Low-loss FeSiAl magnetic powder core material for magnetoelectric element and preparation method and application of low-loss FeSiAl magnetic powder core material
By using non-uniform particle size particles and AlN nanoparticles in the FeSiAl magnetic powder core material, combined with segmented multi-step insulation annealing, the problem of high frequency eddy current loss of FeSiAl magnetic powder core material is solved, and high resistivity and low loss are achieved Effective, suitable for mass production.
Patent Information
- Application Number
- CN202411454269.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-17
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-10-17
AI Technical Summary
FeSiAl magnetic powder core material increases eddy current loss at high frequency, resulting in heat generation of magnetic core. The existing inorganic coating method is complex and not suitable for large-scale production, and the Al thermal reaction is difficult to control, and the generated Al2O3 insulating layer has poor uniformity and a greater resistance increase. Small.
The FeSiAl particles with non-uniform particle size are coated with high resistivity AlN nanoparticles, combined with a segmented multi-step insulation and annealing method, a high resistance and stable AlN insulating layer is constructed to improve the resistivity and density of the FeSiAl magnetic powder core material.
It significantly improves the resistivity and density of FeSiAl magnetic powder core material, effectively suppresses eddy current loss, is suitable for large-scale production, and maintains stable performance at high temperatures.
Smart Images

Figure CN119069201A_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the field of magnetic materials for magnetoelectric components, and relates to a low-loss FeSiAl magnetic powder core material, a preparation method and an application thereof for magnetoelectric components. Background Art
[0002] FeSiAl magnetic powder core material has the characteristics of high saturation magnetic induction intensity, high magnetic permeability frequency stability, high DC superposition resistance, etc. It is an indispensable magnetic material for processing current signals, realizing power transmission and conversion, and is widely used in various magneto-electric components such as inductors and transformers. However, since its main component is high-conductivity FeSiAl metal particles, the resistivity of FeSiAl magnetic powder core material is low, and the eddy current loss of the magnetic core will increase sharply at high frequencies, causing the magnetic core to heat up and deteriorate the performance of the magneto-electric component.
[0003] Insulation coating is an effective method to reduce the eddy current loss of FeSiAl magnetic powder cores. The principle is to wrap a high-resistance insulation layer on the surface of the conductive metal particles to block the conductive process between the metal particles, thereby increasing the resistivity of the material. There are two types of insulation coating commonly used, organic coating and inorganic coating. Organic coating refers to the use of organic matter (such as phenolic resin, silicone resin and epoxy resin) to coat the surface of magnetic metal particles. Organic matter usually has a high resistivity and is good at establishing an insulation layer between conductor particles, but it is also easily damaged under high molding pressure or annealing temperature. Inorganic coating refers to the use of high-resistance inorganic materials to wrap magnetic metal particles. Compared with organic coating, inorganic materials have better temperature stability. The coated FeSiAl magnetic powder core can be annealed at a higher temperature to eliminate the stress introduced during the molding process and obtain better magnetic properties.
[0004] Commonly used inorganic coating materials are various oxides, such as SiO2, Al2O3, MoO3, Y2O3, MgO and MnO. The patent "A FeSiAl soft magnetic composite material and its preparation method" (CN 116825466 A) discloses a method for preparing a FeSiAl soft magnetic composite material. By appropriately increasing the Al content and reducing the Fe content in the composition design, FeSiAl soft magnetic powder is prepared, the prepared FeSiAl powder is evenly mixed with iron oxide, and the Al thermal reaction is generated by heating to generate an Al2O3 insulating layer, thereby improving the insulation of the product. However, in this method, since the Al thermal reaction process is difficult to control, the uniformity of the generated Al2O3 insulating layer is poor, resulting in a small increase in the resistivity of the material, and the lowest loss at 100 kHz 50mT reaches 338kW / m3. In addition, this method is relatively complicated, requires too many steps and raw materials, and is not suitable for industrial mass production. Summary of the invention
[0005] In view of the above problems, the present invention provides a low-loss FeSiAl magnetic powder core material, preparation method and application for magnetoelectric components. By selecting FeSiAl particles with non-uniform particle size, coating with AlN nanoparticles with high resistivity and high stability, a high-resistance and stable AlN insulating layer is constructed, and a segmented multi-step heat preservation annealing method is combined to fully eliminate the stress introduced during the pressing process, thereby preparing a FeSiAl magnetic powder core material with high resistivity and low loss. In addition, the preparation method requires simple raw materials, few process steps, and is suitable for mass production.
[0006] In order to achieve the above application purpose, the technical solution adopted in this application is as follows: In a first aspect, the present invention provides a method for preparing a low-loss FeSiAl magnetic powder core material for a magnetoelectric component, comprising: The FeSiAl metal particles are placed in acetone for cleaning to remove residual oil stains on the surface of the FeSiAl metal particles; The FeSiAl metal particles, the organic coating agent and the inorganic coating agent are mixed with an acetone solution to obtain a mixture; The mixture is placed in a water bath and heated with stirring until the acetone is completely evaporated to obtain a dried powder; The dried powder is pressed into a green body, and annealed in a protective atmosphere to obtain a FeSiAl magnetic powder core material.
[0007] Furthermore, the main material FeSiAl metal particles contain 84.5~84.8% Fe, 9.3~9.6% Si, and the balance is Al; the organic coating agent is epoxy resin, accounting for 1.8~2.0wt% of the weight of the main material; and the inorganic coating agent is AlN nanoparticles, accounting for 1.5~2.0wt% of the weight of the main material.
[0008] Furthermore, the main material is a mixture of FeSiAl metal particles of different particle sizes, and the particle size distribution range is 5-30µm; the inorganic coating agent AlN particles are nanoparticles, and the particle size is less than 100nm.
[0009] Further, the FeSiAl metal particles are placed in acetone for cleaning to remove residual oil stains on the surface of the FeSiAl metal particles, specifically including: The FeSiAl metal particles were placed in an acetone solution and ultrasonically cleaned for 15 min. After ultrasonic cleaning, the top layer of solution was removed and the precipitated part was placed in a fume hood for air drying for 24 h.
[0010] Further, the FeSiAl metal particles, the organic coating agent and the inorganic coating agent are mixed with an acetone solution, specifically comprising: During the mixing process, the organic coating agent is first mixed with the acetone solution, and after the organic coating agent is completely dissolved, the main material and the inorganic coating agent are poured into the acetone solution.
[0011] Further, the mixture is placed in a water bath and heated with stirring until the acetone is completely volatilized to obtain a dried powder, comprising: Heat the mixed solution in a 50°C water bath and stir with a stirrer until the acetone is completely evaporated. After the acetone is evaporated, the powder needs to be crushed and passed through a 40-mesh sieve.
[0012] Further, the dried powder is pressed into a green body, and annealed in a protective atmosphere to obtain a FeSiAl magnetic powder core material, including: The powder is placed in a mold and pressed into a green part at a pressure of 1800 MPa; the green part is annealed in a nitrogen protective atmosphere.
[0013] Furthermore, a segmented insulation method is adopted in the annealing process, and the specific annealing curve is: in the first stage, the temperature is increased from 50°C to 300°C, and the heating rate is 2°C / minute; in the second stage, after the temperature is increased to 300°C, it is kept warm for 1 hour; in the third stage, the temperature is increased from 300°C to 700°C, and the heating rate is 1.5°C / minute; in the fourth stage, after the temperature is increased to 700°C, it is kept warm for 1 hour; in the fifth stage, the temperature is reduced from 700°C to 50°C, and the cooling rate is 2°C / minute.
[0014] In a second aspect, the present invention provides a low-loss FeSiAl magnetic powder core material for magneto-electric components, which is prepared by the method for preparing the low-loss FeSiAl magnetic powder core material for magneto-electric components.
[0015] In a third aspect, the present invention provides the use of the low-loss FeSiAl magnetic powder core material for magneto-electric components as described above, which is used in magneto-electric components.
[0016] Compared with the prior art, the present invention has the following technical effects: On the one hand, the present invention provides a low-loss FeSiAl magnetic powder core material for magnetoelectric elements, which is composed of a main material, an organic coating agent and an inorganic coating agent. The main material is FeSiAl metal particles, and the particle size distribution range is 5~30 µm. During the molding process, FeSiAl particles with small particle size can be filled between FeSiAl particles with large particle size, thereby improving the density and saturation magnetization of the FeSiAl magnetic powder core; the organic coating agent is epoxy resin, and the inorganic coating agent is AlN nanoparticles, which can construct a thin and uniform composite insulating layer on the surface of the FeSiAl particles, thereby improving the overall resistivity of the material. Based on the above ingredients, a high-density, high-resistivity FeSiAl magnetic powder core material can be prepared, which effectively suppresses the core loss.
[0017] On the other hand, the present invention provides a method for preparing a low-loss FeSiAl magnetic powder core material for magnetoelectric components. First, FeSiAl metal particles are cleaned with acetone to remove oil attached to the surface and obtain a high-purity main material; then the organic coating agent is dissolved in acetone, and the main material and the inorganic coating agent are poured into the acetone solution to form a mixed solution; next, the mixed solution is placed in a water bath for heating and stirring, so that the organic coating agent and the inorganic coating agent are fully wrapped on the surface of the FeSiAl particles; finally, the pressed green blank is placed in a tubular furnace and subjected to multi-step heat preservation annealing under nitrogen protection. The core technology of the present invention is that high-resistance AlN nanoparticles are used as inorganic coating agents, combined with water bath heating and stirring, so that the AlN nanoparticles can be evenly distributed on the surface of the FeSiAl particles to form a thin and uniform insulating layer, which significantly improves the resistivity of the FeSiAl magnetic powder core material. At the same time, due to the high temperature stability of AlN, there is no need to worry about its volatilization or decomposition at high temperatures, so that the FeSiAl magnetic powder core can be annealed at a higher temperature, fully eliminating stress, and will not damage the insulating coating layer. In addition, the method for preparing the low-loss FeSiAl magnetic powder core material provided by the present invention requires simple raw materials and has fewer process steps, and can be applied to mass production. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 SEM images of samples of Examples 1 to 4 and Comparative Examples 1 and 2 Figure 2 Example 4 Element distribution of samples DETAILED DESCRIPTION The present invention provides a low-loss FeSiAl magnetic powder core material for magnetoelectric components and a preparation method thereof. The core idea of the present invention is: based on organic + inorganic composite coating, epoxy resin and AlN nanoparticles are used to construct a thin and high-resistance insulating coating layer on the surface of FeSiAl metal magnetic particles, thereby improving the overall resistivity of the material and effectively suppressing eddy current losses; at the same time, a segmented multi-step insulation method is adopted during the sintering process to fully release the stress introduced during the pressing process and obtain excellent electromagnetic properties. The prepared FeSiAl magnetic powder core material has the characteristics of high magnetic permeability, high resistivity, low loss, etc. The preparation process comprises the following steps: S1. Place FeSiAl particles in an acetone solution and perform ultrasonic cleaning. Weigh FeSiAl metal particles in a beaker, add acetone solution until the FeSiAl particles are completely immersed, and place the beaker in an ultrasonic cleaner for ultrasonic cleaning for 15 minutes. After the ultrasonic cleaning is completed, remove the top layer of acetone solution, and place the precipitated part in a fume hood for air drying for 24 hours; S2, the cleaned FeSiAl particles, the organic coating agent and the inorganic coating agent are mixed with an acetone solution. During the mixing process, according to the weight of the FeSiAl particles, 1.8-2.0wt% epoxy resin is first mixed with the acetone solution until the epoxy resin is completely dissolved in the acetone solution, and then the FeSiAl particles and 1.5-2.0wt% AlN nanoparticles are poured into the acetone solution; S3, heat the mixed solution in a 50°C water bath and stir with a stirrer at a speed of 50 rpm until the acetone evaporates, then crush the powder and pass it through a 40-mesh sieve; S4, putting the sieved powder into a mold, pressing it into a ring-shaped green piece and a disc-shaped green piece at a pressure of 1800 MPa, and then placing the green piece in a tube furnace and annealing it under nitrogen protection. The annealing process adopts a segmented insulation method, and the annealing temperature is 700°C; The annealed FeSiAl magnetic powder core samples were tested for relevant properties using the following equipment: The inductance L of the annular sample obtained in step S4 is tested using a Tonghui TH2826A LCR meter under the conditions of 1kHz 600mV, and the effective magnetic permeability μe of the annular sample is calculated according to the formula μe=L∙le∙10-2 / (0.4π∙Ae∙N2), where le is the effective magnetic path length of the annular sample, Ae is the effective magnetic path area of the annular sample, and N is the number of turns of the coil; The resistance R of the disc-shaped sample obtained in step S4 is tested using a Tonghui TH2826A LCR meter under the test conditions of 1kHz 600mV, and the resistivity ρ of the disc-shaped sample is calculated according to the formula ρ=RS / d, where d is the disc thickness and S is the disc area; The loss of the ring sample obtained in step S4 is tested using a BH analyzer of model SY-8218, and the test conditions are 50kHz 100mT, 100kHz 100mT; The microstructure and element distribution of the ring sample obtained in step S4 were characterized using a Hitachi TM3030Plus scanning electron microscope.
[0019] The present invention is described in detail below through specific embodiments.
[0020] Example Table 1 Composition and proportion of samples in Examples 1-4
[0021] Comparative Example Table 2 Sample composition and ratio of comparative examples 1 and 2
[0022] Example 1 A low-loss FeSiAl magnetic powder core material, the preparation steps are as follows: S1. Place FeSiAl particles in an acetone solution and perform ultrasonic cleaning. Weigh 50 g of FeSiAl particles in a beaker, add 100 mL of acetone solution until the FeSiAl particles are completely immersed, and place the beaker in an ultrasonic cleaner for ultrasonic cleaning for 15 min. After the ultrasonic cleaning is completed, remove the top layer of acetone solution, and place the precipitated part in a fume hood for air drying for 24 h. S2, the cleaned FeSiAl particles, organic coating agent and inorganic coating agent are mixed with acetone solution. During the mixing process, according to the weight of the FeSiAl particles, 2.0wt% epoxy resin is first mixed with the acetone solution until the epoxy resin is completely dissolved in the acetone solution, and then the FeSiAl particles and 1.5wt% AlN nanoparticles are poured into the acetone solution; S3, heat the mixed solution in a 50°C water bath and stir with a stirrer at a speed of 50 rpm until the acetone evaporates, then crush the powder and pass it through a 40-mesh sieve; S4, putting the sieved powder into a mold, pressing it into a ring-shaped green piece and a disc-shaped green piece at a pressure of 1800 MPa, and then placing the green piece in a tube furnace and annealing it under nitrogen protection. The annealing process adopts a segmented insulation method, and the annealing temperature is 700°C; Example 2 A low-loss FeSiAl magnetic powder core material, the preparation steps are as follows: S1. Place FeSiAl particles in an acetone solution and perform ultrasonic cleaning. Weigh 50 g of FeSiAl particles in a beaker, add 100 mL of acetone solution until the FeSiAl particles are completely immersed, and place the beaker in an ultrasonic cleaner for ultrasonic cleaning for 15 min. After the ultrasonic cleaning is completed, remove the top layer of acetone solution, and place the precipitated part in a fume hood for air drying for 24 h. S2, the cleaned FeSiAl particles, the organic coating agent and the inorganic coating agent are mixed with an acetone solution. During the mixing process, according to the weight of the FeSiAl particles, 2.0wt% epoxy resin is first mixed with the acetone solution until the epoxy resin is completely dissolved in the acetone solution, and then the FeSiAl particles and 1.7wt% AlN nanoparticles are poured into the acetone solution; Steps S3 and S4 are exactly the same as those in Example 1.
[0023] Example 3 A low-loss FeSiAl magnetic powder core material, the preparation steps are as follows: S1. Place FeSiAl particles in an acetone solution and perform ultrasonic cleaning. Weigh 50 g of FeSiAl particles in a beaker, add 100 mL of acetone solution until the FeSiAl particles are completely immersed, and place the beaker in an ultrasonic cleaner for ultrasonic cleaning for 15 min. After the ultrasonic cleaning is completed, remove the top layer of acetone solution, and place the precipitated part in a fume hood for air drying for 24 h. S2, the cleaned FeSiAl particles, the organic coating agent and the inorganic coating agent are mixed with an acetone solution. During the mixing process, according to the weight of the FeSiAl particles, 2.0wt% epoxy resin is first mixed with the acetone solution until the epoxy resin is completely dissolved in the acetone solution, and then the FeSiAl particles and 1.8wt% AlN nanoparticles are poured into the acetone solution; Steps S3 and S4 are exactly the same as those in Example 1.
[0024] Example 4 A low-loss FeSiAl magnetic powder core material, the preparation steps are as follows: S1. Place FeSiAl particles in an acetone solution and perform ultrasonic cleaning. Weigh 50 g of FeSiAl particles in a beaker, add 100 mL of acetone solution until the FeSiAl particles are completely immersed, and place the beaker in an ultrasonic cleaner for ultrasonic cleaning for 15 min. After the ultrasonic cleaning is completed, remove the top layer of acetone solution, and place the precipitated part in a fume hood for air drying for 24 h. S2, the cleaned FeSiAl particles, the organic coating agent and the inorganic coating agent are mixed with an acetone solution. During the mixing process, according to the weight of the FeSiAl particles, 2.0wt% epoxy resin is first mixed with the acetone solution until the epoxy resin is completely dissolved in the acetone solution, and then the FeSiAl particles and 2.0wt% AlN nanoparticles are poured into the acetone solution; Steps S3 and S4 are exactly the same as those in Example 1.
[0025] Comparative Example 1 A low-loss FeSiAl magnetic powder core material, the preparation steps are as follows: S1. Place FeSiAl particles in an acetone solution and perform ultrasonic cleaning. Weigh 50 g of FeSiAl particles in a beaker, add 100 mL of acetone solution until the FeSiAl particles are completely immersed, and place the beaker in an ultrasonic cleaner for ultrasonic cleaning for 15 min. After the ultrasonic cleaning is completed, remove the top layer of acetone solution, and place the precipitated part in a fume hood for air drying for 24 h. S2, the cleaned FeSiAl particles, the organic coating agent and the inorganic coating agent are mixed with an acetone solution. During the mixing process, according to the weight of the FeSiAl particles, 2.0wt% epoxy resin is first mixed with the acetone solution until the epoxy resin is completely dissolved in the acetone solution, and then the FeSiAl particles are poured into the acetone solution; Steps S3 and S4 are exactly the same as those in Example 1.
[0026] Comparative Example 2 A low-loss FeSiAl magnetic powder core material, the preparation steps are as follows: S1. Place FeSiAl particles in an acetone solution and perform ultrasonic cleaning. Weigh 50 g of FeSiAl particles in a beaker, add 100 mL of acetone solution until the FeSiAl particles are completely immersed, and place the beaker in an ultrasonic cleaner for ultrasonic cleaning for 15 min. After the ultrasonic cleaning is completed, remove the top layer of acetone solution, and place the precipitated part in a fume hood for air drying for 24 h. S2, the cleaned FeSiAl particles, the organic coating agent and the inorganic coating agent are mixed with an acetone solution. During the mixing process, according to the weight of the FeSiAl particles, 2.0wt% epoxy resin is first mixed with the acetone solution until the epoxy resin is completely dissolved in the acetone solution, and then the FeSiAl particles and 2.5wt% AlN nanoparticles are poured into the acetone solution; Steps S3 and S4 are exactly the same as those in Example 1.
[0027] The microstructure of the FeSiAl magnetic powder core of the above embodiment and comparative example is as follows: Figure 1 The relevant performance parameters are shown in Table 3, and the energy spectrum analysis results of Example 4 are shown in Figure 2 shown.
[0028] Table 3 Electromagnetic properties of samples of Examples 1 to 4 and Comparative Examples 1 and 2
[0029] Table 4 Loss separation results of samples of Examples 1 to 4 and Comparative Examples 1 and 2 at 100kHz 100mT
[0030] Depend on Figure 1 SEM images of Figure 2From the element distribution and the electromagnetic performance parameters of Examples 1 to 4 in Table 3, it can be seen that the FeSiAl magnetic powder core material prepared by the present invention has high density, few pores, thin and evenly distributed insulation layer, high resistivity and low loss. At 100kHz 100mT, the loss is lower than 435kW / m3. Among them, the sample of Example 3 has the best comprehensive performance, with a large initial magnetic permeability, a high resistivity and the lowest loss.
[0031] By comparing Example 1 with Example 2, it can be seen that the content of inorganic coating agent AlN nanoparticles is increased to 1.7wt% on the basis of Example 1. Although the magnetic permeability decreases due to the introduction of the non-magnetic phase, the hysteresis loss increases to 314 kW / m3, but the resistivity is also increased, the eddy current loss is suppressed, and the total loss is reduced from 435 kW / m3 to 413 kW / m3.
[0032] By comparing Example 2 with Example 3, it can be seen that further increasing the content of inorganic coating agent AlN nanoparticles to 1.8wt% on the basis of Example 2 reduces the magnetic permeability and increases the hysteresis loss, but also significantly increases the resistivity, reduces the eddy current loss to 74 kW / m3, and thus reduces the total loss to 394 kW / m3.
[0033] By comparing Example 3 with Example 4, it can be seen that by further increasing the content of inorganic coating agent AlN nanoparticles to 2.0wt% on the basis of Example 3, although the resistivity is further improved and the eddy current loss is reduced to 52 kW / m3, the hysteresis loss increases to 364 kW / m3 due to the decrease in magnetic permeability, resulting in an increase in the total loss to 416 kW / m3.
[0034] By comparing Comparative Example 1 with Example 1, it can be seen that when the content of inorganic coating agent AlN nanoparticles is reduced to 0.0wt% on the basis of Example 1, although the magnetic permeability is increased and the hysteresis loss is slightly reduced, the insulation effect of the coating layer is reduced, resulting in a significant decrease in resistivity, an increase in eddy current loss to 244 kW / m3, and an increase in total loss to 510 kW / m3.
[0035] By comparing Comparative Example 2 with Example 4, it can be seen that when the content of inorganic coating agent AlN nanoparticles is further increased to 2.5wt% on the basis of Example 4, although the resistivity increases to 1.15Ω•m and the eddy current loss is only 50 kW / m3, the hysteresis loss increases to 451 kW / m3, resulting in the total loss increasing to 502 kW / m3.
[0036] It can be seen from the above data that in the preparation process of the low-loss FeSiAl magnetic powder core material of the present invention, high-resistance AlN nanoparticles are used as an inorganic coating agent to form a thin and uniform insulating layer, which significantly improves the resistivity of the FeSiAl magnetic powder core material. At the same time, the content of AlN nanoparticles is strictly controlled, and the segmented multi-step heat-insulating sintering method is combined to ensure that the magnetic permeability of the FeSiAl magnetic powder core does not decrease too much, so that the prepared FeSiAl magnetic powder core material has the characteristics of high magnetic permeability, high resistivity and low loss.
[0037] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the above embodiments, ordinary technicians in the relevant field should understand that the specific implementation methods of the present invention can still be modified or replaced by equivalents. Any modification or equivalent replacement that does not depart from the spirit and scope of the present invention should be covered within the scope of protection of the claims of the present invention.
Claims
1. A method for preparing a low-loss FeSiAl magnetic powder core material for a magnetoelectric component, characterized in that: include: The FeSiAl metal particles are placed in acetone for cleaning to remove residual oil stains on the surface of the FeSiAl metal particles; The FeSiAl metal particles, the organic coating agent and the inorganic coating agent are mixed with an acetone solution to obtain a mixture; The mixture is placed in a water bath and heated with stirring until the acetone is completely evaporated to obtain a dried powder; The dried powder is pressed into a green body, and annealed in a protective atmosphere to obtain a FeSiAl magnetic powder core material.
2. The method for preparing a low-loss FeSiAl magnetic powder core material for a magnetoelectric component according to claim 1, characterized in that: The main material FeSiAl metal particles contain 84.5~84.8% Fe, 9.3~9.6% Si, and the balance is Al; the organic coating agent is epoxy resin, accounting for 1.8~2.0wt% of the weight of the main material; the inorganic coating agent is AlN nanoparticles, accounting for 1.5~2.0wt% of the weight of the main material.
3. The method for preparing a low-loss FeSiAl magnetic powder core material for a magnetoelectric component according to claim 1, characterized in that: The main material is a mixture of FeSiAl metal particles of different particle sizes, with a particle size distribution range of 5~30 µm; the inorganic coating agent AlN particles are nanoparticles with a particle size less than 100nm.
4. The method for preparing a low-loss FeSiAl magnetic powder core material for a magnetoelectric component according to claim 1, characterized in that: The FeSiAl metal particles are placed in acetone for cleaning to remove residual oil stains on the surface of the FeSiAl metal particles, specifically including: The FeSiAl metal particles were placed in an acetone solution and ultrasonically cleaned for 15 min. After ultrasonic cleaning, the top layer of solution was removed and the precipitated part was placed in a fume hood for air drying for 24 h.
5. The method for preparing a low-loss FeSiAl magnetic powder core material for a magnetoelectric component according to claim 1, characterized in that: The FeSiAl metal particles, the organic coating agent and the inorganic coating agent are mixed with an acetone solution, specifically comprising: During the mixing process, the organic coating agent is first mixed with the acetone solution, and after the organic coating agent is completely dissolved, the main material and the inorganic coating agent are poured into the acetone solution.
6. The method for preparing a low-loss FeSiAl magnetic powder core material for a magnetoelectric component according to claim 1, characterized in that: The mixture is placed in a water bath and heated with stirring until the acetone is completely volatilized to obtain a dried powder, including: Heat the mixed solution in a 50°C water bath and stir with a stirrer until the acetone is completely evaporated. After the acetone is evaporated, the powder needs to be crushed and passed through a 40-mesh sieve.
7. The method for preparing a low-loss FeSiAl magnetic powder core material for a magnetoelectric component according to claim 1, characterized in that: The dried powder is pressed into a green body, and annealed in a protective atmosphere to obtain a FeSiAl magnetic powder core material, including: The powder is placed in a mold and pressed into a green part at a pressure of 1800 MPa; the green part is annealed in a nitrogen protective atmosphere.
8. The method for preparing a low-loss FeSiAl magnetic powder core material for a magnetoelectric component according to claim 7, characterized in that: The annealing process adopts a segmented insulation method, and the specific annealing curve is as follows: in the first stage, the temperature rises from 50°C to 300°C, and the heating rate is 2°C / min; in the second stage, after the temperature rises to 300°C, it is kept warm for 1h; in the third stage, the temperature rises from 300°C to 700°C, and the heating rate is 1.5°C / min; in the fourth stage, after the temperature rises to 700°C, it is kept warm for 1h; in the fifth stage, the temperature drops from 700°C to 50°C, and the cooling rate is 2°C / min.
9. Low-loss FeSiAl magnetic powder core material for magneto-electric components, characterized in that: The low-loss FeSiAl magnetic powder core material for magnetoelectric components is prepared by the preparation method of any one of claims 1 to 8.
10. The use of the low-loss FeSiAl magnetic powder core material for magneto-electric components according to claim 9, characterized in that: For magnetoelectric components.
Citation Information
Patent Citations
FeSiAl soft magnetic composite material and preparation method thereof
CN116825466A
Preparation method of high thermal conductive insulating soft magnetic metal powder and soft magnetic metal powder
CN109326405A
Low-loss FeSiAl / MnZn ferrite soft magnetic composite magnetic powder core with stable magnetic conductivity and preparation method of low-loss FeSiAl / MnZn ferrite soft magnetic composite magnetic powder core with stable magnetic conductivity
CN113658768A
Magnetic powder material, magnetic device and electronic equipment
CN115691933A
Reactor and method for producing same
WO2011077694A1