Magnetic filter aid for filtering and dewatering fluorine-containing sludge through direct flotation of calcium fluoride and manufacturing method of magnetic filter aid

By using hydrophobically modified natural magnetite powder as a magnetic filter aid, the problems of long filtration time and high moisture content during the filtration and dehydration of fluorine-containing sludge are solved, and efficient calcium fluoride purification and resources are achieved Reuse and the reusable performance of the filter aid is stable.

CN119075902APending Publication Date: 2024-12-06GUOFU NEW MATERIALS (GUANGDONG) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411179945.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-07-17
Filing Date
2024-08-27
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The prior art has problems such as long filtration time, high moisture content of the filter cake and impurity residues in the filtration and dehydration process of fluorinated sludge, which affects the efficient purification of calcium fluoride and resource reuse.

Method used

The hydrophobic modified natural magnetite powder is used as a magnetic filter aid, and the dry ball mill and silane surface modification agent are used to prepare a magnetic filter aid with a particle size of 150-270μm for strengthening filtration separation and realizing fluorination. Highly efficient dehydration of calcium.

Benefits of technology

It significantly shortens the filtration time and reduces the moisture content of the calcium fluoride filter cake. The filter aid is easy to separate from the calcium fluoride product, has good reuse performance, and improves the purification efficiency and resource reuse ability of calcium fluoride. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005011807600000061
    Figure BDA0005011807600000061
  • Figure BDA0005011807600000071
    Figure BDA0005011807600000071
Patent Text Reader

Abstract

The invention discloses a magnetic filter aid for filtration and dehydration of fluorine-containing sludge direct flotation calcium fluoride, the main component of the magnetic filter aid is hydrophobic modified natural magnetite powder, the particle size is 150-270 [mu] m, and the saturation magnetization is greater than 50 emu / g. The invention also provides a manufacturing method thereof. All raw materials for preparing the magnetic hydrophobic filter aid are cheap and easy to obtain, and the preparation method is simple to operate and relatively low in cost. The filtering aid has an excellent filtering aiding effect in fluorine-containing sludge direct flotation calcium fluoride filtering dehydration, the filtering time is remarkably shortened, and the water content of a calcium fluoride filter cake is remarkably reduced. In addition, the magnetic filter aid is easily separated from a calcium fluoride product through a magnet, is stable in reusability and has a very good application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to filtration separation in the process of fluorine-containing sludge flotation purification, and in particular to a magnetic filter aid in the process of fluorine-containing sludge positive flotation calcium fluoride filtration and dehydration and a manufacturing method thereof. Background Art

[0002] A large amount of fluoride-containing wastewater is discharged from the production lines of strategic emerging industries such as the semiconductor and photovoltaic industries. The treatment process of this type of wastewater will produce fluoride-containing sludge with calcium fluoride as the main component. As an important national strategic resource, calcium fluoride is widely used in ceramics, metallurgy, fluorine chemical industry, aviation and other fields. However, fluoride-containing sludge contains not only calcium fluoride, but also a variety of impurities, such as calcium carbonate, calcium hydroxide, calcium sulfate, silica and polyaluminum flocculants. Calcium fluoride in this form cannot be directly applied to the above-mentioned fields. From the perspective of resource recycling and circular economy, it is very necessary to selectively enrich calcium fluoride in fluoride-containing sludge so that the calcium fluoride content and impurity content meet the quality requirements of different industries.

[0003] Due to the complex impurity components in fluorine-containing sludge, it is difficult to achieve the enrichment and extraction of high-purity calcium fluoride by a single means. According to current relevant literature reports, acid-base treatment, flotation, solvent washing, and high-temperature calcination are several typical effective purification methods for the purification of calcium fluoride in fluorine-containing sludge. Among them, flotation has been widely used in the purification and separation of calcium fluoride in natural fluorite due to its mild and efficient separation characteristics, especially for the separation of calcium carbonate and silicon dioxide from calcium fluoride, the flotation method shows excellent separation performance. Based on the successful application of flotation in the enrichment of calcium fluoride in natural fluorite, relevant researchers have developed a flotation process for calcium fluoride in fluorine-containing sludge. Invention patent CN115634775A discloses a method for obtaining calcium fluoride by flotation of calcium fluoride sludge. In the invention, through the action of adjusting agents, inhibitors and collectors, the target component calcium fluoride floats out of the slurry with foam, and the collected foam is filtered and dried to obtain a calcium fluoride product with high purity. However, since the product with calcium fluoride as the main component obtained by flotation has a small particle size and a certain hydrophilicity, there are problems such as long filtration time and high moisture content of the filter cake through vacuum or pressure filtration. Incomplete filtration separation not only increases the drying energy consumption cost of subsequent products, but also causes the chemical agents dispersed in the water to remain in the solid product and cannot be recycled, resulting in the loss of chemical agents. If the filtration separation can be enhanced by adding filter aids, the flotation method for purifying and separating industrial calcium fluoride can have a higher separation efficiency. However, ordinary physical filter aids such as diatomaceous earth and volcanic ash will remain in the product as new impurity components after being added, and chemical filter aids can also be dispersed in the flotation liquid and affect the flotation effect of the next cycle. In summary, the development of new filter aids that are easy to separate and regenerate from calcium fluoride products is an important breakthrough in improving the dehydration effect of calcium fluoride by flotation. However, filter aids used for positive flotation filtration of calcium fluoride from fluoride-containing sludge have not yet been reported in the literature. Summary of the invention

[0004] The present invention provides a magnetic filter aid for fluorine-containing sludge positive flotation calcium fluoride filtration and dehydration and a manufacturing method thereof, so as to solve the technical problem of both strengthening filtration separation and rapidly recovering and reusing calcium fluoride products, and realize efficient purification of industrial calcium fluoride.

[0005] The invention discloses a magnetic filter aid for positive flotation of calcium fluoride filtration and dehydration of fluoride-containing sludge, characterized in that the main component is hydrophobically modified natural magnetite powder, the particle size is 150-270 μm, and the saturation magnetization intensity is greater than 50 emu / g.

[0006] The method for manufacturing a magnetic filter aid for positive flotation of calcium fluoride filtration and dehydration of fluoride-containing sludge is carried out according to the following steps:

[0007] Step 1: Production of natural magnetite powder

[0008] The natural magnetite particles are ground in a dry ball mill, and sieved through 50-mesh and 100-mesh sieves to obtain natural magnetite powder with a particle size of 150 to 270 μm;

[0009] Step 2: Hydrophobic modification of natural magnetite powder using hydrophobic silane surface modifier

[0010] Weigh 50 g of the natural magnetite powder obtained in the first step, add it to 500 mL of ethanol solution of silane surface modifier (volume fraction is 1% to 6%), ultrasonically disperse it for 15 to 30 minutes, stir and react at 30°C and 300 rpm for 12 to 24 hours, use a magnet to separate the solid and liquid, place the solid sample in an oven at 120°C and dry it for 2 hours to obtain hydrophobically modified natural magnetite powder.

[0011] The natural magnetite ore is provided by an iron mine in Panzhihua, Sichuan, and is processed into natural magnetite ore particles of about 3 mm by a crusher.

[0012] In step 1 of the above method, the grinding process in the ball mill is: weigh 2 kg of natural magnetite particles, add them into the ball mill, and grind for 5 to 10 minutes.

[0013] In step 2 of the above method, the silane surface modifier is one of silane coupling agents with different carbon chain lengths, specifically one of methyltrimethoxysilane, propyltrimethoxysilane, octyltrimethoxysilane, dodecyltrimethoxysilane, and hexadecyltrimethoxysilane.

[0014] The present invention has the following advantages:

[0015] (1) All raw materials for preparing hydrophobically modified natural magnetite powder are cheap and readily available, the manufacturing method is simple to operate, and the cost is low.

[0016] (2) The prepared magnetic hydrophobic filter aid has an excellent filter aid effect in the filtration and dehydration of calcium fluoride in the positive flotation of fluoride-containing sludge, the filtration time is significantly shortened, and the moisture content of the calcium fluoride filter cake is significantly reduced. In addition, the magnetic filter aid is easy to separate from the calcium fluoride product by a magnet, and has stable performance in repeated use, and has a good application prospect. DETAILED DESCRIPTION

[0017] The present invention will be further described below in conjunction with specific examples. It should be understood that these examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention.

[0018] Example 1

[0019] The natural magnetite particles are ground in a dry ball mill, screened through 50-mesh and 100-mesh sieves to obtain natural magnetite powder with a particle size of 150 to 270 μm, and recovered by a magnet and stored in a ziplock bag; 50 g of the natural magnetite powder prepared above is weighed, added to 500 mL of an ethanol solution of methyltrimethoxysilane (3% by volume), ultrasonically dispersed for 20 minutes, stirred and reacted at 30° C. and 300 rpm for 12 hours, a magnet is used for solid-liquid separation, and the solid sample is placed in a 120° C. oven and dried for 2 hours to obtain a hydrophobically modified natural magnetite powder.

[0020] Example 2

[0021] The natural magnetite particles are ground in a dry ball mill, screened through 50-mesh and 100-mesh sieves to obtain natural magnetite powder with a particle size of 150 to 270 μm, and recovered by a magnet and stored in a ziplock bag; 50 g of the natural magnetite powder prepared above is weighed, added to 500 mL of an ethanol solution of propyltrimethoxysilane (3% by volume), ultrasonically dispersed for 20 minutes, stirred and reacted at 30° C. and 300 rpm for 12 hours, a magnet is used for solid-liquid separation, and the solid sample is placed in a 120° C. oven and dried for 2 hours to obtain a hydrophobically modified natural magnetite powder.

[0022] Example 3

[0023] The natural magnetite particles are ground in a dry ball mill, screened through 50-mesh and 100-mesh sieves to obtain natural magnetite powder with a particle size of 150 to 270 μm, and recovered in a ziplock bag through a magnet; 50 g of the natural magnetite powder prepared above is weighed, added to 500 mL of an ethanol solution of octyltrimethoxysilane (3% by volume), ultrasonically dispersed for 20 minutes, stirred and reacted at 30° C. and 300 rpm for 12 hours, a magnet is used for solid-liquid separation, and the solid sample is placed in a 120° C. oven and dried for 2 hours to obtain a hydrophobically modified natural magnetite powder.

[0024] Example 4

[0025] The natural magnetite particles are ground in a dry ball mill, screened through 50-mesh and 100-mesh sieves to obtain natural magnetite powder with a particle size of 150 to 270 μm, and recovered by a magnet and stored in a ziplock bag; 50 g of the natural magnetite powder prepared above is weighed, added to 500 mL of an ethanol solution of dodecyltrimethoxysilane (volume fraction of 3%), ultrasonically dispersed for 20 minutes, stirred and reacted at 30° C. and 300 rpm for 12 hours, a magnet is used for solid-liquid separation, and the solid sample is placed in a 120° C. oven and dried for 2 hours to obtain a hydrophobically modified natural magnetite powder.

[0026] Example 5

[0027] The natural magnetite particles are ground in a dry ball mill, screened through 50-mesh and 100-mesh sieves to obtain natural magnetite powder with a particle size of 150-270 μm, and recovered by a magnet and stored in a ziplock bag; 50 g of the natural magnetite powder prepared above is weighed, added to 500 mL of an ethanol solution of hexadecyltrimethoxysilane (volume fraction of 3%), ultrasonically dispersed for 20 minutes, stirred and reacted at 30° C. and 300 rpm for 12 hours, a magnet is used for solid-liquid separation, and the solid sample is placed in a 120° C. oven and dried for 2 hours to obtain a hydrophobically modified natural magnetite powder.

[0028] Example 6

[0029] The natural magnetite particles are ground in a dry ball mill, screened through 50-mesh and 100-mesh sieves to obtain natural magnetite powder with a particle size of 150 to 270 μm, and recovered in a ziplock bag through a magnet; 50 g of the natural magnetite powder prepared above is weighed, added to 500 mL of an ethanol solution of methyltrimethoxysilane (volume fraction of 1%), ultrasonically dispersed for 20 minutes, stirred and reacted at 30° C. and 300 rpm for 12 hours, a magnet is used for solid-liquid separation, and the solid sample is placed in a 120° C. oven and dried for 2 hours to obtain a hydrophobically modified natural magnetite powder.

[0030] Example 7

[0031] The natural magnetite particles are ground in a dry ball mill, screened through 50-mesh and 100-mesh sieves to obtain natural magnetite powder with a particle size of 150 to 270 μm, and recovered in a ziplock bag through a magnet; 50 g of the natural magnetite powder prepared above is weighed, added to 500 mL of an ethanol solution of methyltrimethoxysilane (volume fraction of 1%), ultrasonically dispersed for 20 minutes, stirred and reacted at 30° C. and 300 rpm for 12 hours, a magnet is used for solid-liquid separation, and the solid sample is placed in a 120° C. oven and dried for 2 hours to obtain a hydrophobically modified natural magnetite powder.

[0032] Example 8

[0033] The natural magnetite particles are ground in a dry ball mill, screened through 50-mesh and 100-mesh sieves to obtain natural magnetite powder with a particle size of 150-270 μm, and recovered in a ziplock bag through a magnet; 50 g of the natural magnetite powder prepared above is weighed, added to 500 mL of an ethanol solution of octyltrimethoxysilane (volume fraction of 1%), ultrasonically dispersed for 20 minutes, stirred and reacted at 30° C. and 300 rpm for 12 hours, a magnet is used for solid-liquid separation, and the solid sample is placed in a 120° C. oven and dried for 2 hours to obtain a hydrophobically modified natural magnetite powder.

[0034] Example 9

[0035] The natural magnetite particles are ground in a dry ball mill, screened through 50-mesh and 100-mesh sieves to obtain natural magnetite powder with a particle size of 150-270 μm, and recovered by a magnet and stored in a ziplock bag; 50 g of the natural magnetite powder prepared above is weighed, added to 500 mL of an ethanol solution of dodecyltrimethoxysilane (volume fraction of 1%), ultrasonically dispersed for 20 minutes, stirred and reacted at 30° C. and 300 rpm for 12 hours, a magnet is used for solid-liquid separation, and the solid sample is placed in a 120° C. oven and dried for 2 hours to obtain a hydrophobically modified natural magnetite powder.

[0036] Example 10

[0037] The natural magnetite particles are ground in a dry ball mill, screened through 50-mesh and 100-mesh sieves to obtain natural magnetite powder with a particle size of 150 to 270 μm, and recovered in a ziplock bag through a magnet; 50 g of the natural magnetite powder prepared above is weighed, added to 500 mL of an ethanol solution of hexadecyltrimethoxysilane (volume fraction of 1%), ultrasonically dispersed for 20 minutes, stirred and reacted at 30° C. and 300 rpm for 12 hours, a magnet is used for solid-liquid separation, and the solid sample is placed in a 120° C. oven and dried for 2 hours to obtain a hydrophobically modified natural magnetite powder.

[0038] Embodiment 11

[0039] The natural magnetite particles are ground in a dry ball mill, screened through 50-mesh and 100-mesh sieves to obtain natural magnetite powder with a particle size of 150-270 μm, and recovered by a magnet and stored in a ziplock bag; 50 g of the natural magnetite powder prepared above is weighed, added to 500 mL of an ethanol solution of hexadecyltrimethoxysilane (volume fraction of 2%), ultrasonically dispersed for 20 minutes, stirred and reacted at 30° C. and 300 rpm for 12 hours, a magnet is used for solid-liquid separation, and the solid sample is placed in a 120° C. oven and dried for 2 hours to obtain a hydrophobically modified natural magnetite powder.

[0040] Example 12

[0041] The natural magnetite particles are ground in a dry ball mill, screened through 50-mesh and 100-mesh sieves to obtain natural magnetite powder with a particle size of 150 to 270 μm, and recovered in a ziplock bag through a magnet; 50 g of the natural magnetite powder prepared above is weighed, added to 500 mL of an ethanol solution of hexadecyltrimethoxysilane (4% by volume), ultrasonically dispersed for 20 minutes, stirred and reacted at 30° C. and 300 rpm for 12 hours, a magnet is used for solid-liquid separation, and the solid sample is placed in a 120° C. oven and dried for 2 hours to obtain a hydrophobically modified natural magnetite powder.

[0042] Embodiment 13

[0043] The natural magnetite particles are ground in a dry ball mill, screened through 50-mesh and 100-mesh sieves to obtain natural magnetite powder with a particle size of 150-270 μm, and recovered in a ziplock bag through a magnet; 50 g of the natural magnetite powder prepared above is weighed, added to 500 mL of an ethanol solution of hexadecyltrimethoxysilane (5% by volume), ultrasonically dispersed for 20 minutes, stirred and reacted at 30° C. and 300 rpm for 12 hours, a magnet is used for solid-liquid separation, and the solid sample is placed in a 120° C. oven and dried for 2 hours to obtain a hydrophobically modified natural magnetite powder.

[0044] Embodiment 14

[0045] The natural magnetite particles are ground in a dry ball mill, screened through 50-mesh and 100-mesh sieves to obtain natural magnetite powder with a particle size of 150 to 270 μm, and recovered by a magnet and stored in a ziplock bag; 50 g of the natural magnetite powder prepared above is weighed, added to 500 mL of an ethanol solution of hexadecyltrimethoxysilane (volume fraction of 6%), ultrasonically dispersed for 20 minutes, stirred and reacted at 30° C. and 300 rpm for 12 hours, a magnet is used for solid-liquid separation, and the solid sample is placed in a 120° C. oven and dried for 2 hours to obtain a hydrophobically modified natural magnetite powder.

[0046] Application Example 1

[0047] This application example uses fluorine-containing sludge from a certain enterprise as raw material, and first conducts a flotation test according to the method of patent CN115634775A. The flotation reagents are sodium carbonate, water glass and oleic acid as regulators, inhibitors and collectors, respectively. The hydrophobically modified natural magnetite powder of Example 1-14 is used as a filter aid to conduct a filtration and dehydration test on positive flotation calcium fluoride. The specific steps are as follows: weigh 0.5-3g of filter aid and add it to 100g of positive flotation calcium fluoride foam, stir at room temperature and 300rpm for 5 minutes, then filter with a Buchner funnel with a diameter of 9cm, and the vacuum degree is 0.09MPa. Filter until no liquid drips within 1 minute, record the filtration time and the mass of the wet filter cake, then put the filter cake into a 120-degree oven and dry it to constant weight and record the weight of the dry filter cake, and calculate the moisture content of the wet filter cake. As a blank application example, the above operation is performed without adding any filter aid. It can be seen from Table 1 that, compared with the blank filtration and dehydration test without adding filter aids, the filter aids prepared in all examples can effectively shorten the filtration time and reduce the moisture content of the wet filter cake, especially the filter aids in Examples 5, 12, 13, and 14, which show excellent filtration and dehydration performance. In addition, taking the filter aid in Example 5 as a typical representative, a filtration and dehydration test of positive flotation calcium fluoride was carried out by changing its dosage. The results show that the greater the dosage, the better the filtration effect.

[0048] Table 1 Effect of filter aid type and dosage on the filtration and dewatering performance of positive flotation calcium fluoride

[0049]

[0050]

[0051] Application Example 2

[0052] For application test 17 in application example 1, a reuse test of the filter aid was conducted, and the relevant filtration steps were the same as those described in application example 1. A magnet was used to separate the dried calcium fluoride product and the filter aid, and the recovered mass of the filter aid was recorded. The mass of the filter aid was slightly lost, mainly due to adhesion to the vessel wall and filter paper during the filtration process. The recovered filter aid was used to conduct the same application test, and was recycled 5 times according to the above method. The corresponding effects are shown in Table 2. The filter aid prepared in the embodiment still maintains excellent filter dehydration performance during five repeated uses.

[0053] Table 2 Filtration results of using the filter aid of test 17 in Example 1 for five times

[0054] Number of times of reuse Filter aid recovery amount / g Filter aid dosage / g Filter time / s Wet cake moisture content / % 1 1.92 1.92 667 28.75 2 1.83 1.83 731 29.04 3 1.76 1.76 780 29.35 4 1.66 1.66 825 29.72 5 1.58 1.58 852 30.22

[0055] The present invention and its embodiments are described above, but such description is not restrictive. The application example is only one of the embodiments of the present invention, and the actual application mode is not limited thereto. In short, if ordinary technicians in this field are inspired by it, without departing from the purpose of the invention, they can creatively design filter aids and embodiments similar to the technical solution, which should all fall within the protection scope of the present invention.

Claims

1. A magnetic filter aid for positive flotation of calcium fluoride filtration and dehydration of fluoride-containing sludge, Features: The main component is hydrophobically modified natural magnetite powder with a particle size of 150~270μm and a saturation magnetization intensity greater than 50emu / g.

2. A method for producing a magnetic filter aid for positive flotation of calcium fluoride filtration and dehydration of fluoride-containing sludge as claimed in claim 1, Features: The following steps are involved: Step 1 Preparation of natural magnetite powder The natural magnetite particles are ground in a dry ball mill, and sieved through 50-mesh and 100-mesh sieves to obtain natural magnetite powder with a particle size of 150-270 μm; Step 2: Hydrophobic modification of natural magnetite powder using hydrophobic silane surface modifier Weigh 50 g of the natural magnetite powder obtained in step 1, add it to 500 mL of ethanol solution of silane surface modifier (volume fraction is 1%~6%), ultrasonically disperse it for 15~30 minutes, stir and react at 30°C and 300 rpm for 12~24 hours, use a magnet to separate the solid and liquid, place the solid sample in an oven at 120°C and dry it for 2 hours to obtain hydrophobically modified natural magnetite powder.

3. A method for manufacturing a magnetic filter aid for positive flotation of calcium fluoride filtration and dehydration of fluoride-containing sludge according to claim 2, Features: In the step 1, the natural magnetite ore is provided by an iron mine in Panzhihua, Sichuan, and is processed into natural magnetite ore particles of about 3 mm by a crusher.

4. A method for manufacturing a magnetic filter aid for positive flotation of calcium fluoride filtration and dehydration of fluoride-containing sludge according to claim 2, Features: In the step 1, the grinding process in the ball mill is as follows: 2 kg of natural magnetite particles are weighed and added into the ball mill, and ground for 5 to 10 minutes.

5. A method for manufacturing a magnetic filter aid for positive flotation of calcium fluoride filtration and dehydration of fluoride-containing sludge according to claim 2, Features: In step 2, the silane surface modifier is one of silane coupling agents with different carbon chain lengths, specifically one of methyltrimethoxysilane, propyltrimethoxysilane, octyltrimethoxysilane, dodecyltrimethoxysilane, and hexadecyltrimethoxysilane.