SiBCNHf ceramic precursor with low viscosity and high ceramic yield as well as preparation method and application of SiBCNHf ceramic precursor

Through the combination of low viscosity SiBCNHf ceramic precursor and free radical initiator, the problem of improving the density and density of ceramic-based composite materials is solved, and the preparation of high ceramic yield and high performance ceramic-based composite materials is achieved, which meets high airtightness and the requirements for ablation resistance.

CN119059823APending Publication Date: 2024-12-03INST OF CHEM CHINESE ACAD OF SCI

Patent Information

Application Number
CN202310634688.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-31
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The high viscosity of the existing SiBCNHf ceramic precursors makes it difficult to improve the density and density of ceramic matrix composite materials, and the preparation period is long, which cannot meet the needs of high airtightness and ablation resistance.

Method used

Using a low viscosity SiBCNHf ceramic precursor, the viscosity is ≤30mPa·s by not containing organic solvents and combining free radical initiators, and high curing yield and ceramic yield at 250℃ and 900℃ to ensure ceramic matrix composite High density and density of materials.

Benefits of technology

The SiBCNHf ceramic precursor with low viscosity and high ceramic yield is achieved, which improves the density and airtightness of ceramic matrix composite materials, meets the high-performance needs of ceramic matrix composite materials and coatings, and simplifies the preparation process.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides a SiBCNHf ceramic precursor with low viscosity and high ceramic yield as well as a preparation method and application of the SiBCNHf ceramic precursor. The SiBCNHf ceramic precursor contains elements such as silicon, boron, carbon, nitrogen and hafnium; the SiBCNHf ceramic precursor does not contain an organic solvent, and the viscosity of the SiBCNHf ceramic precursor is less than or equal to 30mPa. S. According to the SiBCNHf ceramic precursor provided by the invention, the processing property of the SiBCNHf ceramic precursor can be emphatically improved while the excellent properties such as high thermal stability, high oxidation resistance and the like of a SiBCNHf ceramic product are maintained, so that infiltration and sealing of a micro-nano porous material are realized. The SiBCNHf ceramic precursor with extremely low viscosity and capable of being subjected to addition curing provided by the invention can be used for realizing impregnation and infiltration of micro-nano pores and other conventional precursors which cannot fill the pores on the surface of a composite material, and vinyl addition curing is initiated by heating, so that the impregnated and infiltrated precursor is retained in situ in the pores, and the impregnation and sealing effects can be greatly improved by virtue of the characteristics.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of ceramic materials, and in particular relates to a SiBCNHf ceramic precursor with low viscosity and high ceramic yield, and a preparation method and application thereof. Background Art

[0002] Silicon boron carbon nitride hafnium (SiBCNHf) ceramics have excellent high temperature resistance (above 2000℃), oxidation resistance and high temperature creep resistance, and are an important high-performance multi-element ceramic material. SiBCNHf ceramics are generally prepared by solidifying and pyrolysis of SiBCNHf ceramic precursors containing elements such as silicon, boron, carbon, nitrogen and hafnium in the molecule.

[0003] At present, the preparation method of SiBCNHf ceramic precursor is generally to add hafnium source compound to silicon-based ceramic precursor or its synthetic raw material. Most of the obtained SiBCNHf ceramic precursor is solid or high-viscosity liquid, which makes it often need to add solvent to dilute it to reduce viscosity when used as a matrix of ceramic-based composite materials. This operation will result in a low overall ceramic yield from precursor to ceramic and a long preparation cycle of composite materials. In addition, the impregnation and cracking process of ceramic-based composite materials is currently the mainstream preparation process for large-sized special-shaped components, and precursors such as polycarbosilane and polyzirconia are usually used as raw materials. The viscosity of these precursors is usually above 100mPa·s, and the density of ceramic-based composite materials prepared therefrom can only reach about 90%. The remaining pores are limited by the viscosity of the precursor and cannot be impregnated and infiltrated, and the density cannot be further improved. Summary of the invention

[0004] In order to improve the technical problems existing in the above-mentioned prior art, the present invention provides a low-viscosity, high-ceramic yield SiBCNHf ceramic precursor and its preparation method and use. The SiBCNHf ceramic precursor has the characteristics of low viscosity and high ceramic yield, and the ceramic-based composite material prepared from the SiBCNHf ceramic precursor has good compactness and high density, which can meet the performance requirements of ceramic-based composite components for air tightness or ablation resistance. The SiBCNHf ceramic precursor has a simple preparation process, which further expands its application in the fields of ceramic-based composite materials and ceramic coatings.

[0005] In order to achieve the above-mentioned invention object, the present invention adopts the following technical scheme:

[0006] A SiBCNHf ceramic precursor contains silicon, boron, carbon, nitrogen and hafnium elements; the SiBCNHf ceramic precursor does not contain an organic solvent and has a viscosity of ≤30 mPa·s.

[0007] According to an embodiment of the present invention, the SiBCNHf ceramic precursor does not contain an organic solvent and has a viscosity of 5 to 25 mPa·s, for example, 10 to 22 mPa·s, such as 12 mPa·s, 15 mPa·s, 18 mPa·s, 20 mPa·s or 22 mPa·s, indicating that the SiBCNHf ceramic precursor has a relatively low viscosity.

[0008] According to an embodiment of the present invention, the curing yield of the SiBCNHf ceramic precursor at 250° C. in an inert atmosphere is ≥85%. This indicates that the SiBCNHf ceramic precursor has a high curing yield. The curing yield refers to the weight ratio of the SiBCNHf ceramic precursor before and after curing, specifically the ratio of the weight of the cured product after curing to the weight of the precursor before curing.

[0009] According to an embodiment of the present invention, the ceramic yield of the SiBCNHf ceramic precursor after pyrolysis at 900° C. in an inert atmosphere is ≥58%. This indicates that the SiBCNHf ceramic precursor has a high ceramic yield. The ceramic yield refers to the weight ratio of the SiBCNHf ceramic precursor before and after pyrolysis, specifically the ratio of the weight of the ceramic after pyrolysis to the weight of the precursor before pyrolysis.

[0010] According to an embodiment of the present invention, after the SiBCNHf ceramic precursor is pyrolyzed at 900° C. in an inert atmosphere, the content of hafnium in the ceramic is ≥3%, indicating that the SiBCNHf ceramic precursor has a relatively high Hf content.

[0011] According to an embodiment of the present invention, the SiBCNHf ceramic precursor further contains a free radical initiator.

[0012] According to an embodiment of the present invention, the free radical initiator is selected from at least one of azobisisobutyronitrile, dicumyl peroxide, dibenzoyl peroxide and azobisisoheptylnitrile.

[0013] According to an embodiment of the present invention, the weight of the free radical initiator accounts for 0.5% to 3% of the total weight of the SiBCNHf ceramic precursor, such as 0.5%, 1%, 1.5%, 2%, 2.5% or 3%. The introduction of the free radical initiator can reduce the curing temperature of the SiBCNHf ceramic precursor and improve its curing yield.

[0014] According to an embodiment of the present invention, the viscosity of the SiBCNHf ceramic precursor after being sealed and stored at 25° C. for 12 months is ≤50 mPa·s, indicating that the SiBCNHf ceramic precursor has good storage stability.

[0015] According to an embodiment of the present invention, the SiBCNHf ceramic precursor is in a liquid state at room temperature.

[0016] According to an embodiment of the present invention, the SiBCNHf ceramic precursor can be pyrolyzed at 900-1500° C. in an inert atmosphere to form SiBCNHf ceramics; preferably, amorphous SiBCNHf ceramics are formed.

[0017] According to an embodiment of the present invention, the weight loss rate of the SiBCNHf ceramic precursor from 900°C to 1500°C under an inert atmosphere is ≤5%. This indicates that the SiBCNHf ceramic has relatively good high-temperature stability. The weight loss rate refers to the weight ratio of the ceramic obtained by pyrolysis of the precursor at 900°C after being heated to pyrolysis at 1500°C, that is, (ceramic weight before pyrolysis at 1500°C - ceramic weight after pyrolysis at 1500°C) / ceramic weight before pyrolysis at 1500°C.

[0018] The present invention also provides a SiBCNHf ceramic precursor, which is prepared by mixing a SiBCN ceramic precursor, a hafnium source and a free radical initiator; wherein the SiBCN ceramic precursor is prepared by a one-pot reaction using boron trichloride as a boron source, vinyl dichlorosilane as a silicon source, ammonia as a nitrogen source and trimethylchlorosilane as a capping agent.

[0019] According to an embodiment of the present invention, the SiBCNHf ceramic precursor is defined as described above.

[0020] According to an embodiment of the present invention, the mixing is performed at room temperature, for example.

[0021] According to an embodiment of the present invention, the mixing is performed under stirring conditions, for example.

[0022] According to the embodiment of the present invention, the mixing time is not particularly defined, as long as it can achieve uniform mixing of the SiBCN ceramic precursor, the hafnium source and the free radical initiator.

[0023] According to an embodiment of the present invention, the vinyl-containing dichlorosilane is at least one selected from methylvinyldichlorosilane, vinyldichlorosilane and divinyldichlorosilane.

[0024] According to an embodiment of the present invention, methyl hydrogen dichlorosilane and / or dimethyl dichlorosilane may be selectively added to the silicon source, wherein the total mole number of methyl hydrogen dichlorosilane and / or dimethyl dichlorosilane does not exceed the total mole number of vinyl dichlorosilane. Exemplarily, the silicon source is vinyl dichlorosilane, or a combination of vinyl dichlorosilane and methyl hydrogen dichlorosilane, or a combination of vinyl dichlorosilane and dimethyl dichlorosilane, or a combination of vinyl dichlorosilane, methyl hydrogen dichlorosilane and dimethyl dichlorosilane.

[0025] According to an embodiment of the present invention, the chemical formula of the hafnium source is Hf(NR2): n (NX2) 4-n , wherein NR2 is at least one of di-n-propylamino, diisopropylamino, diallylamino, tetrahydropyrrolyl and hexahydropyridyl; NX2 is dimethylamino and / or diethylamino; and n is any integer or decimal between 1 and 4.

[0026] According to an embodiment of the present invention, the amount of the hafnium source added is 5% to 10% of the total weight of the SiBCNHf ceramic precursor, for example, 5%, 6%, 7%, 8%, 9% or 10%.

[0027] According to an embodiment of the present invention, the one-pot reaction refers to mixing a boron source, a silicon source, a nitrogen source and a capping agent, reacting them, and directly obtaining the SiBCN ceramic precursor without separating intermediates.

[0028] According to an embodiment of the present invention, a boron source, a silicon source, a nitrogen source and a capping agent are mixed at a temperature of -5 to -20°C; illustratively, the boron source, the silicon source and the capping agent are mixed at a temperature of -5 to -10°C; then, a nitrogen source is added at a temperature of -15 to -20°C and mixing is continued.

[0029] According to an embodiment of the present invention, the reaction is, for example, first reacted at 25-35°C for 3-6 hours, then distilled under reduced pressure at 25-40°C for 1-5 hours, and finally distilled under reduced pressure at 100-120°C for 1-2 hours.

[0030] According to an embodiment of the present invention, the molar ratio of the boron source to the capping agent is 1:(0.15-0.35), for example, 1:0.15, 1:0.20, 1:0.25, 1:0.30 or 1:0.35.

[0031] According to an embodiment of the present invention, the molar ratio of the boron source to the silicon source is 1:(1-3), for example, 1:1, 1:1.5, 1:2, 1:2.5 or 1:3.

[0032] According to an embodiment of the present invention, the molar amount of the nitrogen source is 1.3 to 2 times the sum of the molar number of chlorine in the boron source, the molar number of chlorine in the silicon source and the molar number of chlorine in the capping agent, for example, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9 or 2 times.

[0033] According to an embodiment of the present invention, the one-pot reaction is carried out in the presence of a solvent.

[0034] According to an embodiment of the present invention, the solvent is selected from at least one of petroleum ether, n-heptane, n-hexane, toluene and xylene.

[0035] According to an embodiment of the present invention, the amount of the solvent is 4 to 10 times, for example, 4, 5, 6, 7, 8, 9 or 10 times the total weight of the boron source, the silicon source and the capping agent.

[0036] According to an embodiment of the present invention, the one-pot reaction is carried out under the protection of an inert atmosphere.

[0037] According to an embodiment of the present invention, the inert atmosphere is at least one of nitrogen, argon or helium.

[0038] The present invention also provides a method for preparing the SiBCNHf ceramic precursor, the method comprising the following steps:

[0039] 1) using boron trichloride as a boron source, vinyl dichlorosilane as a silicon source, ammonia as a nitrogen source, and trimethylchlorosilane as a capping agent, a SiBCN ceramic precursor is prepared by a one-pot reaction;

[0040] 2) Mixing the SiBCN ceramic precursor prepared in step 1), a hafnium source and a free radical initiator to prepare the SiBCNHf ceramic precursor.

[0041] According to the embodiment of the present invention, step 1) specifically includes the following steps:

[0042] Boron trichloride, vinyl dichlorosilane, optionally added or not added methyl hydrogen dichlorosilane and / or dimethyl dichlorosilane, ammonia and trimethyl chlorosilane are mixed and reacted to prepare the SiBCN ceramic precursor.

[0043] The mixing is carried out at a temperature of -20 to -5°C, that is, the boron source, silicon source, nitrogen source and capping agent are mixed at a temperature of -5 to -20°C; illustratively, the boron source, silicon source and capping agent are mixed at a temperature of -5 to -10°C; then, the nitrogen source is added at a temperature of -15 to -20°C and the mixing is continued.

[0044] The reaction is, for example, first reacted at 25-35° C. for 3-6 hours, then distilled under reduced pressure at 25-40° C. for 1-5 hours, and finally distilled under reduced pressure at 100-120° C. for 1-2 hours.

[0045] According to an embodiment of the present invention, in step 2), the mixing is performed at room temperature, for example.

[0046] According to an embodiment of the present invention, in step 2), the mixing is performed under stirring conditions, for example.

[0047] According to an embodiment of the present invention, in step 2), the mixing time is not particularly defined, and it only needs to be sufficient to achieve uniform mixing of the SiBCN ceramic precursor, the hafnium source and the free radical initiator.

[0048] According to an embodiment of the present invention, the preparation method comprises the following steps:

[0049] (1) Under the protection of an inert atmosphere, adding a solvent to the system;

[0050] (2) at a temperature of -5 to -10°C, introducing boron trichloride gas into the system, followed by adding vinyl dichlorosilane, optionally with or without methyl hydrogen dichlorosilane and / or dimethyl dichlorosilane, and trimethyl chlorosilane;

[0051] (3) introducing ammonia gas into the system at a temperature of -15 to -20°C;

[0052] (4) reacting at 25-35°C for 3-6 hours and filtering;

[0053] (5) distilling the filtrate under reduced pressure at 25-40°C for 1-5 hours, heating it to 100-120°C and distilling it under reduced pressure for 1-2 hours;

[0054] (6) adding a free radical initiator to the system and stirring evenly;

[0055] (7) Adding a hafnium source into the system and stirring evenly to obtain the SiBCNHf ceramic precursor.

[0056] The present invention also provides application of the SiBCNHf ceramic precursor in ceramic-based composite materials and ceramic coatings.

[0057] According to an embodiment of the present invention, the SiBCNHf ceramic precursor is used for preparing a ceramic-based composite material by a PIP method and as a sealing coating of a ceramic-based composite material.

[0058] Beneficial effects:

[0059] The present invention provides a SiBCNHf ceramic precursor with low viscosity and high ceramic yield, and a preparation method and use thereof. The SiBCNHf ceramic precursor is prepared by using readily available raw materials to prepare a liquid SiBCN ceramic precursor, and then mixing the SiBCN ceramic precursor with a hafnium source and a free radical initiator. The SiBCNHf ceramic precursor has the characteristics of low viscosity, high curing yield and good high-temperature stability, and can achieve the purpose of having both low viscosity and high ceramic yield for the precursor. The SiBCNHf ceramic precursor can achieve impregnation and infiltration of micro-nano porous materials on the surface of composites and other holes that cannot be filled by conventional precursors, and through heating to initiate vinyl addition curing, the impregnated and infiltrated precursor is retained in situ in the holes. The above characteristics can greatly improve the impregnation and sealing effects. The use of the SiBCNHf ceramic precursor can increase the density of the composite material and meet the preparation and application requirements of ceramic matrix composites and their sealing coatings. Detailed Embodiments

[0060] <SiBCN ceramic precursor>

[0061] As described above, the SiBCN ceramic precursor contains silicon, boron, carbon and nitrogen elements.

[0062] In one embodiment, the SiBCN ceramic precursor satisfies (1) the curing weight loss rate of the SiBCN ceramic precursor is ≤10% under an inert atmosphere at 200-250 °C; this shows that the SiBCN ceramic precursor has the characteristic of low curing residue weight. Among them, the curing weight loss rate refers to the weight ratio of the weight lost before and after the precursor curing, specifically the weight difference between the precursor before and after curing and the weight of the precursor before curing, that is, (weight of the precursor - weight of the cured product) / weight of the precursor; 200-250 °C means that the curing temperature is any temperature between 200-250 °C, that is, the curing weight loss rate of the SiBCN ceramic precursor is ≤10% when cured at any temperature between 200-250 °C after rising from room temperature.

[0063] In one embodiment, the SiBCN ceramic precursor satisfies (2) the oxygen content in the ceramic after pyrolysis of the SiBCN ceramic precursor is ≤2% under an inert atmosphere at 900 °C; this shows that the SiBCN ceramic precursor has the characteristic of low oxygen content.

[0064] In one embodiment, the SiBCN ceramic precursor satisfies (3) the weight loss rate of the SiBCN ceramic precursor between 900°C and 1500°C under an inert atmosphere is ≤5%, indicating that the SiBCN ceramic product prepared from the SiBCN ceramic precursor has the characteristic of high thermal stability; wherein the weight loss rate refers to the weight ratio of the ceramic obtained by pyrolysis of the precursor at 900°C after being heated to pyrolysis at 1500°C, that is, (ceramic weight before pyrolysis at 1500°C - ceramic weight after pyrolysis at 1500°C) / ceramic weight before pyrolysis at 1500°C.

[0065] In one embodiment, the SiBCN ceramic precursor does not contain an organic solvent and has a viscosity of ≤20 mPa·s, which indicates that the SiBCN ceramic precursor has a relatively low viscosity.

[0066] In one embodiment, the viscosity of the SiBCN ceramic precursor after being sealed and stored at 25° C. for 12 months is ≤25 mPa·s, indicating that the SiBCN ceramic precursor has good storage stability.

[0067] In one embodiment, the SiBCN ceramic precursor is in a liquid state at room temperature.

[0068] The present invention will be described in further detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only exemplary descriptions and explanations of the present invention and should not be construed as limiting the scope of protection of the present invention. All technologies implemented based on the above content of the present invention are included in the scope that the present invention is intended to protect.

[0069] Unless otherwise specified, the experimental methods used in the following examples are all conventional methods; the reagents, materials, etc. used in the following examples, unless otherwise specified, can be obtained from commercial channels.

[0070] The hafnium source compound Hf(NR2) used in the following examples is n (NX2) 4-n The synthesis method is as follows: using tetrakisdimethylamino hafnium or tetrakisdiethylamino hafnium as a raw material, adding an amine compound HNR2 in a required proportion, stirring and reacting at room temperature for 4 to 24 hours, and then distilling under reduced pressure at 60° C. to obtain the corresponding hafnium source compound.

[0071] Example 1

[0072] Under the protection of inert gas, add 200g of n-hexane to the system, cool to -5°C, introduce 9.0g (77mmol) of boron trichloride gas into the system, then add 16.3g (115mmol) of methylvinyldichlorosilane and 1.7g (15.6mmol) of trimethylchlorosilane. Continue to cool to -15°C, introduce 12g (705mmol) of ammonia into the system, heat the system to 25°C and continue stirring for 3 hours, collect the filtrate by filtration, distill at 30°C for 2 hours, and distill at 120°C for 1 hour to obtain a liquid product. Add diisopropylbenzene peroxide accounting for 1% of the total weight of the liquid product, and add hafnium source Hf(NR2)2(NX2)2 accounting for 6% of the total weight of the liquid product, wherein NR2 is di-n-propylamino and NX2 is diethylamino, stir evenly, and obtain SiBCNHf precursor.

[0073] The obtained SiBCNHf precursor does not contain any organic solvent and has a viscosity of 12 mPa·s.

[0074] The obtained precursor was heated to 60°C at 3°C / min under nitrogen for 1h, then heated to 150°C at 3°C / min for 1h, then heated to 200°C at 3°C / min for 1h, then heated to 250°C at 3°C / min for 2h to obtain a solidified product with a solidification yield of 86.6%. The ceramic yield of the obtained precursor after pyrolysis at 900°C under nitrogen was 58.6%, and the hafnium content in the ceramic product was 3.5%. The weight loss rate of the 900°C pyrolysis product pyrolyzed at 1500°C for 2h in an argon atmosphere was 3.05%, and the obtained ceramic product was an amorphous SiBCNHf ceramic.

[0075] Example 2

[0076] Under the protection of inert gas, add 240g of n-heptane to the system, cool to -10°C, pass 9.0g (77mmol) of boron trichloride gas, then add 16.9g (120mmol) of methylvinyldichlorosilane, 3.7g (32mmol) of methylhydrogendichlorosilane, and 2.1g (19.3mmol) of trimethylchlorosilane. Continue to cool to -15°C, pass 15g (880mmol) of ammonia, heat the system to 35°C and continue to stir and react for 3 hours, filter and collect the filtrate, distill at 40°C for 2 hours, and distill at 120°C for 1 hour to obtain a liquid product. Add diisopropylbenzene peroxide accounting for 1% of the total weight of the liquid product, and add hafnium source Hf(NR2)1(NX2)3 accounting for 8% of the total weight of the liquid product, wherein NR2 is diallylamino and NX2 is diethylamino, stir evenly, and obtain SiBCNHf precursor.

[0077] The viscosity of the obtained SiBCNHf precursor is 22 mPa·s.

[0078] The obtained precursor was heated to 60°C at 3°C / min under nitrogen and kept for 1h, then heated to 150°C at 3°C / min and kept for 1h, then heated to 200°C at 3°C / min and kept for 1h, then heated to 250°C at 3°C / min and kept for 2h to obtain a solidified product with a solidification yield of 85.3%. The ceramic yield of the obtained precursor after pyrolysis at 900°C under nitrogen was 59.1%, and the hafnium content in the ceramic product was 4.5%. The weight loss rate of the 900°C pyrolysis product was 2.68% when the temperature was increased from 10°C / min to 1500°C for 2h under argon atmosphere, and the obtained ceramic product was an amorphous SiBCNHf ceramic.

[0079] Example 3

[0080] Under the protection of inert gas, 300g toluene was added to the system, the temperature was lowered to -10°C, 9.0g (77mmol) of boron trichloride gas was introduced, and then 14.1g (100mmol) of methylvinyldichlorosilane, 11.7g (92mmol) of vinyldichlorosilane, and 2.1g (19.3mmol) of trimethylchlorosilane were added. The temperature was further lowered to -15°C, 17g (1000mmol) of ammonia was introduced, the system was heated to 25°C and the reaction was continued with stirring for 3 hours, the filtrate was collected by filtration, and the liquid product was obtained by vacuum distillation at 30°C for 2 hours, and the liquid product was obtained by vacuum distillation at 100°C for 1 hour. Azobisisobutyronitrile accounting for 2% of the total weight of the liquid product and hafnium source Hf(NR2)3(NX2)1 accounting for 5% of the total weight of the liquid product were added, wherein NR2 is tetrahydropyrrolyl and NX2 is dimethylamino, and the mixture was stirred evenly to obtain SiBCNHf precursor.

[0081] The viscosity of the obtained SiBCNHf precursor is 18 mPa·s.

[0082] The obtained precursor was heated to 60°C at 3°C / min under nitrogen and kept for 1h, then heated to 150°C at 3°C / min and kept for 1h, then heated to 200°C at 3°C / min and kept for 1h, then heated to 250°C at 3°C / min and kept for 2h to obtain a solidified product with a solidification yield of 87.5%. The ceramic yield of the obtained precursor after pyrolysis at 900°C under nitrogen was 59.8%, and the hafnium content in the ceramic product was 3.3%. The weight loss rate of the 900°C pyrolysis product was 3.59% when the temperature was increased from 10°C / min to 1500°C for 2h in an argon atmosphere, and the obtained ceramic product was an amorphous SiBCNHf ceramic.

[0083] The above is an explanation of the embodiments of the present invention. However, the present invention is not limited to the above embodiments. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A SiBCNHf ceramic precursor, wherein: The SiBCNHf ceramic precursor contains silicon, boron, carbon, nitrogen and hafnium elements; the SiBCNHf ceramic precursor does not contain an organic solvent and has a viscosity of ≤30 mPa·s.

2. The SiBCNHf ceramic precursor according to claim 1, wherein: The curing yield of the SiBCNHf ceramic precursor at 250° C. and in an inert atmosphere is ≥85%; and / or, the ceramic yield of the SiBCNHf ceramic precursor after pyrolysis at 900° C. in an inert atmosphere is ≥58%; And / or, the content of hafnium in the ceramic after the SiBCNHf ceramic precursor is pyrolyzed at 900° C. in an inert atmosphere is ≥3%; And / or, the SiBCNHf ceramic precursor has a weight loss rate of ≤5% from 900° C. to 1500° C. in an inert atmosphere.

3. The SiBCNHf ceramic precursor according to claim 1 or 2, wherein: The SiBCNHf ceramic precursor also contains a free radical initiator; Preferably, the free radical initiator is selected from at least one of azobisisobutyronitrile, diisopropylbenzene peroxide, dibenzoyl peroxide and azobisisoheptylnitrile; and / or the weight of the free radical initiator accounts for 0.5% to 3% of the total weight of the SiBCNHf ceramic precursor.

4. A SiBCNHf ceramic precursor, wherein: The SiBCNHf ceramic precursor is prepared by mixing a SiBCN ceramic precursor, a hafnium source and a free radical initiator; wherein the SiBCN ceramic precursor is prepared by a one-pot reaction using boron trichloride as a boron source, vinyl dichlorosilane as a silicon source, ammonia as a nitrogen source and trimethylchlorosilane as a capping agent.

5. The SiBCNHf ceramic precursor according to claim 4, wherein: The vinyl dichlorosilane is selected from at least one of methyl vinyl dichlorosilane, vinyl dichlorosilane and divinyl dichlorosilane; Preferably, methyl hydrogen dichlorosilane and / or dimethyl dichlorosilane are further added to the silicon source, wherein the total mole number of methyl hydrogen dichlorosilane and / or dimethyl dichlorosilane does not exceed the total mole number of vinyl dichlorosilane; Preferably, the chemical formula of the hafnium source is Hf(NR2) n (NX2) 4-n , wherein NR2 is at least one of di-n-propylamino, diisopropylamino, diallylamino, tetrahydropyrrolyl and hexahydropyridyl; NX2 is dimethylamino and / or diethylamino; n is any integer or decimal between 1 and 4; And / or, the amount of the hafnium source added accounts for 5% to 10% of the total weight of the SiBCNHf ceramic precursor.

6. The SiBCNHf ceramic precursor according to claim 4 or 5, wherein: Mixing a boron source, a silicon source, a nitrogen source and a capping agent at a temperature of -5 to -20°C; Preferably, the boron source, the silicon source and the capping agent are mixed at a temperature of -5 to -10°C; then, the nitrogen source is added at a temperature of -15 to -20°C and the mixing is continued; Preferably, the reaction is first carried out at 25-35° C. for 3-6 hours, then distilled under reduced pressure at 25-40° C. for 1-5 hours, and finally distilled under reduced pressure at 100-120° C. for 1-2 hours.

7. The SiBCNHf ceramic precursor according to any one of claims 4 to 6, wherein: The molar ratio of the boron source to the end-capping agent is 1:(0.15-0.35); And / or, the molar ratio of the boron source to the silicon source is 1:(1-3); And / or, the molar amount of the nitrogen source is 1.3 to 2 times the sum of the molar number of the chlorine element in the boron source, the molar number of the chlorine element in the silicon source and the molar number of the chlorine element in the capping agent; Preferably, the one-pot reaction is carried out in the presence of a solvent; Preferably, the solvent is selected from at least one of petroleum ether, n-heptane, n-hexane, toluene and xylene; And / or, the amount of the solvent used is 4 to 10 times the total weight of the boron source, the silicon source and the capping agent.

8. A method for preparing a SiBCNHf ceramic precursor according to any one of claims 1 to 3, the method comprising the following steps: 1) using boron trichloride as a boron source, vinyl dichlorosilane as a silicon source, ammonia as a nitrogen source, and trimethylchlorosilane as a capping agent, a SiBCN ceramic precursor is prepared by a one-pot reaction; 2) Mixing the SiBCN ceramic precursor prepared in step 1), a hafnium source and a free radical initiator to prepare the SiBCNHf ceramic precursor.

9. The preparation method according to claim 8, wherein: Step 1) specifically includes the following steps: Boron trichloride, vinyl dichlorosilane, optionally with or without methyl hydrogen dichlorosilane and / or dimethyl dichlorosilane, ammonia and trimethyl chlorosilane are mixed and reacted to prepare the SiBCN ceramic precursor; Preferably, the mixing is carried out at a temperature of -20 to -5°C, that is, the boron source, silicon source, nitrogen source and capping agent are mixed at a temperature of -5 to -20°C; illustratively, the boron source, silicon source and capping agent are mixed at a temperature of -5 to -10°C; then, the nitrogen source is added at a temperature of -15 to -20°C and the mixing is continued; Preferably, the reaction is first carried out at 25-35° C. for 3-6 hours, then distilled under reduced pressure at 25-40° C. for 1-5 hours, and finally distilled under reduced pressure at 100-120° C. for 1-2 hours.

10. Use of the SiBCNHf ceramic precursor according to any one of claims 1 to 7 in ceramic matrix composites and ceramic coatings.

Citation Information

Patent Citations

  • Liquid borosilicate resin and preparation method and application thereof

    CN105968366A

  • Low-oxygen liquid SiHfBCN ceramic precursor, preparation method and SiHfBCN ceramic

    CN111393579A

Cited By

  • Preparation method of flexible SiBCNHf ceramic fiber fabric for high-temperature electromagnetic shielding

    CN120099711A