Corrosion-resistant high-polishing plastic die steel and preparation method thereof

Through the smelting technology of blast furnace water molten iron and ferroalloy, combined with vacuum self-consumption and high-temperature homogenization treatment, the shortcomings of existing mold steel in high polishing and corrosion resistance are solved, and the preparation of high-quality plastic molds is realized, which meets the polychlorine. The forming demand for materials such as ethylene and fluoroplastics.

CN119061313AActive Publication Date: 2024-12-03DAYE SPECIAL STEEL CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411024797.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-12-03
Estimated Expiration
2044-07-29

AI Technical Summary

Technical Problem

The existing corrosion-resistant plastic mold steel has shortcomings in terms of high polishing and corrosion resistance. Especially when manufacturing plastic products such as polyvinyl chloride, fluoroplastics and ABS, due to the influence of corrosive gases, the surface roughness of the mold cannot meet the high requirements. Moreover, commonly used mold steels have problems such as severe non-metallic inclusions and poor tissue uniformity.

Method used

Blast furnace water molten iron and ferroalloy are used as raw materials, and through vacuum self-consumption smelting, high-temperature homogenization treatment, solid solution treatment and spheroidized annealing, the inclusion and gas content in the mold steel are reduced, and the material structure is improved to reach GB/T35840.3. -Series A annealed structure of standard 2018.

Benefits of technology

It achieves high polishing and corrosion resistance, non-metallic inclusions are no more than 0.5 levels, low oxygen and nitrogen content, zero carbide liquidity, smoothness reaches A1 or A0 levels, and appearance level is 10, meeting high-quality plastic molds Requirements for use.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of die steel manufacturing, in particular to corrosion-resistant high-polishing plastic die steel and a preparation method thereof.The preparation method comprises the following steps that S1, blast furnace molten iron, iron alloy and waste steel serve as raw materials, and after smelting in an alloy smelting furnace and an electric furnace, LF refining and VD degassing are conducted, electrode base metal is poured; s2, the electrode base material is subjected to vacuum consumable smelting in a vacuum consumable furnace, and a steel ingot is obtained; s3, the steel ingot is subjected to high-temperature homogenization treatment and then subjected to multidirectional upsetting and drawing forging treatment; s4, the forge piece is subjected to solution treatment; and S5, the forged piece is subjected to spheroidizing annealing treatment. According to the method, blast furnace molten iron and vacuum consumable smelting are adopted, so that non-metallic inclusions in the plastic die steel are all not larger than 0.5 grade, and through high-temperature homogenization treatment and subsequent solid solution and spheroidizing annealing treatment, the annealing structure of the plastic die steel is within the A series specified by the GB / T35840.3-2018 standard.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of mold steel manufacturing, in particular to a corrosion-resistant high-polishing plastic mold steel and a preparation method thereof. Background Art

[0002] In recent years, with the rapid development of the plastics industry, more and more requirements have been put forward for mold steel, which should not only have high toughness, but also have certain corrosion resistance, especially in the process of manufacturing raw plastic products such as polyvinyl chloride (PVC), fluoroplastics and ABS with flame retardants added, because plastics will decompose into corrosive gases such as hydrogen chloride, hydrogen fluoride and sulfur dioxide in the molten state, which will cause certain corrosion to the mold cavity. The production of molds such as optical lenses has extremely high requirements for surface roughness. The roughness value Ra of the injection mold cavity surface is required to be at the level of 0.1μm to 0.25μm, the mirror processing requires Ra≤0.063μm, and the optical surface requires Ra<0.01μm. Therefore, affected by the working environment, there are a series of requirements for plastic mold steel, such as wear resistance, strength, hardness, polishing, and corrosion resistance. Among them, polishing and corrosion resistance are the most important, because surface wear and corrosion account for about 50% of mold failure forms.

[0003] The polishing of the mold is also called mirror processing, and the standard is divided into 4 levels: A0 = Ra0.008μm, A1 = Ra0.016μm, A3 = Ra0.032μm, A4 = Ra0.063μm. To meet the use requirements of high-quality plastic molds, purity and uniformity are the two major elements of the metallurgical quality of plastic mold steel. At present, the commonly used corrosion-resistant plastic mold steel on the market is 4Cr13NiVSi. This type of mold steel has serious non-metallic inclusions and poor uniformity of organization, which cannot meet the needs of high-polished plastic mold steel. Summary of the invention

[0004] In view of the above-mentioned deficiencies in the prior art, the object of the present invention is to provide a corrosion-resistant and highly polished plastic mold steel and a preparation method thereof. The present invention adopts blast furnace molten iron as raw material to reduce the inclusion content in the mold steel, and adopts vacuum consumable smelting to further reduce the inclusion and gas content in the mold steel, thereby improving the purity, so that the non-metallic inclusions in the obtained plastic mold steel are not greater than level 0.5. The present invention improves the material organization and component segregation by performing high-temperature homogenization treatment, and obtains a fine and uniform spheroidized organization through subsequent solution + spheroidizing annealing treatment, so that the annealed organization of the obtained plastic mold steel can reach within the A series specified in the GB / T35840.3-2018 standard.

[0005] In order to achieve the above object, the present invention adopts the following technical solutions:

[0006] In a first aspect, the present invention provides a method for preparing a corrosion-resistant high-polished plastic mold steel, the preparation method comprising the following steps:

[0007] S1. Using blast furnace iron, ferroalloy and scrap steel as raw materials, after smelting in alloy melting furnace and electric furnace, LF refining, VD degassing, argon gas protection is used to cast electrode base material;

[0008] S2, performing vacuum consumable smelting on the electrode base material in a vacuum consumable furnace to obtain a steel ingot;

[0009] S3, subjecting the steel ingot obtained in step S2 to high temperature homogenization treatment, and then subjecting the steel ingot to multi-directional upsetting forging treatment;

[0010] S4, performing a solution treatment on the forging obtained in step S3, wherein the solution treatment comprises heating the forging to a solution temperature and keeping the temperature, and then performing alternating water-air cooling to obtain a martensite and lower bainite structure;

[0011] S5. Perform spheroidizing annealing treatment on the forging obtained in step S4, wherein the spheroidizing annealing treatment comprises charging the forging obtained in step S4 into a furnace, heating it to 850-900°C, keeping it warm, then reducing the temperature to 790-840°C at a rate greater than 10°C / h and not greater than 20°C / h, then reducing the temperature to 660-700°C at a rate ≤10°C / h, then cooling it to ≤500°C in the furnace, and then taking it out of the furnace and air cooling it.

[0012] Furthermore, the phosphorus content in the blast furnace molten iron is not higher than 0.025%, and the total content of lead, arsenic, tin, antimony and bismuth is not greater than 0.025% by mass percentage;

[0013] and / or, the ferroalloy comprises high carbon ferrochrome, low carbon ferrochrome, ferromolybdenum, ferrovanadium and ferronickel;

[0014] And / or, the scrap steel includes at least one of medium-sized scrap steel and heavy-sized scrap steel.

[0015] Furthermore, in step S1, the ferroalloy is melted uniformly in the alloy melting furnace, and the tapping temperature is 1550-1650°C;

[0016] and / or, in step S1, the blast furnace molten iron and the scrap steel are melted and dephosphorized by the electric furnace, the phosphorus content is not higher than 0.005wt%, and the tapping temperature is 1600-1680°C;

[0017] And / or, in step S1, the molten steel from the alloy melting furnace and the electric furnace is added to the LF refining furnace for desulfurization to no more than 0.003wt%, degassing, and removal of inclusions, and adjusted to the required composition; then VD degassing is performed, and the nitrogen content in the molten steel is no more than 70*10 -6, oxygen content is not more than 10*10 -6 ;

[0018] And / or, in step S1, after the molten steel is subjected to the VD degassing treatment, the molten steel is poured into the consumable electrode mold of the consumable electrode pouring station by ladle pouring to cast the electrode base material, and the electrode base material is obtained after mold cooling and demolding, wherein the temperature of the molten steel ladle is 1510-1560°C, and the mold cooling time is 2h-8h.

[0019] Furthermore, in step S1, after obtaining the electrode base material, the electrode base material is subjected to stress relief annealing, wherein the stress relief annealing includes placing the electrode base material into an annealing furnace, heating it to 750-800°C, keeping it warm according to the effective diameter (2-4h) / 100mm, and then cooling it to no higher than 200°C and air cooling it out of the furnace.

[0020] Furthermore, in step S1, after stress relief annealing is performed on the electrode base material, the electrode base material is subjected to a cutting treatment and a surface polishing treatment.

[0021] Further, in step S2, the melting rate of the vacuum consumable melting is controlled at 6.0-12.0 kg / min;

[0022] and / or, in step S2, shrinkage compensation is started when the remaining electrode base material weight is 3% to 10% of the initial total electrode base material weight;

[0023] And / or, in step S2, after obtaining the steel ingot, the steel ingot is demolded after cooling in the mold for 1h to 5h and then subjected to stress relief annealing. The stress relief annealing includes placing the steel ingot into an annealing furnace, heating it to 750-800°C, keeping it warm according to the effective diameter (2-4h) / 100mm, cooling it to no higher than 200°C in the furnace and air cooling it out of the furnace.

[0024] Further, in step S3, the high temperature homogenization treatment includes subjecting the steel ingot obtained in step S2 to high temperature homogenization treatment at 1200-1300° C. and keeping the temperature at an effective diameter (2-4h) / 100mm;

[0025] And / or, in step S3, the multi-directional upsetting forging process includes: cooling the steel ingot after the high-temperature homogenization treatment to 1100-1200°C, using an upper flat plate and a lower platform for multi-directional upsetting forging, with a pressing amount of 20-50% each time, turning 90° to press another plane, pressing the three planes twice in sequence, with a total forging ratio of 6-12, controlling the final forging temperature to 800-900°C, and obtaining a forging.

[0026] Furthermore, in step S4, the solution temperature is 950-1050°C, and the holding time is 2-5h;

[0027] And / or, in step S4, during the water-air alternating cooling process, water-air alternating cooling is performed twice, the water temperature is not higher than 40°C at the start, the temperature of the forging is reduced to 450-550°C at the first water entry, the forging is air-cooled until the forging is dry at the first water exit, the temperature of the forging is reduced to 250-350°C at the second water entry, the water temperature is not higher than 50°C at the end, and the forging is air-cooled to 100-200°C at the end;

[0028] And / or, in step S5, the forging obtained in step S4 is charged into a furnace and heated to 850-900°C, and kept warm according to the thickness (3-5h) / 100mm.

[0029] Furthermore, the corrosion-resistant high-polished plastic mold steel comprises, by mass percentage, C 0.35-0.45%, Si 0.50-1.20%, Mn 0.50-1.20%, Cr 12.5-14.5%, Mo0.20-0.50%, V 0.20-0.50%, Ni 0.30-0.80%, and the rest is Fe and unavoidable impurities.

[0030] In a second aspect, the present invention provides a corrosion-resistant high-polished plastic mold steel, which is prepared by the preparation method described in the first aspect.

[0031] Compared with the prior art, the beneficial effects of the present invention include at least one of the following:

[0032] (1) The present invention adopts blast furnace molten iron as raw material to reduce the inclusion content in the mold steel, and adopts vacuum consumable smelting to further reduce the inclusion and gas content in the mold steel, thereby improving the purity, so that the non-metallic inclusions in the obtained plastic mold steel are not greater than level 0.5. The present invention improves the material structure and component segregation by performing high-temperature homogenization treatment, and obtains a fine and uniform spheroidized structure through subsequent solid solution + spheroidizing annealing treatment, so that the annealed structure of the obtained plastic mold steel can reach within the A series specified in GB / T35840.3-2018 standard.

[0033] (2) The oxygen mass percentage in the plastic mold steel prepared by the present invention is not more than 10*10 -6 , Nitrogen mass percentage is not more than 60*10 -6 , the liquid precipitation carbide is zero, the smoothness (polishability) reaches A1 (Ra0.016μm) and A0 (Ra0.008μm). After 48h of acid salt spray test in NaCl solution according to GB / T10125-2021, the defect area is 0 (no defect) and the appearance grade is 10 (highest). DETAILED DESCRIPTION

[0034] In order to make the purpose, technical scheme and advantages of the present invention clearer, the technical scheme in the embodiment of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present invention. The process parameters of the following embodiments that do not specify specific conditions are usually based on conventional conditions.

[0035] The endpoints and any values ​​of the ranges disclosed in the present invention are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be regarded as specifically disclosed in the present invention.

[0036] In a first aspect, the present invention provides a method for preparing a corrosion-resistant high-polished plastic mold steel, the preparation method comprising the following steps:

[0037] S1. Using blast furnace iron, ferroalloy and scrap steel as raw materials, after smelting in alloy melting furnace and electric furnace, LF refining, VD degassing, argon gas protection is used to cast electrode base material;

[0038] S2, performing vacuum consumable smelting on the electrode base material in a vacuum consumable furnace to obtain a qualified steel ingot;

[0039] S3, subjecting the steel ingot obtained in step S2 to high temperature homogenization treatment, and then subjecting the steel ingot to multi-directional upsetting forging treatment;

[0040] S4, performing a solution treatment on the forging obtained in step S3, wherein the solution treatment comprises heating the forging to a solution temperature and keeping the temperature, and then performing alternating water-air cooling to obtain a martensite and lower bainite structure;

[0041] S5. Perform spheroidizing annealing treatment on the forging obtained in step S4, wherein the spheroidizing annealing treatment comprises charging the forging obtained in step S4 into a furnace, heating it to 850-900°C (for example, 850°C, 870°C or 900°C), keeping it warm, then reducing the temperature to 790-840°C (for example, 790°C, 810°C or 840°C) at a rate greater than 10°C / h and not greater than 20°C / h, and then reducing the temperature to 660-700°C (for example, 660°C, 680°C or 700°C) at a rate ≤10°C / h, and then cooling it in the furnace to ≤500°C and then taking it out of the furnace for air cooling.

[0042] Martensite is a supersaturated solid solution of carbon in α-Fe. Lower bainite is a mechanical mixture of supersaturated lamellar ferrite and cementite precipitated inside it. There is enough carbon in these two structures, which can quickly precipitate to form a spheroidization core during the subsequent spheroidization process, resulting in a uniform spheroidized structure.

[0043] During the spheroidizing annealing process, the second cooling rate is lower than the first cooling rate. The main purpose is to reduce the degree of supercooling and make the carbides precipitate and grow evenly.

[0044] The present invention adopts blast furnace molten iron as a raw material to reduce the inclusion content in the mold steel, adopts vacuum consumable smelting to eliminate the instability of the smelting process, further reduces the inclusion and gas content in the mold steel, thereby improving the purity, so that the non-metallic inclusions in the obtained plastic mold steel are not greater than level 0.5. The present invention improves the material organization and component segregation through high-temperature homogenization treatment, and obtains a fine and uniform spheroidized organization through subsequent solid solution + spheroidizing annealing treatment, so that the annealed organization of the obtained plastic mold steel can reach within the A series specified in the GB / T35840.3-2018 standard.

[0045] In the above-mentioned method for preparing corrosion-resistant high-polished plastic mold steel, as an optional implementation, the phosphorus content in the blast furnace molten iron is not higher than 0.025%, and the total content of lead, arsenic, tin, antimony and bismuth is not more than 0.025% by mass percentage. P is a harmful element in steel, which causes component segregation and affects the uniformity of the structure. The higher the content, the greater the impact. Therefore, it is necessary to limit the phosphorus content to no more than 0.025%. Lead, arsenic, tin, antimony and bismuth are all trace elements with low melting points. If the content is too high, the grain boundaries will be segregated, affecting the material properties and hot processing.

[0046] In the above-mentioned method for preparing corrosion-resistant and highly polished plastic mold steel, as an optional embodiment, the ferroalloy includes high carbon ferrochrome, low carbon ferrochrome, ferromolybdenum, ferrovanadium and ferronickel; preferably, the phosphorus content in the high carbon ferrochrome is not more than 0.025wt%, and the phosphorus content in the low carbon ferrochrome is not more than 0.025wt%.

[0047] In the above-mentioned method for preparing corrosion-resistant high-polished plastic mold steel, as an optional implementation, the scrap steel includes at least one of medium-sized scrap steel and heavy-duty scrap steel.

[0048] In the above-mentioned method for preparing corrosion-resistant and highly polished plastic mold steel, as an optional implementation mode, in step S1, the ferroalloy is melted evenly by the alloy melting furnace, and the tapping temperature is 1550-1650°C, for example, it can be 1550°C, 1570°C, 1590°C, 1610°C, 1630°C or 1650°C.

[0049] In the above-mentioned method for preparing corrosion-resistant and highly polished plastic mold steel, as an optional implementation, in step S1, the blast furnace molten iron and the scrap steel are melted and dephosphorized using the electric furnace, the phosphorus content is not higher than 0.005wt%, and the tapping temperature is 1600-1680°C (for example, it can be 1600°C, 1620°C, 1640°C, 1660°C or 1680°C).

[0050] In the above-mentioned method for preparing corrosion-resistant high-polished plastic mold steel, as an optional embodiment, in step S1, the molten steel from the alloy melting furnace and the electric furnace is added to the LF refining furnace for desulfurization to no more than 0.003wt%, degassing, and inclusion removal, and adjusted to the required composition; then VD degassing treatment is performed, and the nitrogen content in the molten steel is no more than 70*10 -6 , oxygen content is not more than 10*10 -6 .

[0051] In the above-mentioned preparation method of corrosion-resistant and highly polished plastic mold steel, as an optional implementation mode, in step S1, after the molten steel is subjected to the VD degassing treatment, the steel is poured into the consumable electrode mold of the consumable electrode pouring station by ladle casting to cast the electrode base material, and the electrode base material is obtained after mold cooling and demolding, wherein the temperature of the molten steel ladle is 1510-1560°C (for example, it can be 1510°C, 1530°C or 1560°C), and the mold cooling time is 2h-8h (for example, it can be 2h, 4h, 6h or 8h).

[0052] In the above-mentioned preparation method of corrosion-resistant high-polished plastic mold steel, as an optional implementation, in step S1, after obtaining the electrode base material, the electrode base material is subjected to stress relief annealing, wherein the stress relief annealing includes placing the electrode base material into an annealing furnace, heating it to 750-800°C (for example, it can be 750°C, 770°C or 800°C), keeping it warm according to the effective diameter (2-4h) / 100mm, and then cooling it to no higher than 200°C in the furnace and air cooling it out of the furnace.

[0053] Here, effective diameter = 1 / 2*(upper base diameter + lower base diameter).

[0054] (2~4h) / 100mm / means that according to the effective diameter of the electrode base material, the insulation time is 2-4h for every 100mm. For example, if the effective diameter of the electrode base material is 200mm, the insulation time is 4-8h.

[0055] In the above-mentioned method for preparing corrosion-resistant high-polished plastic mold steel, as an optional implementation, in step S1, in order to ensure the purity of the molten steel, the electrode base material is subjected to a cutting treatment and a surface polishing treatment after the stress relief annealing of the electrode base material. The cutting treatment is used to cut off the part of the electrode base material that is poorly compensated for shrinkage, so as to prevent foreign inclusions from mixing into the molten steel during the smelting process; the surface polishing treatment is used to obtain an electrode base material with good surface quality, so as to prevent surface oxide scale and foreign inclusions from contaminating the molten steel.

[0056] In the above-mentioned method for preparing corrosion-resistant high-polished plastic mold steel, as an optional implementation, in step S2, the melting rate of the vacuum consumable melting is controlled at 6.0-12.0 kg / min (for example, 6 kg / min, 8 kg / min, 10 kg / min or 12.0 kg / min). If the melting rate is too fast, the molten pool is deep, the alloy elements are severely segregated during the solidification process, and the equiaxed crystal band in the center of the ingot is wide, and the quality is poor; if the melting rate is too slow, the molten pool does not obtain enough heat, and cold shut defects are generated on the surface of the steel ingot, affecting the surface quality.

[0057] In the above-mentioned method for preparing corrosion-resistant high-polished plastic mold steel, as an optional implementation, in order to obtain a steel ingot with better internal quality, shrinkage compensation is started when the remaining electrode matrix weight is 3% to 10% (for example, it can be 3%, 5%, 7% or 10%) of the total weight of the initial electrode matrix to avoid the formation of larger shrinkage cavities in the last solidified part of the steel ingot.

[0058] In the above-mentioned preparation method of corrosion-resistant high-polished plastic mold steel, as an optional implementation mode, in step S2, after obtaining the steel ingot, the steel ingot is demolded after cooling for 1h to 5h (for example, 1h, 3h or 5h) and then subjected to stress relief annealing. The stress relief annealing includes charging the steel ingot into an annealing furnace and heating it to 750-800°C (for example, 750°C, 770°C or 800°C), keeping it warm according to the effective diameter (2-4h) / 100mm, and then cooling it to no higher than 200°C in the furnace and air cooling it out of the furnace.

[0059] In the above-mentioned method for preparing corrosion-resistant high-polished plastic mold steel, as an optional embodiment, in step S3, the high-temperature homogenization treatment includes subjecting the steel ingot obtained in step S2 to high-temperature homogenization treatment at 1200-1300°C (for example, 1200°C, 1220°C, 1240°C, 1260°C, 1280°C or 1300°C) and keeping the temperature according to the effective diameter (2-4h) / 100mm to improve the original chemical composition and structural segregation of the steel ingot. If the temperature is too low, the diffusion rate of alloy elements is slow, and the homogenization effect cannot be achieved; if the temperature is too high, the steel ingot is overheated or overburned, which reduces the performance of the steel material and even makes it scrapped.

[0060] In the above-mentioned method for preparing corrosion-resistant high-polished plastic mold steel, as an optional embodiment, in step S3, the multi-directional upsetting forging process includes: cooling the steel ingot after the high-temperature homogenization process to 1100-1200°C (for example, 1100°C, 1120°C, 1140°C, 1160°C, 1180°C or 1200°C), using an upper plate and a lower platform for multi-directional upsetting forging, and pressing down by 20-5 0% (for example, it can be 20%, 30%, 40% or 50%), turn 90° to press another plane, and press the three planes down twice in sequence. The total forging ratio is 6-12 (for example, it can be 6, 8, 10 or 12), ensuring that the core of the forging is fully deformed, and controlling the final forging temperature to 800-900℃ (for example, it can be 800℃, 820℃, 840℃, 860℃, 880℃ or 900℃) to obtain forgings with uniform performance and structure. If the final forging temperature is too high, the grain size will be coarse; if the final forging temperature is too low, the surface of the forging will easily crack. Among them, the calculation method of the forging ratio depends on the specific forging process. The forging ratio during drawing is the ratio of the cross-sectional area before and after drawing, and the forging ratio during upsetting is the ratio of the height before and after upsetting. The total forging ratio is obtained by adding the forging ratios of each process.

[0061] In the above-mentioned preparation method of corrosion-resistant high-polished plastic mold steel, as an optional implementation, in step S4, the solid solution temperature is 950-1050°C (for example, it can be 950°C, 1000°C, or 1050°C), and the insulation time is 2-5h (for example, it can be 2h, 3h or 5h).

[0062] In the preparation method of the corrosion-resistant high-polished plastic mold steel, as an optional embodiment, in step S4, during the water-air alternating cooling process, the water-air alternating cooling is performed twice, the water temperature is not higher than 40°C at the beginning, the temperature of the forging is reduced to 450-550°C (for example, 450°C, 500°C or 550°C) at the first water entry, the water is discharged for the first time and air-cooled until the forging is dry, the temperature of the forging is reduced to 250-350°C (for example, 250°C, 300°C or 350°C) at the second water entry, the water temperature is not higher than 50°C, and finally air-cooled to 100-200°C, for example, 100°C, 120°C, 140°C, 160°C, 180°C or 200°C. If the water temperature is too high at the beginning, the cooling rate decreases, and the purpose of avoiding carbide precipitation cannot be achieved. If the ending water temperature is too high, the cooling capacity decreases, the cooling time is extended, and the martensite or lower bainite structure cannot be obtained. The present invention can make the forgings less prone to cracking through water-air alternating cooling.

[0063] In the above-mentioned method for preparing corrosion-resistant high-polished plastic mold steel, as an optional implementation, in step S5, the forging obtained in step S4 is charged into a furnace and heated to 850-900°C, and is kept warm according to the thickness (3-5h) / 100mm. (3-5h) / 100mm means that according to the thickness of the forging, every 100mm is kept warm for 3-5h, for example, if the thickness of the forging is 200mm, then the holding time is 6-10h.

[0064] In the preparation method of the corrosion-resistant high-polished plastic mold steel, as an optional embodiment, the composition of the corrosion-resistant high-polished plastic mold steel includes, by mass percentage: C 0.35-0.45%, Si 0.50-1.20%, Mn0.50-1.20%, Cr 12.5-14.5%, Mo 0.20-0.50%, V0.20-0.50%, Ni 0.30-0.80%, and the rest is Fe and inevitable impurities. The present invention can improve the corrosion resistance of mold steel and improve liquid precipitation carbide by adding molybdenum.

[0065] In a second aspect, the present invention provides a corrosion-resistant high-polished plastic mold steel, which is prepared by the preparation method described in the first aspect.

[0066] At present, the commonly used corrosion-resistant plastic mold steel on the market is 4Cr13NiVSi, which has poor chloride ion corrosion resistance. The steel of the present invention is based on 4Cr13NiVSi, and an appropriate amount of Mo content is added to improve the corrosion resistance of the steel and prevent pitting of the steel in the chloride solution. At the same time, molybdenum has a solid solution strengthening effect on ferrite and also improves the stability of carbides, thereby improving the strength of the steel. Molybdenum can also play a powerful role in improving the ductility, toughness and wear resistance of steel. In addition, by increasing the content of C and Si elements, the present invention enables the mold steel to obtain a higher hardness and better polishing properties.

[0067] The non-metallic inclusions of the corrosion-resistant high-polished plastic mold steel provided by the present invention are all no greater than 0.5 grade, and the oxygen mass percentage is no greater than 10*10 -6 , Nitrogen mass percentage is not more than 60*10 -6 , the annealed structure can reach the A series specified in GB / T35840.3-2018 standard, the carbide liquid precipitation is zero, and the finish reaches A1 (Ra0.016μm) and A0 (Ra0.008μm). After 48 hours of acid salt spray test in NaCl solution according to GB / T10125-2021, the defect area is 0 (no defect) and the appearance grade is 10 (highest).

[0068] The present invention will be further described in detail below with reference to specific embodiments and comparative examples.

[0069] Example 1

[0070] A corrosion-resistant high-polishing plastic mold steel has the following chemical components and mass percentages: C 0.40%, Si 0.70%, Mn 0.50%, Cr 13.60%, Mo 0.30%, V 0.25%, Ni 0.40%, and the remainder is Fe and inevitable impurities.

[0071] The preparation method of the above-mentioned corrosion-resistant high-polished plastic mold steel comprises the following steps:

[0072] S1. Using an alloy melting furnace to evenly melt high carbon ferrochrome (the phosphorus content in the high carbon ferrochrome is 0.018wt%), low carbon ferrochrome (the phosphorus content in the low carbon ferrochrome is 0.023wt%), ferromolybdenum, ferrovanadium and ferronickel, the tapping temperature is 1570°C; using an electric furnace to melt and dephosphorize molten iron from a blast furnace (the phosphorus content in the blast furnace molten iron is 0.021wt%, and the total content of lead, arsenic, tin, antimony and bismuth is 0.018wt%) and medium-sized scrap steel, the phosphorus content is 0.002wt%, and the tapping temperature is 1640°C; the molten steel from the alloy melting furnace and the electric furnace is added to a LF refining furnace for desulfurization to 0.002wt%, degassing, and inclusion removal, and adjusted to the required composition; then VD degassing is performed, and the nitrogen content in the molten steel is 70*10 -6 , oxygen content is 8*10 -6 ; After the molten steel is subjected to the VD degassing treatment, the ladle is used to cast the molten steel into the consumable electrode mold of the consumable electrode casting station, and argon gas is used to protect the casting of 6t of electrode base material. After mold cooling and demolding, the electrode base material is obtained, wherein the temperature of the molten steel ladle is 1525℃; the mold cooling time is 4h; after obtaining the electrode base material, the electrode base material is loaded into the annealing furnace and heated to 780℃, and kept warm for 24h according to the effective diameter of 4h / 100mm, and then the fire is turned off and cooled to 180℃ with the furnace, and then air-cooled out of the furnace to obtain a good quality electrode base material. The obtained electrode base material is subjected to cutting treatment and surface polishing treatment.

[0073] S2. Place the electrode matrix in a vacuum consumable furnace for vacuum consumable smelting to obtain a steel ingot. During the vacuum consumable smelting process, the melting rate is controlled at 6-8 kg / min. When the remaining electrode matrix weight is 4% of the total weight of the initial electrode matrix, shrinkage compensation begins (the last 4% weight of the electrode matrix begins shrinkage compensation). After obtaining the steel ingot, cool it in the mold for 2 hours, then demould it, place the steel ingot in an annealing furnace and heat it to 780°C. Keep it warm for 20 hours according to the effective diameter of 4h / 100mm, then turn off the fire and cool it to 180°C with the furnace, and air cool it out of the furnace to obtain a steel ingot with good quality.

[0074] S3. The steel ingots are subjected to high temperature homogenization treatment at 1230°C with an effective diameter of 4h / 100mm and heat preservation for 20h, then cooled to 1160°C with the furnace, and multi-directional upsetting forging is performed using an upper flat plate and a lower platform. The pressing amount is 30% each time, and the other plane is turned 90° to press. The three planes are pressed down twice in sequence, with a total forging ratio of 7.5 and a final forging temperature of 810°C to obtain forgings with a thickness of 200mm*width of 810mm*length of 3500mm and uniform performance and structure.

[0075] S4. The forgings are charged into a furnace and heated to a solution temperature of 1020°C. The forgings are kept warm for 2 hours and then cooled alternately in water and air twice. The water temperature is initially 28°C. The temperature of the forgings is lowered to 480°C for the first water entry. The forgings are air-cooled until they are dry after the water exits for the first time. The temperature of the forgings is lowered to 270°C for the second water entry. The water temperature is terminated at 35°C and then air-cooled to 160°C.

[0076] S5. Charge the forgings into a furnace and heat them to 870°C, keep them warm for 6h at a thickness of 3h / 100mm, then reduce the temperature to 830°C at a rate of 15°C / h, and then reduce the temperature to 690°C at a rate of 10°C / h, then cool them in the furnace to 480°C, take them out of the furnace and air cool them to obtain die steel.

[0077] The properties of the corrosion-resistant high-polished plastic mold steel prepared by the above method were tested. Among them, the non-metallic inclusions: Class A (sulfide) coarse series, Class A (sulfide) fine series, Class B (alumina) coarse series, Class B (alumina) fine series, Class C (silicate) coarse series, Class C (silicate) fine series, Class D (spherical oxide) coarse series, Ds (large-particle spherical oxide) coarse series are all 0 level, and Class D (spherical oxide) fine series is 0.5 level; in terms of mass percentage, the oxygen content is 6*10 -6 、Nitrogen content 50*10 -6 ; The annealed structure can reach A2 specified in GB / T35840.3-2018 standard; according to the GB / T18254 test, the carbide liquid precipitation is zero; the finish (polishability) reaches A0 (Ra0.008μm); after 48h of acid salt spray test in NaCl solution according to GB / T10125-2021, the defect area is 0 (no defect) and the appearance grade is 10 (highest).

[0078] Example 2

[0079] A corrosion-resistant high-polishing plastic mold steel has the following chemical components and mass percentages: C 0.42%, Si 0.50%, Mn 0.60%, Cr 13.00%, Mo 0.35%, V 0.35%, Ni 0.60%, and the rest being Fe and inevitable impurities.

[0080] The above-mentioned method for preparing corrosion-resistant high-polished plastic mold steel comprises the following steps:

[0081] S1. Using an alloy melting furnace to evenly melt high carbon ferrochrome (the phosphorus content in the high carbon ferrochrome is 0.018wt%), low carbon ferrochrome (the phosphorus content in the low carbon ferrochrome is 0.023wt%), ferromolybdenum, ferrovanadium and ferronickel, the tapping temperature is 1590°C; using an electric furnace to melt and dephosphorize molten iron from a blast furnace (the phosphorus content in the blast furnace molten iron is 0.021wt%, and the total content of lead, arsenic, tin, antimony and bismuth is 0.018wt%) and medium-sized scrap steel, the phosphorus content is 0.003wt%, and the tapping temperature is 1660°C; the molten steel from the alloy melting furnace and the electric furnace is added to a LF refining furnace for desulfurization to 0.001wt%, degassing, and inclusion removal, and adjusted to the required composition; then VD degassing is performed, and the nitrogen content in the molten steel is 60*10 -6 , oxygen content is 7*10 -6 ; After the molten steel is subjected to the VD degassing treatment, the ladle is used to cast the molten steel into the consumable electrode mold of the consumable electrode casting station, and argon gas is used to protect the casting of 12t of electrode base material. After mold cooling and demolding, the electrode base material is obtained, wherein the ladle temperature of the molten steel is 1535°C and the mold cooling time is 6h; after obtaining the electrode base material, the electrode base material is loaded into the annealing furnace and heated to 760°C, and kept warm for 32h according to the effective diameter of 4h / 100mm, and then the fire is turned off and cooled to 150°C with the furnace, and then air-cooled out of the furnace to obtain a good quality electrode base material. The obtained electrode base material is subjected to cutting treatment and surface polishing treatment.

[0082] S2. The electrode base material is placed in a vacuum consumable furnace for vacuum consumable smelting to obtain a steel ingot. During the vacuum consumable smelting process, the melting rate is controlled at 8-10 kg / min. When the remaining electrode base material weight is 8% of the total weight of the initial electrode base material, shrinkage compensation begins (the last 8% weight of the electrode base material begins to be compensated). After the steel ingot is obtained, the mold cooling time is 3 hours, and then the steel ingot is demoulded and placed in an annealing furnace to heat up to 770°C. It is kept warm for 27 hours according to the effective diameter of 3h / 100mm, and then the fire is turned off and the furnace is cooled to 160°C and air-cooled to obtain a steel ingot of good quality.

[0083] S3. The steel ingots are subjected to high-temperature homogenization treatment at 1270°C with effective diameter of 3h / 100mm and heat preservation for 27h, then cooled to 1150°C with the furnace, and multi-directional upsetting forging is performed using the upper flat plate and the lower platform. The pressing amount is 45% each time, and the other plane is pressed at 90°. The three planes are pressed down twice in sequence, with a total forging ratio of 10.2 and a final forging temperature of 850°C to obtain forgings with a thickness of 350mm*width of 1010mm*length of 3280mm and uniform performance and structure.

[0084] S4. Load the forgings into a furnace, heat to a solution temperature of 1000°C, keep warm for 4 hours, and cool them alternately in water and air twice. The water temperature starts at 25°C, the temperature of the forgings drops to 500°C for the first time they enter the water, the air cools them until the forgings are dry, the temperature of the forgings drops to 290°C for the second time they enter the water, the water temperature ends at 33°C, and then they are air cooled to 130°C.

[0085] S5. The forgings are heated to 890°C in a furnace and kept at this temperature for 12 hours, then reduced to 820°C at a rate of 18°C / h, and then reduced to 660°C at a rate of 8°C / h, and then cooled in the furnace to 450°C and then air-cooled to obtain die steel.

[0086] The properties of the corrosion-resistant high-polished plastic mold steel prepared by the above method were tested. Among them, the non-metallic inclusions: Class D (spherical oxides) fine system is 0.5 level, and the other Class A (sulfide) coarse system, Class A (sulfide) fine system, Class B (alumina) coarse system, Class B (alumina) fine system, Class C (silicate) coarse system, Class C (silicate) fine system, Class D (spherical oxides) coarse system, Ds (large-particle spherical oxides) are all 0 level; in terms of mass percentage, the oxygen content is 4*10 -6 、Nitrogen content 38*10 -6 ; The annealed structure can reach A2 specified in GB / T35840.3-2018 standard; according to the GB / T18254 test, the carbide liquid precipitation is zero; the finish (polishability) reaches A1 (Ra0.016μm); after 48h of acid salt spray test in NaCl solution according to GB / T10125-2021, the defect area is 0 (no defect) and the appearance grade is 10 (highest).

[0087] Example 3

[0088] A corrosion-resistant high-polishing plastic mold steel has the following chemical components and mass percentages: C 0.42%, Si 0.90%, Mn 0.80%, Cr 13.30%, Mo 0.40%, V 0.40%, Ni 0.50%, and the remainder is Fe and inevitable impurities.

[0089] The preparation method of the above-mentioned corrosion-resistant high-polished plastic mold steel comprises the following steps:

[0090] S1. Using an alloy melting furnace to evenly melt high carbon ferrochrome (the phosphorus content in the high carbon ferrochrome is 0.018wt%), low carbon ferrochrome (the phosphorus content in the low carbon ferrochrome is 0.023wt%), ferromolybdenum, ferrovanadium and ferronickel, the tapping temperature is 1600°C; using an electric furnace to melt and dephosphorize molten iron from a blast furnace (the phosphorus content in the blast furnace molten iron is 0.021wt%, and the total content of lead, arsenic, tin, antimony and bismuth is 0.018wt%) and medium-sized scrap steel, the phosphorus content is 0.003wt%, and the tapping temperature is 1660°C; the molten steel from the alloy melting furnace and the electric furnace is added to a LF refining furnace for desulfurization to 0.002wt%, degassing, and inclusion removal, and adjusted to the required composition; then VD degassing is performed, and the nitrogen content in the molten steel is 70*10 -6 , oxygen content is 8*10 -6 ; After the molten steel is subjected to the VD degassing treatment, the ladle is used to cast the molten steel into the consumable electrode mold of the consumable electrode casting station, and argon gas is used to protect the casting of 6t of electrode base material. After mold cooling and demolding, the electrode base material is obtained, wherein the ladle temperature of the molten steel is 1540°C; the mold cooling time is 5h; after obtaining the electrode base material, the electrode base material is placed in an annealing furnace and heated to 780°C, and kept warm for 24h according to the effective diameter of 4h / 100mm, and then the fire is turned off and cooled to 180°C with the furnace, and then air-cooled out of the furnace to obtain a good quality electrode base material. The obtained electrode base material is subjected to cutting treatment and surface polishing treatment.

[0091] S2. The electrode base material is placed in a vacuum consumable furnace for vacuum consumable smelting to obtain a steel ingot. During the vacuum consumable smelting process, the melting rate is controlled at 6-8 kg / min. When the remaining electrode base material weight is 6% of the total weight of the initial electrode base material, shrinkage compensation is started (the last 6% weight of the electrode base material is used for shrinkage compensation). After the steel ingot is obtained, the mold is cooled for 3 hours, then demolded, and the steel ingot is placed in an annealing furnace and heated to 780°C. It is kept warm for 20 hours according to the effective diameter of 4h / 100mm, and then the fire is turned off and cooled to 180°C with the furnace, and then air-cooled out of the furnace to obtain a steel ingot of good quality.

[0092] S3. The steel ingots are subjected to high-temperature homogenization treatment at 1230°C with an effective diameter of 4h / 100mm and heat preservation for 20h, then cooled to 1160°C with the furnace, and multi-directional upsetting forging is performed using an upper flat plate and a lower platform. The pressing amount is 30% each time, and the other plane is turned 90° to press. The three planes are pressed down twice in sequence, with a total forging ratio of 7.5 and a final forging temperature of 810°C to obtain forgings with a thickness of 200mm*width of 810mm*length of 3500mm and uniform performance and structure.

[0093] S4. Charge the forgings mentioned above into a furnace, heat to the solution temperature of 1020°C, keep warm for 2 hours, and cool alternately with water and air. The water temperature starts at 28°C, the temperature of the forgings drops to 500°C when entering water for the first time, air cools the forgings out of water for the first time until they are dry, and the temperature of the forgings drops to 300°C when entering water for the second time. The water temperature ends at 33°C, and then air cools to 160°C.

[0094] S5. Charge the forgings into a furnace and heat them to 870°C, keep them warm for 8 hours at a thickness of 4h / 100mm, then reduce them to 830°C at a rate of 15°C / h, and then reduce them to 690°C at a rate of 10°C / h, then cool them in the furnace to 480°C, take them out of the furnace and air cool them to obtain die steel.

[0095] The properties of the corrosion-resistant high-polished plastic mold steel prepared by the above method were tested. Among them, the non-metallic inclusions: Class A (sulfide) coarse series, Class A (sulfide) fine series, Class B (alumina) coarse series, Class B (alumina) fine series, Class C (silicate) coarse series, Class C (silicate) fine series, Class D (spherical oxide) coarse series, Ds (large-particle spherical oxide) fine series are all level 0, and Class D (spherical oxide) fine series is level 0.5; in terms of mass percentage, the oxygen content is 8*10 -6 、Nitrogen content 40*10 -6 ; The annealed structure can reach A2 specified in GB / T35840.3-2018 standard; according to the GB / T18254 test, the carbide liquid precipitation is zero; the finish (polishability) reaches A0 (Ra0.008μm); after 48h of acid salt spray test in NaCl solution according to GB / T10125-2021, the defect area is 0 (no defect) and the appearance grade is 10 (highest).

[0096] It can be seen from Examples 1-3 that the present invention adopts blast furnace molten iron as a raw material to reduce the inclusion content in the mold steel, and adopts vacuum consumable smelting to further reduce the inclusion and gas content in the mold steel, thereby improving the purity, so that the non-metallic inclusions in the obtained plastic mold steel are not greater than level 0.5. The present invention improves the material organization and component segregation by performing high-temperature homogenization treatment at 1200-1300°C, and obtains a fine and uniform spheroidized organization through subsequent solution + spheroidizing annealing treatment, so that the annealed organization of the obtained plastic mold steel can reach within the A series specified in the GB / T35840.3-2018 standard.

[0097] Comparative Example 1

[0098] The corrosion-resistant high-polishing plastic mold steel provided in this comparative example has the following chemical composition and mass percentage: C 0.40%; Si 0.70%; Mn 0.50%; Cr 13.60%; Mo 0.30%; V 0.25%; Ni 0.40%; the rest is Fe and unavoidable impurities.

[0099] The preparation method of the corrosion-resistant high-polished plastic mold steel is basically the same as that of Example 1, except that:

[0100] In step S2, the electrode base material is smelted by electroslag remelting. The specific process is: add 70wt% CaF2+30wt% CaO electroslag system according to 5% of the weight of the electrode base material, the filling ratio is 0.70, the melting rate is 0.7Kg / h of the crystallizer diameter (unit is mm) (if the crystallizer diameter is Amm, then the melting rate is A*0.7Kg / h), and the whole process is protected by argon.

[0101] The performance of the corrosion-resistant and highly polished plastic mold steel prepared by the above method was tested. Among them, the non-metallic inclusions: Class A (sulfide) coarse and fine systems are both level 0.5, Class B (alumina) coarse and fine systems are both level 1.0, Class C (silicate) coarse and fine systems are both level 0, Class D (spherical oxide) coarse and fine systems are both level 1.0, Ds (large-particle spherical oxide) is level 1.0; the annealed structure can reach A2 specified in GB / T35840.3-2018 standard; according to GB / T18254 test, the carbide liquid precipitation is level 0.5; the finish (polishing) reaches A4 (Ra0.063μm); after 48h of acid salt spray test in NaCl solution according to GB / T10125-2021, the defect area is 0.25<A≤0.5, and the appearance grade is 7.

[0102] It can be seen from this comparative example that the metallurgical method of electroslag remelting has limited ability to remove non-metallic inclusions, and during the electroslag remelting process, new inclusions are formed to a certain extent due to the increase in the content of gases such as oxygen, nitrogen and hydrogen, resulting in the purity of the material failing to meet the polishing requirements of mirror and optical surfaces.

[0103] Comparative Example 2

[0104] The corrosion-resistant high-polishing plastic mold steel provided in this comparative example has the following chemical composition and mass percentage: C 0.40%; Si 0.70%; Mn 0.50%; Cr 13.60%; Mo 0.30%; V 0.25%; Ni 0.40%; the rest is Fe and unavoidable impurities.

[0105] The preparation method of corrosion-resistant high-polished plastic mold steel is basically the same as that of Example 1, except that: in step S5, the forging is charged into a furnace and heated to 870°C and kept warm for 6 hours at a thickness of 3h / 100mm, then the temperature is reduced to 690°C at a rate of 15°C / h, and then the furnace is cooled to 480°C and then air-cooled to obtain the mold steel.

[0106] The performance of the corrosion-resistant and highly polished plastic mold steel prepared by the above method was tested. Among them, the non-metallic inclusions: Class A (sulfide) coarse series, Class A (sulfide) fine series, Class B (alumina) coarse series, Class B (alumina) fine series, Class C (silicate) coarse series, Class C (silicate) fine series, Class D (spherical oxide) coarse series, Ds (large-particle spherical oxide) are all level 0, and Class D (spherical oxide) fine series is level 0.5; the annealed structure can reach B2 specified in GB / T35840.3-2018 standard; according to GB / T18254 test, the carbide liquid precipitation is 0; the finish (polishing) reaches A3 (Ra0.032μm); after 48h of acid salt spray test in NaCl solution according to GB / T10125-2021, the defect area is 0.1<A≤0.25, and the appearance grade is 8.

[0107] It can be seen from this comparative example that in step S5, when only high-speed cooling is performed, the uniformity of the microstructure is reduced and the polishing performance is reduced.

[0108] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing corrosion-resistant high-polished plastic mold steel, characterized in that: The preparation method comprises the following steps: S1. Using blast furnace iron, ferroalloy and scrap steel as raw materials, after smelting in alloy melting furnace and electric furnace, LF refining, VD degassing, argon gas protection is used to cast electrode base material; S2, performing vacuum consumable smelting on the electrode base material in a vacuum consumable furnace to obtain a steel ingot; S3, subjecting the steel ingot obtained in step S2 to high temperature homogenization treatment, and then subjecting the steel ingot to multi-directional upsetting forging treatment; S4, performing a solution treatment on the forging obtained in step S3, wherein the solution treatment comprises heating the forging to a solution temperature and keeping the temperature, and then performing alternating water-air cooling to obtain a martensite and lower bainite structure; S5. Perform spheroidizing annealing treatment on the forging obtained in step S4, wherein the spheroidizing annealing treatment comprises charging the forging obtained in step S4 into a furnace, heating it to 850-900°C, keeping it warm, then reducing the temperature to 790-840°C at a rate greater than 10°C / h and not greater than 20°C / h, then reducing the temperature to 660-700°C at a rate ≤10°C / h, then cooling it to ≤500°C in the furnace, and then taking it out of the furnace and air cooling it.

2. The method for preparing corrosion-resistant high-polished plastic mold steel according to claim 1, characterized in that: The phosphorus content of the blast furnace molten iron is not higher than 0.025% by mass, and the total content of lead, arsenic, tin, antimony and bismuth is not greater than 0.025%; and / or, the ferroalloy comprises high carbon ferrochrome, low carbon ferrochrome, ferromolybdenum, ferrovanadium and ferronickel; And / or, the scrap steel includes at least one of medium-sized scrap steel and heavy-sized scrap steel.

3. The method for preparing the corrosion-resistant high-polished plastic mold steel according to claim 1, characterized in that: In step S1, the ferroalloy is melted uniformly in the alloy melting furnace, and the tapping temperature is 1550-1650° C.; and / or, in step S1, the blast furnace molten iron and the scrap steel are melted and dephosphorized by the electric furnace, the phosphorus content is not higher than 0.005wt%, and the tapping temperature is 1600-1680°C; And / or, in step S1, the molten steel from the alloy melting furnace and the electric furnace is added to the LF refining furnace for desulfurization to no more than 0.003wt%, degassing, and removal of inclusions, and adjusted to the required composition; then VD degassing is performed, and the nitrogen content in the molten steel is no more than 70*10 -6 , oxygen content is not more than 10*10 -6 ; And / or, in step S1, after the molten steel is subjected to the VD degassing treatment, the molten steel is poured into the consumable electrode mold of the consumable electrode pouring station by ladle pouring to cast the electrode base material, and the electrode base material is obtained after mold cooling and demolding, wherein the temperature of the molten steel ladle is 1510-1560°C, and the mold cooling time is 2h-8h.

4. The method for preparing the corrosion-resistant high-polished plastic mold steel according to claim 1, characterized in that: In step S1, after obtaining the electrode base material, the electrode base material is subjected to stress relief annealing, wherein the stress relief annealing includes placing the electrode base material into an annealing furnace, heating it to 750-800°C, keeping it warm according to the effective diameter (2-4h) / 100mm, and then cooling it to no higher than 200°C and air cooling it out of the furnace.

5. The method for preparing the corrosion-resistant high-polished plastic mold steel according to claim 4, characterized in that: In step S1, after stress relief annealing is performed on the electrode base material, the electrode base material is subjected to a cutting process and a surface polishing process.

6. The method for preparing corrosion-resistant high-polished plastic mold steel according to claim 1, characterized in that: In step S2, the melting rate of the vacuum consumable melting is controlled at 6.0-12.0 kg / min; and / or, in step S2, shrinkage compensation is started when the remaining electrode base material weight is 3% to 10% of the initial total electrode base material weight; And / or, in step S2, after obtaining the steel ingot, the steel ingot is demolded after cooling in the mold for 1h to 5h and then subjected to stress relief annealing. The stress relief annealing includes placing the steel ingot into an annealing furnace, heating it to 750-800°C, keeping it warm according to the effective diameter (2-4h) / 100mm, cooling it to no higher than 200°C in the furnace and air cooling it out of the furnace.

7. The method for preparing corrosion-resistant high-polished plastic mold steel according to claim 1, characterized in that: In step S3, the high temperature homogenization treatment includes subjecting the steel ingot obtained in step S2 to high temperature homogenization treatment at 1200-1300° C. and keeping the temperature at an effective diameter (2-4h) / 100mm; And / or, in step S3, the multi-directional upsetting forging process includes: cooling the steel ingot after the high-temperature homogenization treatment to 1100-1200°C, using an upper flat plate and a lower platform for multi-directional upsetting forging, with a pressing amount of 20-50% each time, turning 90° to press another plane, pressing the three planes twice in sequence, with a total forging ratio of 6-12, controlling the final forging temperature to 800-900°C, and obtaining a forging.

8. The method for preparing corrosion-resistant high-polished plastic mold steel according to claim 1, characterized in that: In step S4, the solution temperature is 950-1050°C, and the holding time is 2-5h; And / or, in step S4, during the water-air alternating cooling process, water-air alternating cooling is performed twice, the water temperature is not higher than 40°C at the start, the temperature of the forging is reduced to 450-550°C at the first water entry, the forging is air-cooled until the forging is dry at the first water exit, the temperature of the forging is reduced to 250-350°C at the second water entry, the water temperature is not higher than 50°C at the end, and the forging is air-cooled to 100-200°C at the end; And / or, in step S5, the forging obtained in step S4 is charged into a furnace and heated to 850-900°C, and kept warm according to the thickness (3-5h) / 100mm.

9. The method for preparing corrosion-resistant high-polished plastic mold steel according to claim 1, characterized in that: Measured by mass percentage, the corrosion-resistant high-polished plastic mold steel comprises: C 0.35-0.45%, Si 0.50-1.20%, Mn 0.50-1.20%, Cr 12.5-14.5%, Mo 0.20-0.50%, V 0.20-0.50%, Ni 0.30-0.80%, and the rest is Fe and inevitable impurities.

10. A corrosion-resistant high-polished plastic mold steel, characterized in that: The corrosion-resistant high-polished plastic mold steel is prepared by the preparation method described in any one of claims 1-9.

Citation Information

Patent Citations

  • Anti-cavitation age-hardening high-polishability plastic die steel and preparation method thereof

    CN105002433A

  • Preparation method of high-toughness and high-isotropy ZW868 hot work die steel

    CN107488813A

  • Novel corrosion-resistant pressure casting die steel and preparation method thereof

    CN108385021A

  • Plastic die steel with high toughness, high polishing property and corrosion resistance and preparation method thereof

    CN114540703A

  • Steel for hot extrusion die and preparation method thereof

    CN117327882A