieve low-stress molding of large-sized alumina ceramic components. However, prepolymers usually have a large viscosity and require additional steps to dissolve them in photosensitive resins, which will also increase the viscosity of the printing slurry. The paper "Mask Image Planning for Deformation Control in Projection-Based Stereolithography Process" proposes an optimization method for photosensitive resin printing, which suppresses the warping deformation of the resin through discrete exposure. However, in addition to photosensitive resin, there is a large amount of ceramic powder in the ceramic photocuring slurry, and the printing process is quite different from the pure photosensitive resin printing process. Ceramic powder will reduce the bonding strength of the printed body, and fine feature structures are easily damaged during the material laying process. Therefore, directly using discrete exposure will lead to ceramic printing failure. It is necessary to explore new optimization methods to achieve high-precision photocuring molding of ceramics. Summary of the invention

[0004] The object of the present invention is to provide an alternate projection optimization method based on ceramic digital light processing technology, so as to solve the above-mentioned problems existing in the prior art.

[0005] In order to achieve the above object, the technical solution adopted by the present invention is as follows:

[0006] An alternating projection optimization method based on ceramic digital light processing technology comprises the following steps:

[0007] S100, slicing the printed model to obtain an initial projection pattern;

[0008] S200, obtaining a template base of each layer by setting a function and setting template parameters;

[0009] S300, obtaining the shell through morphological operations and logical operations, and determining the outer wall and inner pattern of each layer according to the shell;

[0010] S400, performing a logic operation on the internal pattern of each layer and the template substrate corresponding to each layer to obtain an optimized internal pattern;

[0011] S500, combining the optimized internal pattern of each layer with the outer wall pattern to obtain an optimized projection pattern;

[0012] S600, setting appropriate printing parameters according to the printing material, manufacturing layer by layer to obtain a ceramic printing blank, and obtaining a ceramic sintered part through post-processing steps such as degreasing and sintering.

[0013] Preferably, in step S100, the initial slice projection pattern is a binary image, the area with a value of 1 needs to be exposed and is white in the slice image; the area with a value of 0 does not need to be exposed and is black in the slice image.

[0014] Preferably, in step S200, the template substrate is obtained through a pattern unit array, and the set template parameters include the shape of the pattern unit and the array spacing; the template substrate patterns of the odd-numbered layers and the even-numbered layers are reversed, and the area with a value of 1 in the template substrate of the odd-numbered layers is reversed to 0, and the area with a value of 0 is reversed to 1;

[0015] The cross ratio of the pattern units of adjacent layers is set, which is determined by the dilation kernel size and is calculated as follows: cross ratio = (number of pattern unit pixels after dilation - number of pattern unit pixels before dilation) / number of pattern unit pixels before dilation.

[0016] Preferably, in step S300, the shell includes a top layer, a bottom layer, an outer wall, etc., the shell area is fully exposed, and the thickness of the top layer and the bottom layer is set to 0-200 μm;

[0017] The initial slice projection pattern is corroded and the corrosion core is set. The outer wall thickness is determined by the size of the corrosion core. The pattern after corrosion is inverted and the outer wall pattern is obtained by performing an intersection operation with the initial slice projection pattern. The outer wall thickness is set to 0.5-2mm. The outer wall pattern is inverted and the inner pattern is obtained by performing an intersection operation with the initial slice projection pattern.

[0018] Preferably, in step S400, the optimized projected internal pattern is obtained by performing an intersection operation on the template base obtained in step 200 and the internal pattern obtained in step 300.

[0019] Preferably, in step 500, the optimized projection pattern is obtained by performing a union operation of the outer wall pattern obtained in step 300 and the optimized projection internal pattern obtained in step 400.

[0020] Preferably, in step 600, the printing parameters are set to a layer thickness of 10-100 μm, a material spreading speed of 1-6 mm / s, and a light intensity of 10-300 mJ / cm 2 .

[0021] Preferably, the shapes of the pattern units include: square, rhombus, parallelogram and triangle.

[0022] Preferably, the array spacing is the spacing between the centers of two pattern units, and the array spacing is determined according to the size of the pattern.

[0023] Preferably, the cross ratio of pattern units of adjacent layers is set to 0-20%.

[0024] The beneficial effects of the present invention are as follows: the present invention discloses an alternating projection optimization method based on ceramic digital light processing technology, comprising the following steps: slicing a printing model to obtain an initial projection pattern; obtaining a template base for each layer by setting a function and setting template parameters; obtaining an outer shell by morphological operations and logical operations, and determining an outer wall and an inner pattern of each layer according to the outer shell; performing logical operations on the inner pattern of each layer and the template base corresponding to each layer to obtain an optimized inner pattern; combining the optimized inner pattern of each layer with the outer wall pattern to obtain an optimized projection pattern; setting appropriate printing parameters according to printing materials, manufacturing layer by layer to obtain a ceramic printing blank, and obtaining a ceramic sintered part through post-processing steps such as degreasing and sintering.

[0025] 1. The present invention can effectively reduce the warping deformation of the printed body during the ceramic digital light processing process, thereby improving the control of the part molding accuracy;

[0026] 2. The present invention directly modifies the projection pattern without modifying the equipment, has good versatility, and can be applied to various types of ceramic light-curing printers;

[0027] 3. The present invention does not require the introduction of additional materials, reduces the steps of batching and post-processing, improves manufacturing efficiency, and can be flexibly applied to photocuring printing of different ceramic materials by directly modifying parameters. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 It is a flow chart of an alternate projection optimization method based on ceramic digital light processing technology of the present invention;

[0029] Figure 2 is a flow chart of another embodiment of the present invention;

[0030] Figure 3 It is a schematic diagram of the present invention;

[0031] Figure 4is an example diagram of warpage comparison between full exposure and alternate exposure of the present invention;

[0032] Figure 5 It is an example diagram of the alternate exposure printing of the blank and the sintered part of the present invention. DETAILED DESCRIPTION

[0033] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings. It should be understood that the specific implementation methods described herein are only used to explain the present invention and are not used to limit the present invention.

[0034] The preparation method of the present invention discretizes the projection center. When the ceramic slurry is exposed to ultraviolet light, the volume shrinks. For a printed layer with only one area, the shrinkage within the layer surface is always toward a certain point within the layer. When a layer is composed of several independent areas, each independent area has a shrinkage center. If the initial exposure pattern can be discretized and divided into multiple areas for exposure, the shrinkage stress of each layer can be dispersed, thereby reducing the deformation of the part. The initial projection pattern of each layer is processed and divided into two parts: the outer wall and the inner pattern. In order to ensure that the outer surface of the part is smooth and has a certain strength, the outer shell is completely exposed. In order to suppress shrinkage deformation, discrete exposure is selected for the internal pattern, and the template base and outer wall parameters are set separately.

[0035] Reference Figure 1 , Figure 2 , Figure 3 , Figure 4 and Figure 5 An alternate projection optimization method based on ceramic digital light processing technology is shown, comprising the following steps:

[0036] S100, slicing the printed model to obtain an initial projection pattern.

[0037] S200, obtaining a template base for each layer by setting a function and setting template parameters.

[0038] S300, obtaining the outer shell through morphological operations and logical operations, and determining the outer wall and inner pattern of each layer according to the outer shell.

[0039] S400, performing a logic operation on the internal pattern of each layer and the template substrate corresponding to each layer to obtain an optimized internal pattern.

[0040] S500, combining the optimized inner pattern of each layer with the outer wall pattern to obtain an optimized projection pattern.

[0041] S600, setting appropriate printing parameters according to the printing material, manufacturing layer by layer to obtain a ceramic printing blank, and obtaining a ceramic sintered part through post-processing steps such as degreasing and sintering.

[0042] Preferably, in step S100, the initial slice projection pattern is a binary image, the area with a value of 1 needs to be exposed and is white in the slice image; the area with a value of 0 does not need to be exposed and is black in the slice image.

[0043] Preferably, in step S200, the template substrate is obtained through a pattern unit array, and the set template parameters include the shape of the pattern unit and the array spacing; the template substrate patterns of the odd-numbered layers and the even-numbered layers are reversed, and the area with a value of 1 in the template substrate of the odd-numbered layers is reversed to 0, and the area with a value of 0 is reversed to 1;

[0044] The cross ratio of the pattern units of adjacent layers is set, which is determined by the dilation kernel size and is calculated as follows: cross ratio = (number of pattern unit pixels after dilation - number of pattern unit pixels before dilation) / number of pattern unit pixels before dilation.

[0045] In this embodiment, the printed model is sliced, and the printing layer thickness and exposure parameters are set to obtain the initial projection pattern corresponding to each layer. The initial slice projection pattern is a binary image, where the area with a value of 1 needs to be exposed and is white in the slice image, and the area with a value of 0 does not need to be exposed and is black in the slice image.

[0046] Preferably, in step S300, the shell includes a top layer, a bottom layer, an outer wall, etc., the shell area is fully exposed, and the thickness of the top layer and the bottom layer is set to 0-200 μm;

[0047] The initial slice projection pattern is corroded and the corrosion core is set. The outer wall thickness is determined by the size of the corrosion core. The pattern after corrosion is inverted and the outer wall pattern is obtained by performing an intersection operation with the initial slice projection pattern. The outer wall thickness is set to 0.5-2mm. The outer wall pattern is inverted and the inner pattern is obtained by performing an intersection operation with the initial slice projection pattern.

[0048] Preferably, in step S400, the optimized projected internal pattern is obtained by performing an intersection operation on the template base obtained in step 200 and the internal pattern obtained in step 300.

[0049] Preferably, in step 500, the optimized projection pattern is obtained by performing a union operation of the outer wall pattern obtained in step 300 and the optimized projection internal pattern obtained in step 400.

[0050] Preferably, in step 600, the printing parameters are set to a layer thickness of 10-100 μm, a material spreading speed of 1-6 mm / s, and a light intensity of 10-300 mJ / cm 2 .

[0051] Preferably, the shapes of the pattern units include: square, rhombus, parallelogram and triangle.

[0052] Preferably, the array spacing is the spacing between the centers of two pattern units, and the array spacing is determined according to the size of the pattern.

[0053] Preferably, the cross ratio of pattern units of adjacent layers is set to 0-20%.

[0054] In this embodiment, refer to Figure 3 The template substrate is shown as being set, and the template substrate is composed of a plurality of discrete pattern unit arrays. Different template substrates are obtained by setting parameters such as the shape, size, and array spacing of the pattern units, wherein the shapes of the pattern units include squares, circles, rectangles, rhombuses, parallelograms, and triangles, etc. The template substrate patterns are set oppositely for odd-numbered layers and even-numbered layers to achieve alternating template substrates, thereby ensuring that each layer of the part is fully exposed during the printing process, and no unexposed slurry is retained in the part to affect the strength of the blank. In addition, the cross ratio of the pattern units of adjacent layers is set to further improve the bonding strength of the blank.

[0055] (3) In order to retain the external features of the printed parts, a shell area is set and fully exposed layer by layer. The shell includes a top layer, a bottom layer, and an outer wall. The number of fully exposed layers of the top layer and the bottom layer is set to obtain top layers and bottom layers of different thicknesses. The thickness of the top layer and the bottom layer is set to 0-200 μm. The outer wall part is obtained by corroding the initial slice projection pattern, inverting the corrosion result, and performing an intersection operation with the initial slice projection pattern. The thickness of the outer wall is determined by the size of the corrosion core, and the thickness of the outer wall is set to 0.5-2 mm; the outer wall pattern is inverted and an intersection operation is performed with the initial slice projection pattern to obtain the internal pattern.

[0056] (4) An optimized internal pattern is obtained by performing an intersection operation on the internal pattern of each layer and the template base corresponding to each layer. The optimized internal pattern divides an initial exposure area into multiple exposure areas, so that the shrinkage stress of the current layer is dispersed, thereby reducing the deformation of the part.

[0057] (5) Combine the optimized internal pattern of each layer with the outer wall pattern, obtain the optimized projection pattern through union operation, set appropriate printing parameters according to the printing material, set the printing layer thickness to 10-100 μm, the material laying speed to 1-6 mm / s, and the light intensity to 10-300 mJ / cm 2 , the ceramic printing body is obtained layer by layer, and the ceramic sintered parts are obtained through post-processing steps such as degreasing and sintering.

[0058] Embodiment 1:

[0059] The model is sliced ​​to obtain the initial projection pattern of each layer; the shape of the pattern unit is set to a square, the size is 0.5 mm, the spacing is 0.5 mm, and the cross ratio is set to 10% to obtain the template base; the thickness of the bottom and top layers is set to 50 μm, and the thickness of the outer wall is 0.5 mm to obtain the internal pattern and the outer shell pattern; the internal pattern is intersected with the template base to obtain the optimized internal pattern, and finally the optimized internal pattern of each layer is combined with the outer wall pattern, and the optimized projection pattern is obtained through a union operation.

[0060] Alumina ceramic slurry with a solid content of 55 vol% was prepared for photocuring, and the printing layer thickness was set to 50 μm, the paving speed was 2 mm / s, and the light intensity was 60 mJ / cm 2 , the ceramic printing body is obtained layer by layer, such as Figure 4 As shown in the figure, a 200-micron-thick thin plate was printed using full exposure and alternating exposure. After being removed from the platform, the fully exposed thin plate was severely deformed, while the warping deformation of the alternatingly exposed thin plate was effectively suppressed. The printed model is shown in Figure 4 As shown, dense ceramic sintered parts are obtained after post-processing steps such as debinding and sintering.

[0061] Embodiment 2:

[0062] The model is sliced ​​to obtain the initial projection pattern of each layer; the shape of the pattern unit is set to an equilateral triangle with a side length of 1 mm, a spacing of 1 mm, and a cross ratio of 0% to obtain a template base; the thickness of the bottom and top layers is set to 25 μm, and the thickness of the outer wall is 1 mm to obtain the internal pattern and the outer shell pattern; the internal pattern is intersected with the template base to obtain the optimized internal pattern, and finally the optimized internal pattern of each layer is combined with the outer wall pattern, and the optimized projection pattern is obtained through a union operation.

[0063] A zirconia ceramic slurry with a solid content of 50 vol% was prepared for photocuring, and the printing layer thickness was set to 100 μm, the material laying speed was set to 6 mm / s, and the light intensity was set to 200 mJ / cm 2 , the ceramic printing body is obtained layer by layer, and dense ceramic sintered parts are obtained through post-processing steps such as degreasing and sintering.

[0064] Embodiment 3:

[0065] The model is sliced ​​to obtain the initial projection pattern of each layer; the shape of the pattern unit is set to a circle, the radius is 1mm, the spacing is 1mm, and the cross ratio is set to 5% to obtain the template base; the thickness of the bottom and top layers is set to 100μm, and the outer wall thickness is 1.5mm to obtain the internal pattern and the outer shell pattern; the internal pattern is intersected with the template base to obtain the optimized internal pattern, and finally the optimized internal pattern of each layer is combined with the outer wall pattern, and the optimized projection pattern is obtained through the union operation.

[0066] A silicon nitride ceramic slurry with a solid content of 45 vol% was prepared for photocuring. The printing layer thickness was set to 10 μm, the paving speed was 1 mm / s, and the light intensity was 10 mJ / cm 2 , the ceramic printing body is obtained layer by layer, and dense ceramic sintered parts are obtained through post-processing steps such as degreasing and sintering.

[0067] Embodiment 4:

[0068] The model is sliced ​​to obtain the initial projection pattern of each layer; the shape of the pattern unit is set to a rhombus, the adjacent side angle is 90°, the side length is 2mm, the spacing is 2mm, and the cross ratio is set to 20% to obtain a template base; the thickness of the bottom and top layers is set to 200μm, and the outer wall thickness is 2mm to obtain the internal pattern and the outer shell pattern; the internal pattern is intersected with the template base to obtain the optimized internal pattern, and finally the optimized internal pattern of each layer is combined with the outer wall pattern, and the optimized projection pattern is obtained through a union operation.

[0069] Alumina ceramic slurry with a solid content of 70 vol% was prepared for photocuring, and the printing layer thickness was set to 200 μm, the paving speed was 4 mm / s, and the light intensity was 300 mJ / cm 2 , the ceramic printing body is obtained layer by layer, and dense ceramic sintered parts are obtained through post-processing steps such as degreasing and sintering.

[0070] By adopting the above technical solution disclosed in the present invention, the following beneficial effects are obtained:

[0071] The invention discloses an alternating projection optimization method based on ceramic digital light processing technology, comprising the following steps: slicing a printing model to obtain an initial projection pattern; obtaining a template base of each layer by setting a function and setting template parameters; obtaining a shell by morphological operations and logical operations, and determining the outer wall and inner pattern of each layer according to the shell; performing logical operations on the inner pattern of each layer and the template base corresponding to each layer to obtain an optimized inner pattern; combining the optimized inner pattern of each layer with the outer wall pattern to obtain an optimized projection pattern; setting appropriate printing parameters according to printing materials, manufacturing a ceramic printing blank layer by layer, and obtaining a ceramic sintered part through post-processing steps such as degreasing and sintering.

[0072] 1. The present invention can effectively reduce the warping deformation of the printed body during the ceramic digital light processing process, thereby improving the control of the part molding accuracy;

[0073] 2. The present invention directly modifies the projection pattern without modifying the equipment, has good versatility, and can be applied to various types of ceramic light-curing printers;

[0074] 3. The present invention does not require the introduction of additional materials, reduces the steps of batching and post-processing, improves manufacturing efficiency, and can be flexibly applied to photocuring printing of different ceramic materials by directly modifying parameters.

[0075] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be considered as the scope of protection of the present invention.

Claims

1. An alternating projection optimization method based on ceramic digital light processing technology, characterized in that: The following steps are involved: S100, slicing the printed model to obtain an initial projection pattern; S200, obtaining a template base for each layer by setting a function and setting the template parameters; S300, obtaining the shell through morphological operations and logical operations, and determining the outer wall and inner pattern of each layer according to the shell; S400, performing a logic operation on the internal pattern of each layer and the template substrate corresponding to each layer to obtain an optimized internal pattern; S500, combining the optimized internal pattern of each layer with the outer wall pattern to obtain an optimized projection pattern; S600, setting appropriate printing parameters according to the printing material, manufacturing layer by layer to obtain a ceramic printing blank, and obtaining a ceramic sintered part through post-processing steps such as degreasing and sintering.

2. The alternating projection optimization method based on ceramic digital light processing technology according to claim 1, characterized in that: In step S100, the initial slice projection pattern is a binary image, the area with a value of 1 needs to be exposed and is white in the slice image; the area with a value of 0 does not need to be exposed and is black in the slice image.

3. The alternating projection optimization method based on ceramic digital light processing technology according to claim 1, characterized in that: In step S200, the template substrate is obtained through a pattern unit array, and the template parameters set include the shape of the pattern unit and the array spacing; the template substrate patterns of the odd-numbered layers and the even-numbered layers are reversed, and the area with a value of 1 in the template substrate of the odd-numbered layers is reversed to 0, and the area with a value of 0 is reversed to 1; The cross ratio of the pattern units of adjacent layers is set, which is determined by the dilation kernel size and is calculated as follows: cross ratio = (number of pattern unit pixels after dilation - number of pattern unit pixels before dilation) / number of pattern unit pixels before dilation.

4. The alternating projection optimization method based on ceramic digital light processing technology according to claim 1, characterized in that: In step S300, the shell includes a top layer, a bottom layer, an outer wall, etc., the entire shell area is exposed, and the thickness of the top layer and the bottom layer is set to 0-200 μm; The initial slice projection pattern is corroded and the corrosion core is set. The outer wall thickness is determined by the size of the corrosion core. The pattern after corrosion is inverted and the outer wall pattern is obtained by performing an intersection operation with the initial slice projection pattern. The outer wall thickness is set to 0.5-2mm. The outer wall pattern is inverted and the inner pattern is obtained by performing an intersection operation with the initial slice projection pattern.

5. The alternating projection optimization method based on ceramic digital light processing technology according to claim 1, characterized in that: In step S400, the optimized projected internal pattern is obtained by performing an intersection operation on the template base obtained in step 200 and the internal pattern obtained in step 300.

6. The alternating projection optimization method based on ceramic digital light processing technology according to claim 1, characterized in that: In step 500 , the optimized projection pattern is obtained by performing a union operation on the outer wall pattern obtained in step 300 and the optimized projection internal pattern obtained in step 400 .

7. The alternating projection optimization method based on ceramic digital light processing technology according to claim 1, characterized in that: In step 600, the printing parameters are set to a layer thickness of 10-100 μm, a material spreading speed of 1-6 mm / s, and a light intensity of 10-300 mJ / cm 2 .

8. The alternating projection optimization method based on ceramic digital light processing technology according to claim 3 is characterized in that: The shapes of the pattern units include: square, rhombus, parallelogram and triangle.

9. The alternating projection optimization method based on ceramic digital light processing technology according to claim 3, characterized in that: The array spacing is the spacing between the centers of two pattern units, and the array spacing is determined according to the size of the pattern.

10. The alternating projection optimization method based on ceramic digital light processing technology according to claim 3, characterized in that: The cross ratio of the pattern units of adjacent layers is set to 0-20%.