Preparation method of smelting crucible for smelting iron-based alloy
By using corundum cylinder protective layer and unequal chamfered structure in the iron-based alloy smelting crucible, combined with the ramming device and the baking and sintering process, the cracks and liquid leakage of the crucible in the high temperature environment are solved, and the crucible is improved Density and service life, and achieve high-quality alloy powder preparation, ensuring the safety and harmless material.
Patent Information
- Application Number
- CN202411174316.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-12-03
AI Technical Summary
Existing iron-based alloy smelting crucibles are prone to cracks, liquid leakage and short service life in high temperature environments, which affect the quality and cost of alloy powders, and traditional materials are harmful to human health.
The corundum tube is used as the protective layer and the unequal chamfered structure, combined with the ramming device and the baking and sintering process, to ensure the density and high strength of the crucible, and form a high-strength sintering layer through semi-automatic knotting and slow baking at low temperatures.
It significantly improves the density and service life of the crucible, reduces the inclusion rate of alloy powder, ensures high-quality iron-based alloy powder preparation, and the material is safe and harmless.
Smart Images

Figure CN119063475A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of smelting furnace construction, and in particular to a method for preparing a smelting crucible for smelting iron-based alloys. Background Art
[0002] At present, the preparation of alloy powder for 3D printing mostly adopts prefabricated melting crucibles. For the preparation of iron-based alloy powder, the melting point of iron-based alloy is relatively high, reaching above 1450℃, and the gas atomization powder making has requirements on the superheat of metal. The melting temperature of iron-based alloy needs to be further improved. The high temperature environment puts forward high requirements on the quality of prefabricated crucibles. Poor quality crucibles are very easy to crack and perforate due to high temperature. For example, if the density of the crucible is not good, it is easy to crack at high temperature, and even leakage occurs during smelting, which leads to its extremely short service life, high furnace building frequency, high labor intensity and low production efficiency. In addition, poor quality crucibles will also affect the purity of alloy solution. For example, when the vibrating material of crucible furnace lining is not tight, the crucible is very easy to crack or the inner surface falls off, and even dry vibrating material will be mixed in the molten metal liquid, which will affect the purity of metal powder, making the quality of iron-based alloy powder for 3D printing poor and the cost high, and the advantages over traditional iron-based parts manufacturing and processing are not obvious. Therefore, there is an urgent need for a method for preparing a high-quality smelting crucible that is suitable for preparing high-quality iron-based alloy powder. Summary of the invention
[0003] The object of the present invention is to provide a method for preparing a smelting crucible for smelting iron-based alloys, which can solve the technical problems mentioned in the above background technology.
[0004] To achieve the above object, the present invention provides the following technical solution: a method for preparing a smelting crucible for smelting an iron-based alloy, comprising the following steps:
[0005] S1 installs the coil;
[0006] S2 Crucible Knotting:
[0007] The coil support base plate is embedded in the bottom of the coil, and a protective layer is placed on the inner wall of the coil;
[0008] Add dry vibration material to the furnace lining and ram it. After ramming to a predetermined height, put it into an iron mold, the iron mold is coaxial with the coil of the medium frequency melting furnace, continue to add dry vibration material to the furnace lining, tie the side wall of the crucible, and the intersection corner of the side wall of the crucible and the bottom of the crucible is a chamfered structure;
[0009] S3 crucible baking and sintering.
[0010] In a preferred embodiment, the protective layer is a corundum tube. Using a high-hardness corundum tube as the protective layer can prevent the dry vibration material from penetrating into the coil turns and causing displacement, thereby ensuring that the density of the crucible does not change.
[0011] In a preferred embodiment, the chamfer structure at the intersection corner of the crucible side wall and the crucible bottom is constructed as an unequal chamfer, the long side of the unequal chamfer corresponds to the direction of the crucible side wall, and the short side of the unequal chamfer corresponds to the direction of the crucible bottom. This structural setting can make the molten steel pressure borne by the chamfer position deviate to the direction of the crucible side wall, thereby effectively sharing the pressure at the bottom of the crucible. In addition, the corundum tube protective layer is provided on the outside of the crucible wall with high-strength support, which can prevent the dry vibration material from seeping outward under high pressure. The pressure of the molten steel and the force of the corundum tube cooperate with each other to further improve the density of the crucible.
[0012] In a preferred embodiment, a ramming device is used to ram the dry vibration material of the furnace lining, the ramming device includes a support part, a driving part and a ramming part, the support part includes a leg and a ring frame connected to the top of the leg, the driving part includes a pneumatic pick slidably connected to the ring frame, and the ramming part includes a rod connected to the bottom end of the pneumatic pick and a flat hammer connected to the end of the rod. The ramming device can realize semi-automatic knotting of the crucible, effectively improve the knotting uniformity, and improve the working efficiency.
[0013] In a preferred embodiment, a vibrating fork is connected to one side of the flat hammer, and the vibrating fork is higher than the surface of the flat hammer. The vibrating fork can make the layers of vibrated materials more closely connected, prevent stratification during the ramming process, and improve its density.
[0014] In a preferred embodiment, the height of the vibrating fork above the flat hammer surface should be set to 1 / 3-1 / 4 of the feeding height. This setting can ensure the connection strength between the layers of vibrating materials without affecting the compaction effect. Setting it too low will affect the connection strength, and setting it too high will affect the compaction effect.
[0015] In a preferred embodiment, during the melting process of the S3 iron material, the molten iron occupies more than 90% of the volume of the crucible, so as to avoid excessive temperature difference between the upper and lower parts and thermal stress causing cracking and peeling of the furnace lining.
[0016] In a preferred embodiment, S3 crucible baking and sintering comprises the following steps:
[0017] Heat the charge to 1000-1100℃ at a uniform heating rate and keep it warm;
[0018] After the heat preservation is completed, the temperature is continuously raised to 1620-1660°C at a uniform speed to melt the iron material, and the temperature is kept to sinter the inner surface of the crucible;
[0019] After the insulation is completed, impurities in the molten metal are removed and the furnace is vacuumed.
[0020] In a preferred embodiment, in S3, the charge is heated to 1000-1100°C at a heating rate of 250±10°C / h, and the temperature is increased at a uniform rate in the early stage to remove the free water vapor in the knotted dry vibration material and the moisture inside the coil glue. If the heating is slow, it will take a long time. If the heating is too fast, the consistency of the heating rate around the crucible cannot be guaranteed, which affects the discharge of water vapor. The crucible wall is also prone to thermal stress. The inner surface of the crucible is prone to peeling in the later stage, which affects the purity of the alloy. The charge is heated to 1620-1660°C at a heating rate of 200±10°C / h. If the heating is slow, it will take a long time. If the heating is too fast, the consistency of the heating rate around the crucible cannot be guaranteed. The temperature of the material at different positions is prone to temperature difference, which affects the uniformity of the sintering effect.
[0021] Another aspect of the present invention provides a technical solution for a smelting crucible, which is prepared by the preparation method described in any of the above solutions.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] 1. The present invention adopts a corundum tube protective layer to replace the traditional asbestos cloth, which not only does not cause harm to the user's body, but also can prevent the dry vibration material from penetrating into the coil turns and causing displacement, thereby ensuring that the density of the crucible does not change; at the same time, by setting the intersection corner structure of the crucible bottom and the crucible wall as a chamfered structure, the crucible can be effectively prevented from cracking, and by further setting the chamfer as an unequal chamfer, the molten steel pressure borne by the chamfered position can be biased toward the direction of the crucible side wall, thereby effectively sharing the pressure at the bottom of the crucible, and cooperating with the corundum tube protective layer to provide high-strength support on the outside of the crucible wall, it can prevent the dry vibration material from seeping outward under high pressure, and the pressure of the molten steel and the force of the corundum tube can cooperate with each other to further improve the density of the crucible.
[0024] 2. The ramming device can realize semi-automatic knotting of the crucible, effectively improve the knotting uniformity and improve the working efficiency. By setting a pneumatic pick with radial position adjustment, a height-adjustable ramming part and a vibrating fork, the connection between each layer of the vibrating material can be made tighter, preventing stratification during the ramming process, and further ensuring the uniformity of the ramming and the density of the crucible.
[0025] 3. In the baking and sintering process, slow baking at low temperature in a non-vacuum environment and high-temperature full-furnace sintering can ensure the formation of a high-strength sintered layer, improve the density of the crucible, and reduce the mixing of dry vibration materials. Combined with the removal of nitrogen and oxygen in a vacuum environment, the purity of the alloy solution can be further improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 Schematic diagram of the simulated structure of a melting crucible in an embodiment of the present invention;
[0027] Figure 2 It is a schematic diagram of the overall structure of the ramming device in the embodiment of the invention;
[0028] Figure 3 yes Figure 2 Bottom view of the A part;
[0029] Figure 4 yes Figure 2 Bottom view of the B part;
[0030] Figure 5 Schematic diagram of the matching structure of the furnace collar and the furnace nozzle in the embodiment of the present invention;
[0031] Figure 6 This is a temperature rise curve of crucible baking and sintering in an embodiment of the present invention.
[0032] The meaning of each number in the figure is:
[0033] 1. Support part; 11. Support leg; 12. Ring frame; 2. Driving part; 21. Sliding part; 22. Pneumatic pick connecting plate; 23. Pulley connecting plate; 24. Long hole; 25. Pneumatic pick; 3. Ramming part; 31. Rod; 32. Flat hammer; 33. Vibrating fork; 34. Adapter plate; 4. Furnace collar; 5. Furnace nozzle; 6. Corundum tube; 7. Iron mold; 8. Iron ingot; 9. Coil; 10. Support bottom plate; 101. Unequal chamfer. DETAILED DESCRIPTION
[0034] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0035] In the description of the present invention, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as limiting the present invention.
[0036] refer to Figure 1 The present invention provides a method for preparing a smelting crucible for smelting an iron-based alloy, comprising the following steps:
[0037] S1 installing coil 9 and protecting coil 9: using coil putty to protect the outer surface of the smelting coil 9.
[0038] The smelting coil 9 is installed in the medium frequency smelting furnace, and the outer surface of the smelting coil 9 is protected by coil putty. By evenly applying the coil putty on the inner and outer surfaces of the coil 9, it can play an insulating role, effectively prevent the coil 9 from igniting due to aging of the coil 9 and metal impurities, and buffer the expansion and contraction of the working lining.
[0039] Specifically, add 6-10% water to the coil glue and stir evenly. Excessive water will reduce the strength of the glue and easily cause cracks. The amount of water added can be adjusted appropriately according to the actual use. Spread the coil glue evenly so that the glue is embedded in the turns of the coil 9. The coating thickness is 6-8mm. The surface should be smooth and flat. Ensure that the glue layer and the coil 9 are concentric. Dry naturally for more than 72 hours, or bake at low temperature for more than 10 hours at 20-30℃ to slowly evaporate the moisture of the coil glue so that the coil glue is fixed and does not peel off. If the moisture evaporates too quickly, it will easily cause the coil glue to crack.
[0040] The baking of the coil cement can be carried out simultaneously with the baking of the crucible, so as to ensure that the coil cement on the surface of the induction coil 9 is in a completely solidified and dry state.
[0041] S2 Crucible Knotting:
[0042] S2.1 Embed the coil support base plate 10 into the bottom of the coil 9 as the bottom support of the coil 9. The diameter of the coil support base plate 10 is consistent with the outer diameter of the coil 9 and the thickness is 20-30 mm, which depends on the supporting weight;
[0043] S2.2 A protective layer is placed on the inner wall of the coil 9. The protective layer is preferably a corundum tube 6 with a thickness of 20-25mm, and the gap between the coil 9 and the corundum tube 6 is filled with coil glue. Compared with the traditional asbestos cloth, the corundum tube 6 structure has better safety performance and will not cause harm to the user's body. On the other hand, by adopting the protective layer of the corundum tube 6, it is possible to avoid damage to the induction coil 9 caused by the vibrating hammer fork during the subsequent vibration process, and it is also possible to prevent the dry vibration material from seeping out of the coil 9 from the gaps between the turns of the coil 9 and the bottom gaps during the vibration process. In addition, the traditional asbestos cloth is relatively soft. During long-term use, the dry vibration material will penetrate into the direction of the asbestos cloth, thereby affecting the density of the crucible. By using the corundum tube 6 with a sufficiently high hardness as a protective layer, the infiltration of the dry vibration material can be prevented, ensuring that the density of the crucible does not change.
[0044] The coil support base plate 10 is also made of high-strength material, such as asbestos board or corundum. During the vibration process, the high-strength asbestos board can provide high-strength support to the ramming material and cooperate with the applied vibration force to generate interaction force, thereby improving the ramming density of the dry vibration material.
[0045] S2.3 Dry knotting:
[0046] Add dry vibration material to the lining of the medium frequency melting furnace for ramming process, ram to a predetermined height, put the iron mold 7 in after leveling, the iron mold 7 should be kept coaxial with the coil 9, and the top of the iron mold 7 is flush with the top of the coil 9. The predetermined height should be set at least to the position of the second turn of the coil 9 at the bottom, so that it has sufficient thickness to ensure that the temperature at the bottom of the crucible is not too low to prevent the phenomenon of steel solidification. In practical applications, the medium frequency furnace induction coil 9 generates dense magnetic lines of force, which generates induced eddy currents and heats up the ferromagnetic material to achieve the purpose of heating the material. The bottom of the crucible should be higher than the bottom induction coil by more than two turns, at least level, otherwise the temperature at the bottom is too low, which will cause poor melting of molten steel. On the other hand, under the continuous erosion of molten steel, the bottom of the crucible that is too thin is prone to leakage, posing a safety hazard.
[0047] It should be noted that the bottom of the crucible bears the static pressure of the entire molten steel, especially the intersection corner of the crucible bottom and the crucible wall is the weakest link of the crucible. It is not easy to tamp evenly when tying a knot at this location. In addition, the thickness of the crucible sand here varies greatly, and the heat dissipation conditions are different. Sintering cracks are easily generated at the corner under high-temperature smelting environment, resulting in steel leakage. Therefore, the intersection corner position of the crucible bottom and the crucible wall requires a higher knotting quality.
[0048] In the present invention, the intersection corner structure of the crucible bottom and the crucible wall is set to a chamfered structure, such as Figure 1 As shown, the chamfer is set to form a buffer between the bottom of the crucible and the crucible wall, avoiding uneven heat dissipation due to sudden changes in thickness. The chamfer can also increase the force-bearing area of the position, making it less prone to cracking. Preferably, the chamfer is constructed as an unequal chamfer 101, the long side of the unequal chamfer 101 corresponds to the direction of the side wall of the crucible, and the short side of the unequal chamfer 101 corresponds to the direction of the bottom of the crucible. The structural setting can make the molten steel pressure borne by the chamfer position deviate to the direction of the crucible wall, which can effectively share the pressure at the bottom of the crucible. In addition, the protective layer of the corundum tube 6 is provided on the outside of the crucible wall with high-strength support, which can prevent the dry vibration material from seeping outward under high pressure. The pressure of the molten steel and the force of the corundum tube 6 cooperate with each other to further improve the density of the crucible.
[0049] The following is combined again Figure 1The specification parameters of the unequal chamfer 101 are further described in detail. In the present invention, the length m of the short side in the unequal chamfer 101 is set to be between 0.10d<m<0.15d, and d is the inner diameter of the crucible. Within this range, the chamfer size is appropriate, which not only ensures that the chamfer can provide sufficient buffer, but also ensures the capacity of the crucible, avoids the impact of excessive cutting angle on the crucible capacity, and the bottom stability can also be guaranteed. Among them, the angle α between the short side and the third side of the chamfer is set between 50°-65°. This angle setting can effectively deviate the molten steel pressure borne by the chamfer position toward the direction of the crucible side wall, thereby sharing the pressure at the bottom of the crucible. If the angle is set too small, the pressure of the molten steel cannot be effectively shared. If the angle is set too large, it will affect the capacity of the crucible, and it is also easy to form sharp corners, increasing the risk of sintering cracks.
[0050] In order to improve the ramming quality, a ramming device is used to tie knots in batches:
[0051] S2.3.1 Knotting of crucible bottom
[0052] Add dry vibration material to the furnace lining in batches for knotting. The height of the first layer of material at the bottom of the crucible is 40-60mm. Use the flat hammer of the ramming device to punch and automatically ram evenly along the circular track of the coil 9. The overlapping area of two adjacent ramming tracks is 20-30%. The pulley moves forward for one circle and then moves in the reverse direction. Ramming in the forward and reverse directions, ramming 2-4 circles for each track. After that, add 30-40mm of dry vibration material per layer, repeat the ramming steps to knot to the position of the preset chamfer height.
[0053] like Figure 2-Figure 4 As shown, the ramming device involved in the present invention includes a supporting part 1, a driving part 2 and a ramming part 3, the supporting part 1 includes a plurality of legs 11 and an annular frame 12 connected to the top of the legs 11, the annular frame 12 is constructed as an annular guide rail structure that roughly matches the diameter of the induction coil 9, and the driving part 2 is slidably connected to the annular guide rail.
[0054] Specifically, the driving unit 2 includes a pneumatic pick 25 and an electric hoist pulley 21. The top of the pneumatic pick 25 is slidably connected to the annular guide rail through the electric hoist pulley 21. The top of the pneumatic pick 25 is fixedly connected with a pneumatic pick connecting plate 22, and the bottom of the electric hoist pulley 21 is connected with a pulley connecting plate 23. The pneumatic pick connecting plate 22 is connected to the pulley connecting plate 23, and then the pneumatic pick 25 is driven to perform annular motion through the electric hoist pulley. The pulley connecting plate 23 is provided with a long hole 24 along the radial direction of the annular guide rail. By adjusting the installation position of the pneumatic pick connecting plate 22 in the long hole 24, the radial position of the pneumatic pick 25 can be adjusted to change its knotting trajectory so that it can match the ramming requirements of different positions and achieve a more uniform ramming effect.
[0055] In the present device, the ramming part 3 includes a rod 31 and a flat hammer 32 fixedly connected to the end of the rod 31. The rod 31 is detachably connected to the bottom end of the pneumatic jackhammer 25. The diameter of the hammer head of the flat hammer 32 is set according to the distance between the outer wall of the crucible and the inner wall of the furnace. Figure 1 and Figure 3 In order to strengthen the connection between the layers of vibrating materials and prevent stratification during the ramming process, the ramming part 3 further includes a ramming fork 33 fixedly connected to one side of the flat hammer 32, and the ramming fork 33 is fixedly connected to one side of the flat hammer 32 through an adapter plate 34. Figure 4 The vibrating fork 33 is constructed as a plurality of fork-shaped protrusions fixedly connected to a mounting plate. The vibrating fork 33 should be slightly higher than the surface of the flat hammer 32, and is used to fork the surface of the dry vibrating material punched by the flat hammer 32 to increase the connection between the layers of vibrating material. To ensure the connection strength between the vibrating fork 33 and the flat hammer 32, the two ends of the adapter plate 34 are respectively connected to the flat hammer 32 and the mounting plate by welding. To ensure the connection strength between the layers of vibrating material and not affect the compaction effect, the height of the vibrating fork 33 above the surface of the flat hammer 32 should be set to 1 / 3-1 / 4 of the feeding height. Setting it too low will affect the connection strength, and setting it too high will affect the compaction effect.
[0056] In the present device, the height of the ramming part 3 is adjustable to adapt to the changing height of the feeding material, thereby further ensuring the ramming effect.
[0057] By adopting the ramming device provided by the present invention, semi-automatic knotting of the crucible can be achieved, the knotting uniformity can be effectively improved, and the working efficiency can be improved. By providing a pneumatic jackhammer 25 with radial position adjustment, a height-adjustable ramming part 3, and a vibrating fork 33, the connection between each layer of the vibrated material can be made tighter, stratification can be prevented during the ramming process, and the uniformity and density of the ramming can be further ensured.
[0058] S2.3.2 Knotting of crucible wall
[0059] Use a flat shovel to shovel out the bottom space and chamfered structure of the crucible, install the iron mold 7 to the bottom of the crucible, continue to add the dry vibration material of the furnace lining, and start to tie the side wall of the crucible. It is understandable that the spacing between the outer wall of the iron mold 7 and the corundum tube 6 is the thickness of the side wall of the crucible. Because the side wall of the crucible shares a certain bottom pressure and bears the reaction force from the corundum tube 6, it is necessary to set the thickness of the side wall of the crucible to between 2.5-3 times the thickness of the side wall of the corundum tube 6. This thickness enables the side wall of the crucible to have sufficient strength to share the pressure of the molten steel, and the density can be further improved under the interaction of the pressure of the molten steel and the force of the corundum tube 6. If the thickness of the side wall of the crucible is set too thin, leakage will occur under the continuous erosion of the molten steel, thereby affecting the service life of the crucible. The side wall of the crucible cannot be set too thick to avoid affecting the induction heating of the coil 9.
[0060] Fix the matching iron mold 7 to the bottom of the crucible, and put the alloy ingot or other heavy objects into the iron mold 7 to press it tightly to prevent the iron mold 7 from moving when the furnace is fired. The operation of knotting the side wall of the crucible is the same as that of knotting the bottom of the crucible. The layered knotting method is still used, and each layer is added with 30-40mm. The knots are tied tightly layer by layer. When the knot height is 30-40mm from the top of the coil 9, the furnace collar 4 and the furnace nozzle 5 are installed.
[0061] S2.3.3 Install the furnace collar 4 and furnace nozzle 5
[0062] Spray alcohol on the knotted dry vibration material to moisten it, first install the prefabricated furnace collar 4, then install the prefabricated furnace nozzle 5, the matching structure of the two is as follows Figure 5 As shown, different parts are bonded and transitioned by plastic refractory materials. The prefabricated furnace collar 4 and furnace nozzle 5 are both formed by high-pressure pressing of refractory materials and sintered at high temperature, and have high strength and high temperature resistance.
[0063] S3 crucible baking and sintering
[0064] Baking and sintering are slow baking at low temperature in a non-vacuum environment, sintering in a full furnace at high temperature, and removing nitrogen and oxygen in a vacuum environment. By calculating the height of the molten metal after the feeding and melting in advance, the appropriate furnace collar 4 height is installed in advance to ensure full furnace sintering, that is, the height of the sintered steel liquid must be at least the same as the height of the rammed dry vibration material to achieve complete sintering of the dry vibration material. The purpose of baking and sintering the crucible furnace lining is to fully remove the moisture in the furnace lining, and finally sinter it at high temperature into a dense layer with high strength. There is no pause between the baking furnace and the first furnace smelting, and continuous full furnace opening for more than 2-3 furnaces is conducive to the formation of a sufficiently thick sintering layer.
[0065] After the furnace is finished and the molten iron is poured out, the sintered layer on the inner surface of the crucible is relatively thin. Continuous production of 2-3 furnaces can increase the thickness and strength of the sintered layer. The inner surface temperature of the crucible that has just been sintered is relatively high, and the sintered layer is relatively thin. Continuous production can keep the sintered layer at a high temperature all the time, and the water vapor in the air will not corrode the crucible. The quality of the sintered crucible is relatively stable. If the furnace is stopped after sintering, the crucible will be corroded by the water vapor in the air after cooling down. If it is heated again in subsequent production, the thermal expansion and contraction of the crucible that has just been baked and the erosion of water vapor will reduce the service life of the crucible.
[0066] The specific steps include:
[0067] S3.1 One-time heating
[0068] Heat the charge to 1050±50℃ at a heating rate of 250±10℃ / h and keep it at this temperature for 1h. During the heating period, use dual colorimetric infrared temperature measurement to confirm the oven temperature. Adjust the power according to the temperature and maintain the heating curve of the oven process, such as Figure 6 shown.
[0069] In the early stage, the temperature is raised at a uniform rate to remove the free water vapor in the knotted dry vibration material and the moisture inside the coil glue. If the temperature rises slowly, it will take a long time. If the temperature rises too quickly, the consistency of the heating rate around the crucible cannot be guaranteed, which affects the discharge of water vapor. The crucible wall is also prone to thermal stress. The inner surface of the crucible is prone to peeling in the later stage, which affects the purity of the alloy. The reason why it stays at around 1050°C is that this temperature does not reach the melting point of the iron mold 7 and the iron ingot 8 of the baking furnace charge, and will not melt the iron mold 7. It can thoroughly achieve the drying effect and also shape the dry vibration material close to the outer surface of the iron mold 7, ensuring that when the iron mold 7 melts in the next step, the dry vibration material will not immediately collapse or fall off, so as to avoid mixing the dry vibration material into the alloy solution. It should be noted that the crucible specifications above 500kg need to be kept warm for 2-5 hours.
[0070] 3.2 Secondary heating
[0071] After the insulation is finished, continue to heat up at a uniform speed, and heat the charge to 1640±20℃ at a heating rate of 200±10℃ / h to prepare for melting the iron. It is advisable that the molten iron occupies more than 90% of the crucible volume to avoid excessive temperature difference between the upper and lower parts, and thermal stress causing cracking and peeling of the furnace lining. During the secondary heating process, the temperature is raised at a uniform rate of 200℃ / h. If the heating is slow, it will take a long time. If the heating is too fast, the consistency of the heating rate around the crucible cannot be guaranteed. The temperature of the material at different positions is prone to temperature difference, which affects the uniformity of the sintering effect.
[0072] The molten iron in the crucible is kept at a temperature of 1640±20℃ for 1-1.2h to continuously sinter the inner surface of the crucible, so that a relatively complete glaze layer is formed on the inner surface of the crucible to resist the erosion of the molten metal liquid.
[0073] It should be noted that the heating power of the drying furnace and the first two furnaces should be 70%-80% of the full power. In the initial stage of use, the sintering layer is relatively thin, and excessive electromagnetic stirring can easily damage the furnace lining.
[0074] S4 Atomized Metal Liquid Treatment
[0075] After the insulation is completed, a slag-forming agent is added to the surface of the molten metal for slag-forming and slag-stripping treatment to reduce non-metallic inclusions in the molten metal and improve its purity. After the slag stripping is completed, the furnace cover is closed and vacuum is drawn to remove the oxygen and nitrogen content of the molten steel. The molten metal is kept warm by maintaining half power (high voltage, high vacuum coil 9 is easy to discharge) until it is evacuated to the ultimate vacuum (within 10 Pa). The ultimate vacuum state is maintained for more than 15 minutes, and then the protective gas is quickly filled. The temperature is raised to 70%-80% of the full power to the pouring temperature for atomization and powder making. Before closing the furnace, impurity adsorption cakes or balls can be added to the surface of the alloy liquid to adsorb and agglomerate oxide impurities that float to the surface again due to electromagnetic stirring during the vacuuming period.
[0076] The present invention is further described in detail below in conjunction with the embodiments. It should also be understood that the following embodiments are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by technicians in this field based on the above content of the present invention all belong to the scope of protection of the present invention.
[0077] Example 1
[0078] The method for preparing a smelting crucible for smelting an iron-based alloy provided in this embodiment comprises the following steps:
[0079] S1 installing coil 9 and protecting coil 9: using coil putty to protect the outer surface of the smelting coil 9.
[0080] The smelting coil 9 is installed in the medium frequency smelting furnace, and the outer surface of the smelting coil 9 is protected by coil cement.
[0081] S2 Crucible Knotting:
[0082] S2.1 Insert the coil 9 support base plate 10 into the bottom of the coil 9. The diameter of the coil 9 support base plate 10 is consistent with the outer diameter of the coil 9, the thickness is 30mm, and the material is asbestos board;
[0083] S2.2 A protective layer of a 25 mm thick corundum tube 6 is placed on the inner wall of the coil 9, and the gap between the coil 9 and the corundum tube 6 is filled with coil glue.
[0084] S2.3 Dry knotting:
[0085] S2.3.1 Knotting of crucible bottom
[0086] Add dry vibration materials to the lining of the medium frequency melting furnace in batches for knotting. The height of the first layer of material at the bottom of the crucible is 50mm. Use the flat hammer of the ramming device to punch and automatically ram along the circular track of the coil 9. The overlapping area of two adjacent ramming tracks is 30%. The pulley moves forward for one circle and then moves in the reverse direction. Ramming in the forward and reverse directions, ramming 2 circles for each track. After that, add 30mm of dry vibration materials for each layer, repeat the ramming steps to tie the knot to the position of the preset chamfer height.
[0087] S2.3.2 Knotting of crucible wall
[0088] Use a flat shovel to shovel out the bottom space and chamfer structure of the crucible. The chamfer structure is an unequal chamfer 101. The long side of the unequal chamfer 101 corresponds to the direction of the crucible wall, and the short side of the unequal chamfer 101 corresponds to the direction of the bottom of the crucible. The angle α between the short side and the third side of the chamfer is set at 65°. After fixing the matching iron mold 7 to the bottom of the crucible, continue to add dry vibration material to the furnace lining, and start knotting the side wall of the crucible. The alloy ingot is loaded into the iron mold 7 and pressed tightly to prevent the iron mold 7 from moving during the furnace. The preset thickness of the crucible side wall is 62.5mm. The layered knotting method is used to knot the side wall of the crucible. Each layer is added with 30mm, and the knots are tied tightly layer by layer. When the knotting height is 40mm from the top of the coil 9, the installation operation of the furnace collar 4 and the furnace nozzle 5 is transferred.
[0089] S2.3.3 Install the furnace collar 4 and furnace nozzle 5
[0090] Spray alcohol on the knotted dry vibration material to moisten it, first install the prefabricated furnace collar 4, then install the prefabricated furnace nozzle 5, use plastic refractory materials to bond and transition between different components, the prefabricated furnace collar 4 and the furnace nozzle 5 are both formed by high-pressure pressing of refractory materials and sintered at high temperature, and have high strength and high temperature resistance.
[0091] S3 crucible baking and sintering
[0092] S3.1 One-time heating
[0093] The charge was heated to 1050°C at a heating rate of 250°C / h and kept at this temperature for 1h. During the heating period, dual-colorimetric infrared temperature measurement was used to confirm the furnace temperature, and the power was adjusted according to the temperature to maintain the heating curve of the furnace baking process.
[0094] S3.2 Secondary heating
[0095] After the insulation is finished, the temperature is raised at a uniform rate, and the charge is heated to 1640℃ at a heating rate of 200℃ / h to prepare for melting the iron. The molten iron occupies more than 90% of the crucible volume to avoid excessive temperature difference between the upper and lower parts, and thermal stress causing cracking and peeling of the furnace lining. The molten iron in the crucible is kept at 1640℃ for 1h to continuously sinter the inner surface of the crucible, so that a relatively intact glaze layer is formed on the inner surface of the crucible.
[0096] The heating power produced by the drying furnace and the first two furnaces is about 70% of the full power.
[0097] S4 Atomized Metal Liquid Treatment
[0098] After the insulation is completed, a slag-forming agent is added to the surface of the molten metal for slag-forming and slag-stripping treatment to reduce non-metallic inclusions in the molten metal and improve its purity. After the slag stripping is completed, the furnace cover is closed and vacuum is drawn to remove the oxygen and nitrogen content of the molten steel. The molten metal is kept warm at half power until it is vacuumed to the ultimate vacuum (within 10 Pa). The ultimate vacuum state is maintained for more than 15 minutes, and then the protective gas is quickly filled. The temperature is raised to 70% of the full power to the pouring temperature for atomization and powdering. Before the furnace is closed, an impurity adsorption cake is added to the surface of the alloy liquid to adsorb and aggregate oxide impurities that float to the surface again due to electromagnetic stirring during vacuuming.
[0099] Example 2
[0100] The method for preparing a smelting crucible for smelting an iron-based alloy provided in this embodiment comprises the following steps:
[0101] S1 installs coil 9 and coil 9 protection:
[0102] The smelting coil 9 is installed in the medium frequency smelting furnace, and the outer surface of the smelting coil 9 is protected by coil cement.
[0103] S2 Crucible Knotting:
[0104] S2.1 Insert the coil 9 support base plate 10 into the bottom of the coil 9. The diameter of the coil 9 support base plate 10 is consistent with the outer diameter of the coil 9, the thickness is 20mm, and the material is asbestos board;
[0105] S2.2 A protective layer of a 20 mm thick corundum tube 6 is placed on the inner wall of the coil 9, and the gap between the coil 9 and the corundum tube 6 is filled with coil glue.
[0106] S2.3 Dry knotting:
[0107] S2.3.1 Knotting of crucible bottom
[0108] Add dry vibration materials to the lining of the medium frequency melting furnace in batches for knotting. The height of the first layer of material at the bottom of the crucible is 60mm. Use the flat hammer of the ramming device to punch and automatically ram along the circular track of the coil 9. The overlapping area of two adjacent ramming tracks is 20%. The pulley moves forward for one circle and then moves in the reverse direction. Ramming in the forward and reverse directions, ramming 3 circles for each track. After that, add 40mm of dry vibration materials per layer, repeat the ramming steps to tie the knot to the position of the preset chamfer height.
[0109] S2.3.2 Knotting of crucible wall
[0110] Use a flat shovel to shovel out the bottom space and chamfer structure of the crucible. The chamfer structure is an unequal chamfer 101. The long side of the unequal chamfer 101 corresponds to the direction of the crucible wall, and the short side of the unequal chamfer 101 corresponds to the direction of the bottom of the crucible. The angle α between the short side and the third side of the chamfer is set at 50°. After fixing the appropriate iron mold 7 to the bottom of the crucible, continue to add dry vibration material to the furnace lining, and start knotting the side wall of the crucible. The alloy ingot is loaded into the iron mold 7 and pressed tightly to prevent the iron mold 7 from moving during the furnace. The preset thickness of the crucible side wall is 75mm. The layered knotting method is used to knot the side wall of the crucible. Each layer is added with 30mm, and the knots are tied tightly layer by layer. When the knotting height is 30mm from the top of the coil 9, the installation operation of the furnace collar 4 and the furnace nozzle 5 is transferred.
[0111] S2.3.3 Install the furnace collar 4 and furnace nozzle 5
[0112] Spray alcohol on the knotted dry vibration material to moisten it, first install the prefabricated furnace collar 4, then install the prefabricated furnace nozzle 5, use plastic refractory materials to bond and transition between different components, the prefabricated furnace collar 4 and the furnace nozzle 5 are both formed by high-pressure pressing of refractory materials and sintered at high temperature, and have high strength and high temperature resistance.
[0113] S3 crucible baking and sintering
[0114] S3.1 One-time heating
[0115] The charge was heated to 1050°C at a heating rate of 255°C / h and kept at this temperature for 1h. During the heating period, dual-colorimetric infrared temperature measurement was used to confirm the furnace temperature, and the power was adjusted according to the temperature to maintain the heating curve of the furnace baking process.
[0116] S3.2 Secondary heating
[0117] After the insulation is finished, the temperature is raised at a uniform rate, and the charge is heated to 1660℃ at a heating rate of 210℃ / h to prepare for melting the iron. The molten iron occupies more than 90% of the crucible volume to avoid excessive temperature difference between the upper and lower parts, and thermal stress causing cracking and peeling of the furnace lining. The molten iron in the crucible is kept at 1660℃ for 1h to continuously sinter the inner surface of the crucible, so that a relatively intact glaze layer is formed on the inner surface of the crucible.
[0118] The heating power produced by the drying furnace and the first two furnaces is about 70% of the full power.
[0119] S4 Atomized Metal Liquid Treatment
[0120] After the insulation is completed, a slag-forming agent is added to the surface of the molten metal for slag-forming and slag-stripping treatment to reduce non-metallic inclusions in the molten metal and improve its purity. After the slag stripping is completed, the furnace cover is closed and vacuum is drawn to remove the oxygen and nitrogen content of the molten steel. The molten metal is kept warm at half power until it is vacuumed to the ultimate vacuum (within 10 Pa). The ultimate vacuum state is maintained for more than 15 minutes, and then the protective gas is quickly filled. The temperature is raised to 70% of the full power to the pouring temperature for atomization and powdering. Before the furnace is closed, an impurity adsorption cake is added to the surface of the alloy liquid to adsorb and aggregate oxide impurities that float to the surface again due to electromagnetic stirring during vacuuming.
[0121] Comparative Example 1
[0122] The preparation method of the smelting crucible for smelting iron-based alloy provided in Comparative Example 1 is substantially the same as that in Example 1, and therefore, for the sake of brevity, only the differences are described in detail herein.
[0123] In comparative example 1, S2.2 the protective layer inserted into the inner wall of the coil 9 is asbestos cloth, and the appropriately cut asbestos cloth is laid on the inner wall of the coil 9.
[0124] Comparative Example 2
[0125] The preparation method of the smelting crucible for smelting iron-based alloy provided in Comparative Example 2 is substantially the same as that in Example 1, and therefore, for the sake of brevity, only the differences are described in detail herein.
[0126] In comparative example 2, S2.3 is dry knotting to knot the corner structure at the junction of the crucible bottom and the crucible wall into a right-angle structure.
[0127] Comparative Example 3
[0128] The preparation method of the smelting crucible for smelting iron-based alloy provided in Comparative Example 3 is substantially the same as that in Example 1, and therefore, for the sake of brevity, only the differences are described in detail herein.
[0129] In comparative example 3, in S2.2, the protective layer inserted into the inner wall of the coil 9 is asbestos cloth, and the appropriately cut asbestos cloth is laid on the inner wall of the coil 9; and in S2.3, in the dry knotting step, the junction corner structure of the crucible bottom and the crucible wall is knotted into a right-angle structure.
[0130] Comparative Example 4
[0131] The preparation method of the smelting crucible for smelting iron-based alloy provided in Comparative Example 4 is substantially the same as that in Example 1, and therefore, for the sake of brevity, only the differences are described in detail herein.
[0132] In comparative example 4, S2.3 dry knotting, in the unequal chamfer 101, the angle α between the short side and the third side of the chamfer is set at 46°.
[0133] Comparative Example 5
[0134] The preparation method of the smelting crucible for smelting iron-based alloy provided in Comparative Example 5 is substantially the same as that in Example 1, and therefore, for the sake of brevity, only the differences are described in detail herein.
[0135] In comparative example 5, S2.3 dry knotting, the preset crucible side wall thickness, that is, the distance between the outer wall of the iron mold 7 and the corundum tube 6 is 50 mm.
[0136] Purity parameters of the melting crucibles and alloy powders prepared in Example 1, Example 2 and Comparative Examples 1 to 5 are shown in Table 1:
[0137] Table 1
[0138]
[0139] From the above data we can see that:
[0140] In Comparative Example 1, the inner wall of the coil uses asbestos cloth as a protective layer. During long-term use, the dry vibration material will penetrate into the asbestos cloth, thereby affecting the density of the crucible, and the powder inclusion rate is high;
[0141] In Comparative Example 2, the intersection corner structure of the crucible bottom and the crucible side wall is knotted into a right-angle structure, the thickness of the crucible side wall and the bottom varies greatly, the heat dissipation conditions are different, and sintering cracks are easily generated in a high-temperature smelting environment;
[0142] In Comparative Example 3, asbestos cloth is used as a protective layer, and the corner structure of the crucible bottom and the crucible wall is tied into a right-angle structure, which not only easily causes sintering cracks in the crucible, but also makes the dry vibration material loose and seeping out during long-term use, which has a great impact on the density and life of the crucible, and has a great impact on the purity of the powder;
[0143] In comparative example 4, in the unequal chamfer 101, the angle α between the short side and the third side of the chamfer is set too small, so the crucible side wall and the corundum tube 6 cannot effectively share the pressure of the molten steel, which will have a certain impact on the density of the sintered layer;
[0144] In Comparative Example 5, the preset crucible side wall thickness is too thin to withstand the continuous erosion of the molten steel, thereby affecting its service life.
[0145] The melting crucible prepared by the preparation method of Example 1 and Example 2 adopts a corundum tube protective layer and an unequal chamfer 101 structure, and cooperates with a baking and sintering process. The density of the sintered layer of the melting crucible prepared and the quality of the crucible are significantly higher than those of the comparative examples, thereby effectively improving the service life of the melting crucible. Correspondingly, the inclusion rate of the alloy powder prepared by the melting crucible is also lower.
[0146] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited by the above embodiments. The above embodiments and descriptions are only preferred examples of the present invention and are not intended to limit the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention. The scope of protection of the present invention is defined by the attached claims and their equivalents.
Claims
1. A method for preparing a smelting crucible for smelting an iron-based alloy, characterized in that: The following steps are involved: S1 coil protection; S2 Crucible Knotting: The coil support base plate is embedded in the bottom of the coil, and a protective layer is placed on the inner wall of the coil; Add dry vibration material to the furnace lining and ram it. After ramming to a predetermined height, put it into an iron mold, and the iron mold is coaxial with the coil of the medium frequency melting furnace; continue to add dry vibration material to the furnace lining to tie the side wall of the crucible, and the intersection corner of the side wall of the crucible and the bottom of the crucible is a chamfered structure; S3 crucible baking and sintering.
2. The method for preparing a smelting crucible for smelting an iron-based alloy according to claim 1, characterized in that: The protective layer is a corundum tube.
3. The method for preparing a smelting crucible for smelting an iron-based alloy according to claim 2, characterized in that: The chamfer structure at the junction corner between the crucible side wall and the crucible bottom is constructed as an unequal chamfer, the long side of the unequal chamfer corresponds to the direction of the crucible side wall, and the short side of the unequal chamfer corresponds to the direction of the crucible bottom.
4. The method for preparing a smelting crucible for smelting an iron-based alloy according to claim 1, characterized in that: A ramming device is used to ram the dry vibrating material of the furnace lining, the ramming device includes a supporting part, a driving part and a ramming part, the supporting part includes a support leg and an annular frame connected to the top of the support leg, the driving part includes a pneumatic pick slidably connected to the annular frame, and the ramming part includes a rod connected to the bottom end of the pneumatic pick and a flat hammer connected to the end of the rod.
5. The method for preparing a smelting crucible for smelting an iron-based alloy according to claim 4, characterized in that: A vibrating fork is connected to one side of the flat hammer, and the vibrating fork is higher than the surface of the flat hammer.
6. The method for preparing a smelting crucible for smelting an iron-based alloy according to claim 5, characterized in that: The height of the vibrating fork above the flat hammer surface should be set to 1 / 3-1 / 4 of the feeding height.
7. The method for preparing a smelting crucible for smelting an iron-based alloy according to claim 1, characterized in that: During the melting process of S3 iron material, the molten iron occupies more than 90% of the crucible volume.
8. The method for preparing a smelting crucible for smelting an iron-based alloy according to claim 1, characterized in that: S3 crucible baking and sintering, including the following steps: Heat the charge to 1000-1100℃ at a uniform heating rate and keep it warm; After the heat preservation is completed, the temperature is continuously raised to 1620-1660°C at a uniform speed to melt the iron material, and the temperature is kept to sinter the inner surface of the crucible; After the insulation is completed, impurities in the molten metal are removed and the furnace is vacuumed.
9. The method for preparing a smelting crucible for smelting an iron-based alloy according to claim 8, characterized in that: In S3, the charge is heated to 1000-1100°C at a heating rate of 250±10°C / h; and the charge is heated to 1620-1660°C at a heating rate of 200±10°C / h.
10. A melting crucible, characterized in that: The method is prepared by any one of claims 1 to 9.