Silicon-based adsorbing material as well as preparation method and application thereof
A silicon-based adsorption material effectively separates and removes trace thorium from rare earth elements, enhancing product quality and environmental compliance by utilizing a coupled silicon sphere compound, addressing the challenges of thorium contamination in existing technologies.
Patent Information
- Application Number
- CN202310657082.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-05
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2043-06-05
AI Technical Summary
Existing methods struggle to effectively separate and remove trace thorium from rare earth elements, which affects the quality of high-purity rare earth products and poses environmental risks due to thorium's radioactive nature, and thorium contamination in waste liquids exceeds emission standards.
A silicon-based adsorption material is developed, comprising silicon spheres coupled with a specific compound (Formula I) using a silane coupling agent, allowing for selective extraction and separation of thorium from rare earth solutions and industrial wastewaters.
The silicon-based adsorption material achieves high selectivity and efficiency in thorium removal, improving product purity and meeting environmental standards, with the ability to regenerate and recycle the adsorbent.
Smart Images

Figure CN119075921A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of thorium extraction, and in particular to a silicon-based adsorption material for extracting thorium, a preparation method thereof and application thereof. Background Art
[0002] The radioactive thorium element has similar chemical properties to rare earths and is usually found in rare earth ores. Compared with trivalent rare earth elements, thorium has a stronger ability to be extracted. Therefore, in the process of extracting rare earths, the presence of thorium will reduce the extraction ability of the extractant for trivalent rare earths and affect the separation effect of rare earths.
[0003] In a single high-purity rare earth product, the presence of trace thorium will seriously affect the product quality. For example, the particle radiation generated by the trace thorium remaining in the rare earth oxide will damage the rare earth doped barium titanate ceramics, resulting in a decrease in photocurrent and an increase in dark current; the radioactive impurity content index of the high-purity tungsten oxide used in the positron emission tomography (PET) system is required to be less than 0.5ppm of radioactive element thorium; and if the domestic high-purity lutetium oxide product contains 0.54-18ppm thorium, the resulting radioactive background will directly affect the light output performance of the scintillation crystal device made of lutetium oxide.
[0004] In addition, there is still a small amount of thorium in the waste liquid generated by the rare earth separation industry that cannot be easily removed, so it is necessary to deeply remove the thorium contained in the waste liquid to make it meet the emission standards of the "Rare Earth Industry Pollutant Emission Standard" (GB26451-2011) (the total amount of radioactive elements thorium and uranium is not higher than 0.1mg / L). Therefore, based on environmental impact and economic factors, it is very urgent to develop a deep thorium removal technology.
[0005] At present, solvent extraction is widely used to separate and enrich thorium from rare earth solutions. CN201610533648.4 discloses a method for removing radioactive thorium from lanthanum chloride solution, wherein lanthanum chloride is extracted with saponified P507 extractant for 5 to 15 levels, washed with 0.5 to 3 mol / L hydrochloric acid for 10 to 40 levels, and stripped with 4 to 5 mol / L hydrochloric acid. The total number of extraction, washing and stripping in the embodiment is 35 to 54 levels. CN201510148009.1 discloses a method for extracting high-purity thorium from excellent slag, wherein dimethylheptyl methylphosphonate (P350) is used as an extractant and kerosene is used as a diluent. The number of extraction levels is 4 to 20, the number of washing levels is 4 to 20, and the number of stripping levels is 4 to 20. The total number of extraction, washing and stripping in the embodiment is 21 to 35. It can be seen that it is difficult to achieve effective separation of thorium and rare earth with limited extraction levels.
[0006] Therefore, it is necessary to further develop new and effective methods for separating thorium and rare earths. Summary of the invention
[0007] The adsorption method is particularly suitable for the enrichment and separation of low-concentration ions, and has the advantages of high selectivity, small amount of secondary waste, and easy desorption. Therefore, a highly selective adsorbent for the radioactive element thorium is invented, and the solid-liquid adsorption method is used to separate and remove trace thorium from various types of feed liquids. This can not only eliminate the radioactive pollution of thorium to the environment and high-purity rare earth products, but also provide a reference and reference for the extraction and separation of thorium from other rare earth mineral leaching solutions, which is of great significance to the green and sustainable development of the rare earth industry.
[0008] Based on this, the inventors designed and prepared a silicon-based adsorption material, and experimentally confirmed that it can be used to selectively extract thorium from a mixture of thorium and rare earth, and then used to remove thorium from rare earth leachate or rare earth industrial wastewater, thereby completing the present invention.
[0009] In one aspect, the present invention provides a silicon-based adsorption material comprising:
[0010] (1) Silicon balls;
[0011] (2) Compound of formula I coupled with silicon spheres:
[0012]
[0013] Wherein, R1 is selected from C1-C 10 Alkyl, C6-C 10 Aryl, C6-C 10 Aryl C1-C2 alkyl, C3-C 10 Cycloalkyl, C3-C 10 Cycloalkyl C1-C2 alkyl;
[0014] R2 and R3 are each independently selected from hydrogen, C1-C4 alkyl, C3-C 10 Cycloalkyl, C3-C 10 Cycloalkyl C1-C2 alkyl, C6-C 10 Aryl, C6-C 10 Aryl C1-C2 alkyl;
[0015] R4 is selected from C1-C 10 Alkyl, C3-C6 cycloalkyl, C3-C6 cycloalkylC1-C2 alkyl, C6-C 10 Aryl, C6-C 10 Aryl C1-C2 alkyl.
[0016] In some embodiments, R1 is selected from C1-C8 alkyl, phenyl, C1-C4 alkylphenyl, phenyl C1-C2 alkyl, in particular, R1 is selected from C2-C8 alkyl, phenyl, tolyl, xylyl, ethylphenyl, benzyl, phenethyl.
[0017] In some embodiments, R2 and R3 are each independently selected from hydrogen, C1-C4 alkyl, in particular, R2 and R3 are each independently selected from hydrogen, methyl, ethyl, more particularly, in particular, R2 and R3 are each independently selected from hydrogen, methyl.
[0018] In some embodiments, R4 is selected from C1-C8 alkyl, phenyl, C1-C4 alkylphenyl, phenyl C1-C2 alkyl, in particular, R4 is selected from C2-C8 alkyl, phenyl, tolyl, xylyl, ethylphenyl, benzyl, phenethyl.
[0019] In some embodiments, the compound of formula I is selected from one or more of the following compounds:
[0020]
[0021]
[0022] In the present invention, silica spheres, sometimes also referred to as silica gel, refer to silica microspheres. There is no particular limitation on the silica spheres, as long as they are suitable for use as a chromatographic column substrate. For example, the silica spheres may have a particle size of 100-200 mesh, and / or: 300-500 m 2 / g specific surface area, but not limited thereto.
[0023] The compound of formula I can be coupled to the silicon sphere by any suitable method, as long as the method does not affect the purpose of the final application. For example, the compound of formula I can be modified so that it has a group that can react with the surface of the silicon sphere, and then react with the silicon sphere to couple to the surface of the silicon sphere, or the surface of the silicon sphere can be modified so that it has a group that can react with the compound of formula I, and then react with the compound of formula I to couple the compound of formula I to the surface of the silicon sphere.
[0024] In some embodiments, in the silicon-based adsorption material, the compound of formula I is coupled to the surface of the silicon sphere through the nitrogen on it. For example, the silicon-based adsorption material may include a structure of formula III:
[0025]
[0026] Wherein, R1 to R4 are defined as above, and X represents a linking group. However, the structure of formula III is only schematic, and the structure of the silicon-based adsorbent material of the present invention is not limited to formula III. For example, multiple compounds of formula I may be coupled to a silicon ball, and the connection between the linking group X and the silicon ball may not be a single bond, but connected via multiple bonds.
[0027] In some embodiments, in the silicon-based adsorption material, the compound of formula I is coupled to the silicon sphere via a silane coupling agent, that is, the silicon-based adsorption material has the following structure: silicon sphere-silane coupling agent-compound of formula I.
[0028] Here, the silane coupling agent acts as a linker. On the one hand, it is connected to the silicon sphere through the action of the inorganic-philic group of the silane coupling agent (i.e., the siloxy group of the silane coupling agent) and the surface group of the silicon sphere. On the other hand, it is covalently connected to the compound of formula I through the organic-philic group of the silane coupling agent (i.e., the organic functional group of the silane coupling agent), thereby coupling the compound of formula I to the silicon sphere to obtain the silicon-based adsorption material.
[0029] The silane coupling agent can be any silane coupling agent that can achieve the above-mentioned purpose.
[0030] In some embodiments, the silane coupling agent has a functional group that can directly react with the amine group in the structure of the compound of Formula I. In this case, the silane coupling agent can be directly reacted with the compound of Formula I to covalently connect one end of the silane coupling agent to the amine group in the structure of the compound of Formula I through the reaction of the organic functional group of the silane coupling agent with the amine group in the structure of the compound of Formula I. In this case, X in Formula III is a group derived from the silane coupling agent.
[0031] In some embodiments, the silane coupling agent is represented by the following formula II:
[0032]
[0033] Wherein, R5, R6 and R7 are each independently selected from C1-C4 alkyl and C1-C4 alkoxy, and at least one is an alkoxy; preferably, they are each independently selected from C1-C2 alkyl (methyl, ethyl) and C1-C2 alkoxy (methoxy, ethoxy), and at least one is an alkoxy;
[0034] R8 is selected from halogen (especially Cl, bromine and iodine), epoxy (ie oxirane), epoxymethoxy (ie glycidyloxy) and isocyanate;
[0035] n is an integer from 1 to 8.
[0036] In some embodiments, the silane coupling agent is selected from epoxy silane, halogen silane, isocyanate silane, which respectively have epoxy groups, halogen groups and isocyanate groups that can react with amine groups. These silanes can be trialkoxy silanes, dialkoxy silanes or monoalkoxy silanes.
[0037] Epoxysilane refers to a silane coupling agent with at least one epoxy group in the molecule. For example, epoxysilane can be 3-(2,3-epoxypropyloxy)propyltrimethoxysilane (KH-560), 5,6-epoxyhexyltriethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 3-(2,3-epoxypropyloxy)propyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-[(2,3)-epoxypropyloxy]propylmethyldimethoxysilane, 3-(2,3-epoxypropyloxy)propyltrimethoxysilane, (3-epoxypropyloxy)dimethylethoxysilane, etc., but are not limited thereto.
[0038] When epoxy silane is used as a silane coupling agent, the epoxy group in the epoxy silane can undergo an addition reaction with the amine group in the compound structure of Formula I to open the ring and covalently connect one end of the epoxy silane to the amine group in the compound structure of Formula I. In this case, X in Formula III can be represented, for example, as etc., wherein R6, R7 and n are as defined above.
[0039] Halogen silane refers to a silane coupling agent with at least one halogen group in the molecule. Halogen includes fluorine, chlorine, bromine and iodine. The halogen groups particularly common in silane coupling agents are chlorine and bromine. For example, the halogen silane can be 3-bromopropyltrimethoxysilane, 4-bromobutyltrimethoxysilane, 5-bromopentyltrimethoxysilane, 7-bromoheptyltrimethoxysilane, 3-chloroisopropyltrimethoxysilane, chloromethyltrimethoxysilane, chloromethyltriethoxysilane, 3-chloropropyltrimethoxysilane, 3-chloropropyltriethoxysilane, 3-iodopropyltrimethoxysilane, chloromethylmethyldiethoxysilane, 3-chloropropylmethyldiethoxysilane, 3-chloropropylmethyltrimethoxysilane, chloromethyldimethylethoxysilane, chloromethyldimethylmethoxysilane, but is not limited thereto.
[0040] When halogen silane is used as a silane coupling agent, halogen silane can be used as a halogenated hydrocarbon to undergo an amination reaction with the amine group in the structure of the compound of formula I, thereby removing the halogen group and making one end of the halogen silane covalently connected to the amine group in the structure of the compound of formula I. In some embodiments, in order to promote the amination reaction, it can be carried out in the presence of an acid binding agent. Common acid binding agents are, for example, 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU), but are not limited thereto. At this time, X in formula III can be represented, for example, as wherein R6, R7 and n are as defined above.
[0041] Isocyanate silane refers to a silane coupling agent with at least one isocyanate in the molecule. For example, the isocyanate silane can be 3-isocyanate propyl triethoxy silane, 3-isocyanate propyl trimethoxy silane, 3-isocyanate propyl methyl diethoxy silane, 3-isocyanate propyl methyl dimethoxy silane, etc., but is not limited thereto.
[0042] When isocyanate silane is used as a silane coupling agent, the isocyanate group in the isocyanate silane can undergo a nucleophilic addition reaction with the amine group in the compound structure of Formula I to generate a urea group and covalently connect one end of the isocyanate silane to the amine group in the compound structure of Formula I. In this case, X in Formula III can be represented, for example, as wherein R6, R7 and n are as defined above.
[0043] The silane coupling agent can also be hydroxysilane, aldehyde silane, carboxyl silane, etc., and one end of the silane coupling agent is covalently connected to the amine group in the structure of the compound of formula I through the reaction of hydroxyl, aldehyde, carboxyl and other groups with amine groups.
[0044] In other embodiments, the silane coupling agent does not have a functional group that can directly react with the amine group in the structure of the compound of formula I. In this case, one end of the silane coupling agent can be covalently connected to the amine group in the structure of the compound of formula I through a connecting group by adding another compound that plays a connecting role as a connecting agent, or the silane coupling agent can be modified to have a functional group that can directly react with the amine group in the structure of the compound of formula I.
[0045] There is no particular limitation on the source of the compound of formula I. The compound of formula I may be commercially available, or may be synthesized by a person skilled in the art by designing a synthetic route based on its structure in combination with a synthetic method in organic chemistry, or may be synthesized similarly to the method described below and in the examples.
[0046] For example, compounds of formula I can be synthesized as follows:
[0047]
[0048] As shown in the reaction formula, the compound of formula IA is hydrolyzed to obtain the compound of formula I,
[0049] Here, R1 to R4 are as defined above, and R1' is defined the same as R1.
[0050] There is no particular limitation on the source of the compound of formula IA. The compound of formula IA may be commercially available, or may be synthesized by a person skilled in the art according to a synthetic route designed based on its structure in combination with synthetic methods in organic chemistry. For example, the compound of formula IA may be synthesized according to known methods in the prior art (such as patent 201610227923X).
[0051] Based on the known structure of the silicon-based adsorbent material according to the present invention, those skilled in the art can design a synthesis route and synthesize it according to its structure in combination with the synthesis method in organic chemistry, for example, it can be synthesized similarly with reference to the method in the existing literature (Functionalisation of mesoporous silica gel with 2-[(phosphonomethyl)-amino]acetic acid functional groups. Characterisation and application, Applied Surface Science, Volume 288, 1 January 2014, Pages 373-380). Alternatively, the silicon-based adsorbent material according to the present invention can be synthesized by the following method or with reference to the method disclosed in the examples of the present application.
[0052] In some embodiments, a method for preparing the above silicon-based adsorption material is provided, comprising:
[0053] (1) coupling the compound of formula I with a silane coupling agent of formula II to obtain a coupling compound of formula IV;
[0054]
[0055] (2) allowing the coupling compound of formula IV to undergo a coupling reaction with silicon spheres to obtain a silicon-based adsorption material;
[0056] wherein R1 to R8, n are as defined above, and L is selected from a direct bond,
[0057] In step (1), the molar ratio of the compound of formula I to the silane coupling agent of formula II is not particularly limited as long as the target compound can be obtained, for example, it can be 1:0.5-1.5, for example, 1:0.8-1.2, for example, 1:1.0, 1:1.1, etc.
[0058] Step (1) can be carried out in an organic solvent. There is no particular limitation on the type of organic solvent, as long as it has no adverse effect on the reaction. For example, the organic solvent includes, but is not limited to, methanol, ethanol, acetonitrile, tetrahydrofuran, and dioxane, and can be any one or more thereof.
[0059] The reaction temperature of step (1) is not particularly limited as long as the coupling reaction can be carried out. For example, the reaction temperature can be 50-100°C, such as 65-80°C, such as 65°C, 70°C, 75°C or 80°C, but is not limited thereto.
[0060] The reaction time of step (1) is not particularly limited as long as the desired target compound can be obtained. For example, the reaction time can be 2 hours or more, 5 hours or more, 10 hours or more, 12 hours or more, for example, 12-72 hours, 24-40 hours, for example, 24 hours, 28 hours, 32 hours, 36 hours or 40 hours, but is not limited thereto.
[0061] In step (2), the mass ratio of the coupling compound of formula IV to the silicon spheres is not particularly limited, for example, it can be 1:0.5-5, for example, 1:0.8-4, for example, 1:1.0, 1:1.5, 1:2.0, 1:3.0, etc., but is not limited thereto.
[0062] Step (2) can be carried out in an organic solvent. There is no particular limitation on the type of organic solvent, as long as it has no adverse effect on the reaction. For example, the organic solvent includes but is not limited to toluene, xylene, trimethylbenzene, cyclohexane, n-heptane, isooctane, and can be any one or more thereof.
[0063] The reaction temperature of step (2) is not particularly limited as long as the coupling reaction can be carried out. For example, the reaction temperature can be 60-150°C, such as 80-120°C, such as 90°C, 100°C, 110°C or 120°C, but is not limited thereto.
[0064] The reaction time of step (2) is not particularly limited as long as the desired target product can be obtained. For example, the reaction time can be more than 2 hours, more than 5 hours, more than 10 hours, more than 12 hours, such as 12-96 hours, 48-72 hours, such as 48 hours, 54 hours, 60 hours, 66 hours or 72 hours, but is not limited thereto.
[0065] Another aspect of the present invention provides a coupling compound of formula IV:
[0066]
[0067] wherein R1 to R7 and n are as defined above, and L is selected from a direct bond,
[0068] The present invention has been experimentally verified that the silicon-based adsorption material of the present invention can be used as an extractant to extract thorium with high selectivity, thereby separating thorium from rare earth elements.
[0069] Therefore, another aspect of the present invention provides the use of the obtained silicon-based adsorption material in preparing an extractant for extracting thorium. The extractant here is sometimes also called an adsorbent.
[0070] Another aspect of the present invention provides a method for extracting thorium, the method comprising the step of contacting a thorium-containing feed liquid with the silicon-based adsorbent material of the present invention to extract thorium from the feed liquid. After the thorium is extracted, the silicon-based adsorbent material adsorbs thorium, which is sometimes referred to as a thorium-containing silicon-based adsorbent material.
[0071] In one embodiment, the method for extracting thorium according to the present invention further comprises: optionally washing the thorium-containing silicon-based adsorption material with a washing liquid, and stripping the thorium in the silicon-based adsorption material with a stripping liquid.
[0072] The washing process can remove the impurity elements adsorbed by the silicon-based adsorbent material, improve the purity of the thorium adsorbed on the silicon-based adsorbent material, and thus help improve the purity of the final thorium product. The washing liquid can be nitric acid, sulfuric acid, hydrochloric acid or a mixed solution of the above acids in any proportion. The acidity of the washing liquid is calculated as the hydrogen ion molar concentration, which is about 0.2 to 8 mol / L.
[0073] The stripping process is used to elute thorium in the silicon-based adsorbent material to obtain a thorium-containing stripping product, and then produce a thorium product. The stripping solution can also be called a stripping solution, a stripping agent or a stripping solution, which is a mixed solution of nitric acid, hydrochloric acid, sulfuric acid or the above acids, or a carbonate aqueous solution. The carbonate can be an alkali metal salt, an alkaline earth metal salt or an ammonium salt, such as a sodium salt, a potassium salt, etc. Preferably, when an acid solution is used as a stripping solution, the acidity is about 0.05 to 2 mol / L calculated as the molar concentration of hydrogen ions; when a sodium carbonate aqueous solution is used, its concentration can be about 0.5 to 5 wt%. Preferably, the stripping solution is a dilute nitric acid with a concentration of about 0.1 to 0.5 mol / L or a sodium carbonate aqueous solution with a concentration of about 0.5 to 3 wt%.
[0074] The silicon-based adsorption material after stripping can be recycled and used again to extract and separate thorium from the thorium-containing liquid.
[0075] The thorium-containing feed liquid contains thorium and mineral acid and other non-thorium elements. Among them, the thorium concentration can be about 0.0001-2.0 mol / L, preferably about 0.0003-1 mol / L. In addition, the feed liquid may also contain other elements such as rare earth, alkali metal, alkaline earth metal, transition metal and non-metallic elements. There is no restriction on the raw materials for preparing the thorium-containing feed liquid, as long as it contains thorium. Raw materials suitable for preparing the feed liquid include various thorium-containing raw materials, such as monazite, bastnaesite, mixed ore of bastnaesite and monazite, thorium enrichment, etc. The above-mentioned thorium-containing raw materials are pretreated and dissolved with nitric acid, hydrochloric acid, sulfuric acid, phosphoric acid or a mixed acid thereof to obtain a feed liquid suitable for the method of the present invention. In addition, in practical applications, the feed liquid may also contain other elements such as rare earth, alkali metal, alkaline earth metal, transition metal and non-metallic elements (the type and content of which depend on the composition of the thorium raw material mineral). In this case, the method of the present invention can be used to extract and separate thorium with high selectivity, thereby separating it from non-thorium impurity elements.
[0076] In some embodiments, the thorium-containing solution may also be a high-purity rare earth solution, a rare earth leaching solution, or a rare earth industrial wastewater solution, but is not limited thereto.
[0077] Preferably, the pH of the thorium-containing feed solution can be 0 to 4, preferably 1-4, such as 1.5, 2, 2.5, 3, 3.5, etc., but not limited thereto. Within the above pH range, it is beneficial for the silicon-based adsorbent material of the present invention to maintain a relatively high adsorption capacity, thereby efficiently extracting thorium. In the case of exceeding the above pH range, the adsorption capacity of the silicon-based adsorbent material of the present invention will be reduced, resulting in reduced extraction efficiency. Therefore, when the pH of the original thorium-containing feed solution (such as high-purity rare earth feed solution, rare earth leaching solution, rare earth industrial wastewater feed solution) is not within the above range, it is preferred to adjust the pH of the original thorium-containing feed solution to the above range to improve the extraction efficiency of thorium. The thorium-containing feed solution is generally a nitric acid, sulfuric acid or hydrochloric acid solution, but not limited thereto. Therefore, the present invention also provides a method for separating thorium from a thorium-containing high-purity rare earth feed solution, the method comprising the step of contacting the thorium-containing high-purity rare earth feed solution with the silicon-based adsorbent material of the present invention to extract thorium from the feed solution. The concentration of thorium in the thorium-containing high-purity rare earth solution can be above 0.1ppm, above 0.5ppm, or above 1ppm. There is no particular limit on the upper limit of the concentration, for example, it can be below 1000ppm, below 500ppm, etc. The "high-purity rare earth solution" here can be a solution of a single rare earth element, which can be a solution obtained in the production process of high-purity rare earth products, or a solution obtained by treating a rare earth product with a single rare earth element purity of 99.9% or more. After treatment, the removal rate of thorium in the thorium-containing high-purity rare earth solution can reach more than 90%, especially more than 95%, or even more than 97%.
[0078] The present invention also provides a method for separating thorium from a rare earth leachate containing thorium, the method comprising the step of contacting the rare earth leachate containing thorium with the silicon-based adsorption material of the present invention to extract thorium from the rare earth leachate. The rare earth leachate contains rare earth, thorium and mineral acid and other non-thorium elements, the specific types and contents of which depend on the composition of the rare earth raw material mineral. In addition, the rare earth leachate may also contain other elements such as alkali metals, alkaline earth metals, transition metals and non-metallic elements. The raw materials suitable for preparing the rare earth leachate include various rare earth raw materials, such as rare earth minerals, rare earth enriched materials, etc. The above-mentioned rare earth-containing raw materials are pretreated and dissolved with nitric acid, hydrochloric acid, sulfuric acid, phosphoric acid or a mixed acid thereof to obtain a rare earth leachate suitable for the method of the present invention. After treatment, the removal rate of thorium in the rare earth leachate can reach more than 90%, especially more than 95%, or even more than 97%.
[0079] The present invention also provides a method for separating thorium from thorium-containing rare earth industrial wastewater, the method comprising the step of contacting the thorium-containing rare earth industrial wastewater with the silicon-based adsorbent material of the present invention to extract thorium from the rare earth industrial wastewater. "Rare earth industrial wastewater" refers to waste liquid generated by the rare earth separation industry, which contains a small amount of rare earth elements (e.g., each rare earth element of more than 1 mmol / L, more than 10 mmol / L, and less than 200 mmol / L, less than 100 mmol / L) and trace amounts of thorium (e.g., thorium of more than 0.1 ppm, more than 0.5 ppm, more than 1 ppm, and less than 1000 ppm, less than 500 ppm). After treatment, the removal rate of thorium in the rare earth industrial wastewater can reach more than 90%, especially more than 95%, or even more than 97%.
[0080] In some embodiments, the method for extracting thorium according to the present invention further comprises the step of regenerating the silicon-based adsorbent material of the present invention. The regeneration can be performed by treating the silicon-based adsorbent material of the present invention with an inorganic acid. The inorganic acid can be selected from hydrochloric acid, sulfuric acid and nitric acid. The thorium adsorbed on the silicon-based adsorbent material can be eluted by regeneration. The eluted thorium can be used to prepare a thorium product after enrichment.
[0081] the term
[0082] In the present invention, "separation of thorium" refers to the extraction of thorium (i.e. tetravalent thorium (IV) or tetravalent thorium ion Th) by extraction. 4 + ) and rare earth (i.e. lanthanide elements or trivalent lanthanide ions Ln 3+ ) separated.
[0083] In the present invention, rare earth elements refer to lanthanum (La), cerium (Ce), praseodymium (Pr), neodymium (Nd), samarium (Sm), europium (Eu), gadolinium (Gd), terbium (Tb), dysprosium (Dy), holmium (Ho), erbium (Er), thulium (Tm), ytterbium (Yb), lutetium (Lu), yttrium (Y) and scandium (Sc).
[0084] In the present invention, C1-C 10 Alkyl refers to a straight or branched chain alkyl group containing 1 to 10 carbon atoms, such as a straight or branched chain alkyl group having 1, 2, 3, 4, 5, 6, 7, 8, 9 or 10 carbon atoms, including but not limited to methyl, ethyl, n-propyl, isopropyl, n-butyl, tert-butyl, isobutyl, n-pentyl, neopentyl, isopentyl, hexyl, heptyl, octyl, nonyl, decyl, etc. The meanings of C1-C8 alkyl, C2-C8 alkyl, C1-C4 alkyl, C1-C2 alkyl, etc. are deduced by analogy.
[0085] In the present invention, C3-C 10 Cycloalkyl refers to a saturated cyclic alkyl group containing 3 to 10 carbon atoms including the carbon number of the substituent, and the saturated cyclic alkyl group may be a monocyclic or bicyclic group, such as cyclopropyl, cyclobutyl, cyclopentyl, methylcyclopentyl, cyclohexyl, methylcyclohexyl, dimethylcyclohexyl, cycloheptyl, cyclooctyl, etc., and the substituent may be one or more substituents selected from C1-C4 alkyl. The meaning of C5-C6 cycloalkyl, etc. is similar.
[0086] In the present invention, C6-C 10 Aryl refers to an aromatic group containing 6 to 10 carbon atoms including the carbon number of substituents, such as phenyl and phenyl substituted with one or more substituents selected from C1-C4 alkyl, such as tolyl, dimethylphenyl, trimethylphenyl, ethylphenyl, etc.
[0087] Unless otherwise specified, the numerical ranges listed in the present invention include the endpoints and all point values therein that are increased or decreased by the smallest unit of the endpoints and all sub-ranges composed of these point values.
[0088] Unless otherwise stated, the numerical values in the present invention represent approximate measurements or limitations of the range of embodiments including slight deviations from given values and having approximately the mentioned values and having the mentioned exact values. Except for the last example described in detail, all numerical values of parameters (e.g., quantities or conditions) in this application document (including the appended claims) should be understood as modified by the term "approximately" in all cases, regardless of whether "approximately" actually appears before the numerical value. "Approximately" means that the numerical value described allows for slight imprecision (some close to precision in the value; approximately or reasonably close to the value; approximately). If the imprecision provided by "approximately" is not understood in this ordinary sense in the art, the "approximately" used herein at least represents the changes that can be produced by ordinary methods of measuring and using these parameters. For example, "approximately" can include less than or equal to 15%, less than or equal to 10%, less than or equal to 5%, less than or equal to 4%, less than or equal to 3%, less than or equal to 2%, less than or equal to 1%, less than or equal to 0.5%, less than or equal to 0.1% of the change, and in some aspects, less than or equal to 0.01% of the change.
[0089] The present invention has been described above in detail, but the present invention is not limited to the above contents.
[0090] Beneficial Effects
[0091] The silicon-based adsorption material of the present invention has the advantages of simple preparation method, wide raw material source and low cost, strong selectivity for thorium, large adsorption capacity, little influence of pH value on adsorption capacity, no saponification agent is used in the removal process, and environmental friendliness. The silicon-based adsorption material can be widely used for removing impurities of thorium ions in high-purity rare earth solutions, and after use, the adsorbent can be regenerated with inorganic acid to complete the recycling of the adsorbent. BRIEF DESCRIPTION OF THE DRAWINGS
[0092] Figure 1 A scanning electron microscope photograph showing the silicon-based adsorption material prepared in Example 1 of the present invention.
[0093] Figure 2 The infrared spectra of the silicon spheres and the prepared silicon-based adsorption material used in Example 1 of the present invention are shown. DETAILED DESCRIPTION
[0094] In order to further illustrate the solutions of the present invention, specific embodiments of the present invention are provided to help those skilled in the art understand and implement the present invention, but the present invention is not limited to these embodiments.
[0095] In addition, it should be noted that the structure of the silicon-based adsorption material given here is schematic and does not constitute a limitation to the present invention.
[0096] Example
[0097] Reagents and sources
[0098] Bis(2-ethylhexyl)phosphite, diphenyl phosphite, diethyl phosphite, and dibenzyl phosphite were purchased from Shanghai Lai Ya Shi Chemical Co., Ltd. Paraformaldehyde, 2-ethylhexylamine, isobutylamine, cyclopropylmethylamine, cyclohexylmethylamine, 3-chloropropyltrimethoxysilane, and γ-glycidyloxypropyltrimethoxysilane were purchased from Aladdin Reagent Co., Ltd.
[0099] The silica spheres were purchased from Qingdao Jiyida Silica Sphere Reagent Factory. The particle size was 100-200 mesh and the specific surface area was 400-500m 2 / g. The silicon spheres were activated before use.
[0100] Other reagents (such as acids, organic solvents, etc.) were all commercially available analytical grade reagents.
[0101] The purity of the product was determined by ICP-OES (instrument model: PQ9000, manufacturer: Jena) and ICP-MS (instrument model: Agilent 8900, manufacturer: Agilent).
[0102] The NMR instrument was Varian Mercury 300.
[0103] The high-resolution field emission scanning electron microscope was JSM-IT800.
[0104] The Fourier transform infrared spectrometer was iS5.
[0105] Example 1: Preparation of 2-ethylhexylaminomethylphosphonic acid monophenyl ester silicon-based adsorption material
[0106] (1) Preparation of 2-ethylhexylaminomethylphosphonic acid diphenyl ester
[0107]
[0108] In a single-necked flask equipped with a mechanical stirrer and a condensing reflux device, diphenyl phosphite (1 mol), paraformaldehyde (1.1 mol), 2-ethylhexylamine (1.1 mol), acetonitrile (800 ml) and p-toluenesulfonic acid (0.8 g) were added, stirred and refluxed, and reacted at 80-90° C. for 8 h. The acetonitrile was removed by rotary evaporation, and the residue was washed with an aqueous sodium carbonate solution equivalent to p-toluenesulfonic acid and a hydrochloric acid equivalent to 2-ethylhexylamine in turn to remove unreacted products, and 2-ethylhexylaminomethylphosphonic acid diphenyl ester was obtained, which was directly used in the next step.
[0109] (2) Preparation of 2-ethylhexylaminomethylphosphonic acid monophenyl ester
[0110]
[0111] The 2-ethylhexylaminomethylphosphonic acid diphenyl ester obtained in step (1) was added to a single-necked flask, and then potassium hydroxide aqueous solution (1.5 mol, 600 ml) and ethanol (800 ml) were added, stirred and refluxed, and reacted at 80-90° C. for 36 hours. After removing the ethanol by rotary evaporation, the residue was washed with a slightly excess amount of hydrochloric acid relative to potassium hydroxide to remove potassium hydroxide, and then dried with excess anhydrous Na2SO4 to obtain 2-ethylhexylaminomethylphosphonic acid monophenyl ester, which was directly used in the next step.
[0112] (3) Preparation of coupling compounds
[0113]
[0114] Add 2-ethylhexylaminomethylphosphonic acid monophenyl ester (1 mol) prepared in step (2) into a single-necked flask, then add γ-glycidyloxypropyltrimethoxysilane (1.2 mol) and acetonitrile (800 ml), stir and reflux, react at 65-85°C for 24 hours, and remove acetonitrile by rotary evaporation to obtain a coupling compound, which is directly used in the next step.
[0115] (4) Preparation of silicon-based adsorption materials
[0116]
[0117] The coupling compound (1 mol) prepared in step (3) was added into a single-necked flask, and then silicon balls (150 g) and toluene (800 ml) were added, stirred and refluxed, reacted at 105-115° C. for 48 h, and toluene was removed by rotary evaporation. The mixture was washed with deionized water and ethanol in turn, and vacuum dried to obtain a silicon-based adsorption material.
[0118] Silicon-based adsorption materials: 1 H NMR (500MHz, CDCl3) δ7.01-6.93 (m, Ph-H), 4.63-3.47 (m, Si-H, Si-OH), 1.72-0.62 (m, CH, CH2, CH3)
[0119] Figure 1 The scanning electron microscope image of the silicon-based adsorbent prepared above is shown. The image shows that the silicon-based adsorbent material basically maintains the original shape of the silicon sphere.
[0120] Figure 2 Infrared spectra of silicon spheres (SG) and the silicon-based adsorbent material (SG-PHO) prepared above are shown.
[0121] For silicon sphere (SG), 1079.00cm -1 The strong peak at 808.27cm is the antisymmetric absorption peak of the silicon-based framework Si-O-Si. -1 and 464.21cm -1The two peaks appearing at 1092.18 cm-1 are the stretching vibration and bending vibration peaks of Si-O-Si. These three peaks are characteristic peaks of silicon-based carriers. For the adsorbent (SG-PHO), the positions of the three peaks are at 1092.18 cm-1. -1 , 803.21cm -1 , 461.18cm -1 , there was no significant change after modification, indicating that cross-linking the coupling compound to the silica spheres did not affect the chemical structure of the silica spheres. In addition, the silica spheres (SG) and the silica-based adsorbent (SG-PHO) at 3450 cm -1 The large absorption peak on the left and right can be considered as the stretching vibration peak of the silanol group OH on the silica surface and the physically adsorbed water OH on the surface.
[0122] It is worth noting that silica spheres (SG) at 970 cm -1 There is a side peak at , which is caused by the stretching vibration of the silanol group. In contrast, the peak of the silicon-based adsorbent (SG-PHO) disappears at this position, indicating that most of the active sites on the surface of the silicon sphere have been successfully grafted.
[0123] In addition, for silicon-based adsorbent material (SG-PHO), 2927.44 cm -1 The peak of CH stretching vibration is 1641.17 cm -1 The peak at 1400 cm is the bending vibration peak of the silanol OH and the surface physically adsorbed water OH. -1 Up to 1450cm -1 A series of peaks are CH bending vibration peaks on saturated hydrocarbons or benzene rings. -1 There is a small peak at 1000cm, which can be considered as the stretching vibration peak of P=O. The PO bond and the CN bond generally exist at 1000cm -1 Up to 1100cm -1 At 889.32cm, it is blocked by the antisymmetric absorption peak of Si-O-Si to form a giant peak. -1 The out-of-plane bending vibration peak of 1-substituted benzene.
[0124] The above infrared results show that the coupling compound is successfully grafted onto the surface of silicon spheres in the silicon-based adsorption material.
[0125] Example 2: Preparation of 2-ethylhexylaminomethylphosphonic acid monobenzene silicon-based adsorption material
[0126] The target silicon-based adsorption material was prepared by the same process as in Example 1 except that diphenyl phosphite was used instead of diphenyl phosphite.
[0127] (1) 2-Ethylhexylaminomethylphosphonic acid dibenzyl ester
[0128]
[0129] (2) 2-Ethylhexylaminomethylphosphonic acid monoester
[0130]
[0131] (3) Coupling compounds
[0132]
[0133] (4) Silicon-based adsorption materials
[0134]
[0135] Silicon-based adsorption materials: 1 H NMR (500MHz, CDCl3) δ7.06-6.97 (m, Ph-H), 4.47-3.59 (m, Si-H, Si-OH), 1.04-0.61 (m, CH, CH2, CH3)
[0136] Example 3: Preparation of 2-ethylhexylaminomethylphosphonic acid monoethyl ester silicon-based adsorption material
[0137] The target silicon-based adsorption material was prepared by the same process as in Example 1 except that diethyl phosphite was used instead of diphenyl phosphite.
[0138] (1) Diethyl 2-ethylhexylaminomethylphosphonate
[0139]
[0140] (2) 2-Ethylhexylaminomethylphosphonic acid monoethyl ester
[0141]
[0142] (3) Coupling compounds
[0143]
[0144] (4) Silicon-based adsorption materials
[0145]
[0146] Silicon-based adsorption materials: 1 H NMR (500MHz, CDCl3) δ4.25-3.40 (m, Si-H, Si-OH), 1.09-0.66 (m, CH, CH2, CH)
[0147] Example 4: Preparation of 2-ethylhexylaminomethylphosphonic acid mono(2-ethylhexyl) ester silicon-based adsorption material
[0148] The target silicon-based adsorption material was prepared by the same process as in Example 1 except that bis(2-ethylhexyl)phosphite was used instead of diphenyl phosphite.
[0149] (1) 2-Ethylhexylaminomethylphosphonic acid di(2-ethylhexyl) ester
[0150]
[0151] (2) 2-Ethylhexylaminomethylphosphonic acid mono(2-ethylhexyl) ester
[0152]
[0153] (3) Coupling compounds
[0154]
[0155] (4) Silicon-based adsorption materials
[0156]
[0157] Silicon-based adsorption materials: 1 H NMR (500MHz, CDCl3) δ4.39-3.28 (m, Si-H, Si-OH), 1.15-0.59 (m, CH, CH2, CH3)
[0158] Example 5: Preparation of 2-methylpropylaminomethylphosphonic acid monophenyl ester silicon-based adsorption material
[0159] The target silicon-based adsorption material was prepared by the same process as in Example 1 except that isobutylamine was used instead of 2-ethylhexylamine.
[0160] (1) 2-Methylpropylaminomethylphosphonic acid diphenyl ester
[0161]
[0162] (2) 2-Methylpropylaminomethylphosphonic acid monophenyl ester
[0163]
[0164] (3) Coupling compounds
[0165]
[0166] (4) Silicon-based adsorption materials
[0167]
[0168] Silicon-based adsorption materials: 1H NMR (500MHz, CDCl3) δ7.09-6.99 (m, Ph-H), 4.96-3.28 (m, Si-H, Si-OH), 1.45-0.63 (m, CH, CH2, CH3)
[0169] Example 6: Preparation of cyclopropylmethylaminomethylphosphonic acid monophenyl ester silicon-based adsorption material
[0170] The target silicon-based adsorption material was prepared by the same process as in Example 1 except that cyclopropylmethylamine was used instead of 2-ethylhexylamine.
[0171] (1) Cyclopropylmethylaminomethylphosphonic acid diphenyl ester
[0172]
[0173] (2) Cyclopropylmethylaminomethylphosphonic acid monophenyl ester
[0174]
[0175] (3) Coupling compounds
[0176]
[0177] (4) Silicon-based adsorption materials
[0178]
[0179] Silicon-based adsorption materials: 1 H NMR (500MHz, CDCl3) δ7.04-6.85 (m, Ph-H), 4.83-3.31 (m, Si-H, Si-OH), 1.38-0.59 (m, CH, CH2, CH3)
[0180] Example 7: Preparation of cyclohexylmethylaminomethylphosphonic acid monophenyl ester silicon-based adsorption material
[0181] The target silicon-based adsorption material was prepared by the same process as in Example 1 except that cyclohexylmethylamine was used instead of 2-ethylhexylamine.
[0182] (1) Cyclohexylmethylaminomethylphosphonic acid diphenyl ester
[0183]
[0184] (2) Cyclohexylmethylaminomethylphosphonic acid monophenyl ester
[0185]
[0186] (3) Coupling compounds
[0187]
[0188] (4) Silicon-based adsorption materials
[0189]
[0190] Silicon-based adsorption materials: 1 H NMR (500MHz, CDCl3) δ7.12-6.96 (m, Ph-H), 4.79-3.42 (m, Si-H, Si-OH), 1.58-0.57 (m, CH, CH2, CH3)
[0191] Example 8: Preparation of 2-ethylhexylaminomethylphosphonic acid monophenyl ester silicon-based adsorption material
[0192] The target silicon-based adsorbent material was prepared by the same process as in Example 1 except that 3-chloropropyltrimethoxysilane was used instead of γ-glycidyloxypropyltrimethoxysilane.
[0193] (3) Coupling compounds
[0194]
[0195] (4) Silicon-based adsorption materials
[0196]
[0197] Silicon-based adsorption materials: 1 H NMR (500MHz, CDCl3) δ6.93-6.65(m,Ph-H), 5.51-3.32(m,Si-H,Si-OH), 3.32(m,Cl-CH2-R), 1.08-0.64(m,CH,CH2,CH3)
[0198] Comparative Example 1: Preparation of 2-ethylhexylaminomethylphosphonic acid diphenyl ester silicon-based adsorption material
[0199] The 2-ethylhexylaminomethylphosphonic acid diphenyl ester silicon-based adsorbent material was prepared according to the method of Example 1, except that the 2-ethylhexylaminomethylphosphonic acid diphenyl ester obtained in step (1) was directly used in step (3) instead of 2-ethylhexylaminomethylphosphonic acid monophenyl ester, and step (2) of hydrolysis with potassium hydroxide was not performed.
[0200]
[0201] Silicon-based adsorption materials: 1H NMR (500MHz, CDCl3) δ6.98-6.84(m,Ph-H), 4.85-3.59(m,Si-H,Si-OH), 1.84-0.57(m,CH,CH2,CH3)
[0202] Comparative Example 2: Preparation of 2-ethylhexylaminomethylphosphonic acid di(2-ethylhexyl) ester silicon-based adsorption material
[0203] The 2-ethylhexylaminomethylphosphonic acid di(2-ethylhexyl) ester silicon-based adsorbent material was prepared according to the method of Example 4, except that the 2-ethylhexylaminomethylphosphonic acid di(2-ethylhexyl) ester obtained in step (1) was directly used in step (3) instead of 2-ethylhexylaminomethylphosphonic acid mono(2-ethylhexyl) ester, and step (2) of hydrolysis with potassium hydroxide was not performed.
[0204]
[0205] Silicon-based adsorption materials: 1 H NMR (500MHz, CDCl3) δ4.49-3.38 (m, Si-H, Si-OH), 1.48-0.52 (m, CH, CH2, CH3)
[0206] Experimental Example 1: Determination of adsorption capacity
[0207] Preparation of feed solution: Take a single solution of thorium chloride, precipitate it with the same amount of sodium carbonate, centrifuge it, add excess sulfuric acid to dissolve the precipitate to obtain a thorium sulfate solution, and titrate it to obtain the concentration of the thorium sulfate solution. Then use distilled water to dilute the thorium sulfate solution to the required concentration. In this way, a Th(IV) feed solution with a concentration of 2mmol / L is prepared.
[0208] 40 mg of the silicon-based adsorbent material obtained in Examples 1 to 8 and Comparative Examples 1-2 was weighed, 8 mL of the above-prepared solution was added, the pH was adjusted to 3.5 using a sulfuric acid solution, and the mixture was shaken at 30°C for 60 h on an air bath thermostatic shaker with an oscillation rate of 300 rpm to perform a static adsorption experiment. After the adsorption was completed, the silicon-based adsorbent material was filtered out, and the filtrate was taken to determine the thorium ion (Th 4+ )concentration.
[0209] Then, the adsorption amount of ions by the silicon-based adsorbent material is calculated using formula (1):
[0210]
[0211] Where, Q represents the adsorption amount (mg / g), C i With C tRespectively represent the concentration of ions before and after adsorption (mg / L), V represents the volume of the feed solution (L), and m represents the amount of silicon-based adsorption material used (g).
[0212] Since thorium ions (Th 4+ ), therefore, the adsorption amount measured above can be regarded as the adsorption capacity of the silicon-based adsorbent material. The adsorption capacity of thorium by the silicon-based adsorbent materials of Examples 1 to 8 and Comparative Examples 1-2 is shown in Table 1.
[0213] Table 1 Adsorption capacity of thorium by silicon-based adsorption materials of various embodiments and comparative examples (mg / g)
[0214]
[0215] Comparing the results of Examples 1 to 8 with Comparative Examples 1 and 2, it can be seen that the silicon-based adsorption material of the present invention has a better adsorption effect on thorium.
[0216] In addition, compared with the 6-toluenesulfonyl ester-β-cyclodextrin bridged diphenylethylenedione (BBβ-CD) adsorbent disclosed in CN105664873A and the hydrogel bead adsorbent disclosed in CN111841512A, the silicon-based adsorbent material of the present invention has a significantly higher adsorption capacity.
[0217] Separation Example 1
[0218] Preparation of simulated mixed rare earth leaching solution: Take single lanthanum sulfate, cerium sulfate, praseodymium sulfate, neodymium sulfate, samarium sulfate, europium sulfate, gadolinium sulfate, terbium sulfate, dysprosium sulfate, holmium sulfate, erbium sulfate, thulium sulfate, ytterbium sulfate, lutetium sulfate, yttrium sulfate and the thorium sulfate solution prepared in Experimental Example 1, calcium sulfate, iron sulfate, magnesium sulfate and aluminum sulfate solution, calculate the required volume of each solution and add distilled water to make up the volume, thereby preparing a mixed rare earth leaching solution containing La(Ⅲ), Ce(Ⅲ), Pr(Ⅲ), Nd(Ⅲ), Sm(Ⅲ), Eu(Ⅲ), Gd(Ⅲ), Tb(Ⅲ), Dy(Ⅲ), Ho(Ⅲ), Er(Ⅲ), Tm(Ⅲ), Yb(Ⅲ), Lu(Ⅲ), Y(Ⅲ), Ca(Ⅱ), Fe(Ⅲ), Mg(Ⅱ), Al(Ⅲ) and Th(Ⅳ) in a sulfuric acid system with a concentration of 2 mmol / L.
[0219] Weigh 40 mg (± 0.02 mg) of the silicon-based adsorbent material prepared in Example 1 and place it in a threaded sample bottle, add the mixed rare earth leaching solution prepared above, adjust the pH to 1, 1.5, 2, 2.5, 3 and 3.5 respectively, and shake at 30°C for 60 hours on an air bath constant temperature shaker with an oscillation rate of 300 rpm to conduct a static adsorption experiment. After the adsorption is completed, filter out the silicon-based adsorbent material, take the filtrate, and test the equilibrium pH. The pH change before and after the adsorption experiment is shown in Table 2. In addition, the concentration of each ion in the solution before and after adsorption was determined by ICP-OES, and then the above formula (1) and the following formula (2) were used to calculate the adsorption amount and adsorption rate of various elements. The results are shown in Table 2.
[0220] The adsorption rate of the silicon-based adsorbent material for the ions to be tested is calculated using formula (2).
[0221]
[0222] Where A represents the adsorption rate (%), C i With C t Represent the concentration of the ion to be measured before and after adsorption (mg / L), respectively.
[0223] Table 2 Adsorption amount Q (mg / g) and adsorption rate A (%) of various elements by silicon-based adsorption materials at different pH values
[0224]
[0225]
[0226] Among them, pH i represents the initial pH, pH e Represents equilibrium pH.
[0227] The results in Table 2 show that, in the case of the coexistence of thorium and rare earth element ions, the silicon-based adsorbent material according to the present invention can selectively adsorb thorium, and basically does not adsorb other elements before thorium is completely adsorbed. In addition, the adsorption of thorium by the silicon-based adsorbent material according to the present invention is less affected by pH.
[0228] Thorium removal from high purity rare earth products
[0229] Separation Example 2
[0230] Simulate the preparation of high-purity rare earth product solution: take a single lanthanum sulfate solution and a single thorium sulfate solution, mix them according to the concentration ratio, add distilled water and use sulfuric acid solution to adjust the pH, and finally fix the volume to prepare a solution with a pH of 3 and a concentration of 20 mmol / L La(III) and 100 ppm Th(IV).
[0231] 25 g of the silicon-based adsorbent obtained in Example 1 was weighed and filled on a chromatography column with a diameter of 1 cm and a total length of 0.5 m. Clean water was passed to wash the adsorbent and compact it. Air was then passed to discharge the water in the column. The above prepared liquid was passed, and the fractions were collected. The concentrations of La(III) and Th(IV) were determined using ICP-OES. After column purification, the residual concentration of thorium was 0.02 ppm, and the removal rate of thorium reached 99.98%.
[0232] Separation Example 3
[0233] Preparation of simulated high-purity rare earth product solution: Take a single lutetium sulfate solution and a single thorium sulfate solution, mix them according to the concentration ratio, add distilled water and use sulfuric acid solution to adjust the pH, and finally make up the volume to prepare a solution containing Lu(III) at a concentration of 20 mmol / L and Th(IV) at a concentration of 200 ppm.
[0234] 50 g of the silicon-based adsorbent obtained in Example 8 was weighed and filled on a chromatography column with a diameter of 1 cm and a total length of 1 m. Clean water was passed to wash the adsorbent and compact it. Air was then passed to discharge the water in the column. The above prepared feed solution was passed, and the fractions were collected. The concentrations of Lu (III) and Th (IV) were determined using ICP-OES. After column purification, the residual concentration of thorium was 4.1 ppm, and the thorium removal rate reached 97.95%.
[0235] Thorium Removal from Rare Earth Leachate
[0236] Separation Example 4
[0237] Preparation of simulated rare earth leaching solution: Take single lanthanum sulfate, cerium sulfate, praseodymium sulfate, neodymium sulfate, samarium sulfate, europium sulfate, gadolinium sulfate, terbium sulfate, dysprosium sulfate, holmium sulfate, erbium sulfate, thulium sulfate, ytterbium sulfate, lutetium sulfate, yttrium sulfate and the above-prepared thorium sulfate solution, mix them according to the concentration ratio, add distilled water and use sulfuric acid solution to adjust the pH, and finally make up the volume. Thus, a feed solution with a pH of 3 and containing La(Ⅲ), Ce(Ⅲ), Pr(Ⅲ), Nd(Ⅲ), Sm(Ⅲ), Eu(Ⅲ), Gd(Ⅲ), Tb(Ⅲ), Dy(Ⅲ), Ho(Ⅲ), Er(Ⅲ), Tm(Ⅲ), Yb(Ⅲ), Lu(Ⅲ), Y(Ⅲ) at a concentration of 50 mmol / L and Th(Ⅳ) at a concentration of 10 mmol / L is prepared.
[0238] 75 g of the silicon-based adsorbent obtained in Example 5 was weighed and filled on a chromatography column with a diameter of 1 cm and a total length of 1.5 m. Clean water was passed to wash the adsorbent and compact it. Air was then passed to discharge the water in the column. The rare earth leaching solution prepared above was passed, and the fractions were collected. The concentrations of 16 kinds of rare earths were determined using ICP-OES. After column purification, the removal rate of thorium reached 98.56%.
[0239] Separation Example 5
[0240] 100 g of the silicon-based adsorbent obtained in Example 3 was weighed and filled on a chromatography column with a diameter of 1 cm and a total length of 2 m. Clean water was passed to wash the adsorbent and compact it. Air was then passed to discharge the water in the column. The rare earth leaching solution prepared in Separation Example 4 was passed, and the fractions were collected. The concentrations of 16 kinds of rare earths were determined using ICP-OES. After column purification, the removal rate of thorium reached 99.49%.
[0241] Thorium Removal from Rare Earth Industrial Wastewater
[0242] Separation Example 6
[0243] Preparation of simulated rare earth industrial wastewater: take single lanthanum sulfate, cerium sulfate, praseodymium sulfate, neodymium sulfate, samarium sulfate, europium sulfate, gadolinium sulfate, terbium sulfate, dysprosium sulfate, holmium sulfate, erbium sulfate, thulium sulfate, ytterbium sulfate, lutetium sulfate, yttrium sulfate and the thorium sulfate solution, calcium sulfate, iron sulfate, magnesium sulfate and aluminum sulfate solution prepared above, calculate the required volume of each solution, add distilled water and use sulfuric acid solution to adjust the pH, and finally make up to volume. In this way, rare earth industrial wastewater with a pH of 3 and containing La(Ⅲ), Ce(Ⅲ), Pr(Ⅲ), Nd(Ⅲ), Sm(Ⅲ), Eu(Ⅲ), Gd(Ⅲ), Tb(Ⅲ), Dy(Ⅲ), Ho(Ⅲ), Er(Ⅲ), Tm(Ⅲ), Yb(Ⅲ), Lu(Ⅲ), Y(Ⅲ), Ca(Ⅱ), Fe(Ⅲ), Mg(Ⅱ), Al(Ⅲ) at a concentration of 200 ppm and Th(Ⅳ) at a concentration of 200 ppm was prepared.
[0244] 100 g of the silicon-based adsorbent obtained in Example 6 was weighed and filled on a chromatography column with a diameter of 1 cm and a total length of 2 m. Clean water was passed to wash the adsorbent and compact it. Air was then passed to discharge the water in the column. The rare earth industrial wastewater prepared above was passed, and the fractions were collected. The concentrations of 19 ions were determined using ICP-OES, and the concentration of thorium ions was determined using ICP-MS. After column purification, the removal rate of thorium reached 99.7%.
[0245] Separation Example 7
[0246] Preparation of simulated rare earth industrial wastewater: single lanthanum sulfate, cerium sulfate, praseodymium sulfate, neodymium sulfate, samarium sulfate, europium sulfate, gadolinium sulfate, terbium sulfate, dysprosium sulfate, holmium sulfate, erbium sulfate, thulium sulfate, ytterbium sulfate, lutetium sulfate, yttrium sulfate and the thorium sulfate solution, calcium sulfate, iron sulfate, magnesium sulfate and aluminum sulfate solution prepared above. Calculate the required volume of each solution, add distilled water and use sulfuric acid solution to adjust the pH, and finally make up to volume. In this way, rare earth industrial wastewater with a pH of 3 and containing La(Ⅲ), Ce(Ⅲ), Pr(Ⅲ), Nd(Ⅲ), Sm(Ⅲ), Eu(Ⅲ), Gd(Ⅲ), Tb(Ⅲ), Dy(Ⅲ), Ho(Ⅲ), Er(Ⅲ), Tm(Ⅲ), Yb(Ⅲ), Lu(Ⅲ), Y(Ⅲ), Ca(Ⅱ), Fe(Ⅲ), Mg(Ⅱ), Al(Ⅲ) at a concentration of 10 mmol / L and Th(Ⅳ) at a concentration of 125 ppm was prepared.
[0247] 75 g of the silicon-based adsorbent obtained in Example 4 was weighed and filled on a chromatography column with a diameter of 1 cm and a total length of 1.5 m. Clean water was passed to wash the adsorbent and compact it. Air was then passed to discharge the water in the column. The rare earth industrial wastewater prepared above was passed, and the fractions were collected. The concentrations of 19 ions were determined using ICP-OES, and the concentration of thorium ions was determined using ICP-MS. After column purification, the removal rate of thorium reached 98.79%.
[0248] In summary, the silicon-based adsorption material of the present invention has the advantages of simple preparation method, strong selectivity for thorium, large adsorption capacity, adsorption capacity is less affected by pH value, good circulation performance and no saponification agent is used in the removal process, and is environmentally friendly. It can be widely used for extraction and separation of thorium, and can also be used for adsorption and removal of thorium, and has good application prospects.
[0249] The purpose, technical scheme and beneficial effects of the present invention have been described in detail above in conjunction with specific embodiments. It should be understood that the above is only a specific embodiment of the present invention and is not intended to limit the present invention. Various modifications, replacements or improvements can be made within the spirit and principles of the present invention, and these modifications, replacements and improvements should all be included in the protection scope of the present invention.
Claims
1. A silicon-based adsorption material comprising: (1) Silicon balls; (2) Compound of formula I coupled with silicon spheres: Wherein, R1 is selected from C1-C 10 Alkyl, C6-C 10 Aryl, C6-C 10 Aryl C1-C2 alkyl, C3-C 10 Cycloalkyl, C3-C 10 Cycloalkyl C1-C2 alkyl; R2 and R3 are each independently selected from hydrogen, C1-C4 alkyl, C3-C 10 Cycloalkyl, C3-C 10 Cycloalkyl C1-C2 alkyl, C6-C 10 Aryl, C6-C 10 Aryl C1-C2 alkyl; R4 is selected from C1-C 10 Alkyl, C3-C6 cycloalkyl, C3-C6 cycloalkylC1-C2 alkyl, C6-C 10 Aryl, C6-C 10 Aryl C1-C2 alkyl.
2. The silicon-based adsorption material according to claim 1, wherein R1 is selected from C1-C8 alkyl, phenyl, C1-C4 alkylphenyl, phenyl C1-C2 alkyl, in particular, R1 is selected from C2-C8 alkyl, phenyl, tolyl, xylyl, ethylphenyl, benzyl, phenethyl; and / or R2 and R3 are each independently selected from hydrogen, C1-C4 alkyl, in particular, R2 and R3 are each independently selected from hydrogen, methyl, ethyl, more in particular, in particular, R2 and R3 are each independently selected from hydrogen, methyl; and / or R4 is selected from C1-C8 alkyl, phenyl, C1-C4 alkylphenyl, phenyl C1-C2 alkyl, in particular, R4 is selected from C2-C8 alkyl, phenyl, tolyl, xylyl, ethylphenyl, benzyl, phenethyl; In particular, the compound of formula I is selected from the following compounds:
3. The silicon-based adsorption material according to claim 1 or 2, wherein In the silicon-based adsorption material, the compound of formula I is coupled to the surface of the silicon sphere via the nitrogen thereon; In particular, the silicon-based adsorption material comprises a structure of formula III: Wherein, R1 to R4 are as defined in claim 1, X represents a linking group, in particular a group derived from a silane coupling agent; and / or In the silicon-based adsorption material, the compound of formula I is coupled to the silicon sphere via a silane coupling agent; Preferably, the silane coupling agent has a functional group capable of directly reacting with the amine group in the structure of the compound of formula I. The silane coupling agent directly reacts with the compound of formula I to covalently connect one end of the silane coupling agent to the amine group in the structure of the compound of formula I through the reaction of the organic functional group of the silane coupling agent with the amine group in the structure of the compound of formula I.
4. The silicon-based adsorption material according to claim 3, wherein The silane coupling agent is shown in the following formula II: Wherein, R5, R6 and R7 are each independently selected from C1-C4 alkyl and C1-C4 alkoxy, and at least one is an alkoxy; preferably, each independently selected from C1-C2 alkyl and C1-C2 alkoxy, and at least one is an alkoxy; R8 is selected from halogen, epoxy, epoxymethoxy and isocyanate; n is an integer from 1 to 8; In particular, the silane coupling agent is selected from epoxy silane, halogen silane, isocyanate silane; In particular, the epoxysilane is selected from 3-(2,3-epoxypropyloxy)propyltrimethoxysilane, 5,6-epoxyhexyltriethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 3-(2,3-epoxypropyloxy)propyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-[(2,3)-epoxypropyloxy]propylmethyldimethoxysilane, 3-(2,3-epoxypropyloxy)propyltrimethoxysilane, (3-epoxypropyloxy)dimethylethoxysilane; The halogen silane is selected from 3-bromopropyltrimethoxysilane, 4-bromobutyltrimethoxysilane, 5-bromopentyltrimethoxysilane, 7-bromoheptyltrimethoxysilane, 3-chloroisopropyltrimethoxysilane, chloromethyltrimethoxysilane, chloromethyltriethoxysilane, 3-chloropropyltrimethoxysilane, 3-chloropropyltriethoxysilane, 3-iodopropyltrimethoxysilane, chloromethylmethyldiethoxysilane, 3-chloropropylmethyldiethoxysilane, 3-chloropropylmethyltrimethoxysilane, chloromethyldimethylethoxysilane, chloromethyldimethylmethoxysilane; The isocyanate silane is selected from 3-isocyanate propyl triethoxy silane, 3-isocyanate propyl trimethoxy silane, 3-isocyanate propyl methyl diethoxy silane, 3-isocyanate propyl methyl dimethoxy silane; In particular, X is selected from wherein R6, R7 and n are as defined in Formula II.
5. A method for preparing a silicon-based adsorption material, comprising: (1) coupling the compound of formula I with a silane coupling agent of formula II to obtain a coupling compound of formula IV; (2) allowing the coupling compound of formula IV to undergo a coupling reaction with silicon spheres to obtain a silicon-based adsorption material; Wherein, R1 to R4 are as defined in claim 1 or 2, R5 to R8 and n are as defined in claim 4, L is selected from direct bond, 6. The method of claim 5, wherein: In step (1), the molar ratio of the compound of formula I to the silane coupling agent of formula II is 1:0.5-1.5, for example 1:0.8-1.2; and / or Step (1) is carried out in an organic solvent, in particular, the organic solvent is selected from any one or more of methanol, ethanol, acetonitrile, tetrahydrofuran, and dioxane; and / or The reaction temperature of step (1) is 50-100°C, for example 65-80°C; and / or The reaction time of step (1) is 2 hours or more, 5 hours or more, 10 hours or more, 12 hours or more, for example 12-72 hours or 24-40 hours; and / or In step (2), the mass ratio of the coupling compound of formula IV to the silicon sphere is 1:0.5-5, for example 1:0.8-4; and / or Step (2) is carried out in an organic solvent, in particular, the organic solvent is selected from any one or more of toluene, xylene, trimethylolbenzene, cyclohexane, n-heptane, isooctane; and / or The reaction temperature of step (2) is 60-150°C, for example 80-120°C; and / or The reaction time of step (2) is more than 2 hours, more than 5 hours, more than 10 hours, more than 12 hours, for example, 12-96 hours, 48-72 hours.
7. The coupling compound of formula IV: in, R1 to R8, n are as defined in claim 5, L is selected from direct bond, 8. Use of the silicon-based adsorption material according to any one of claims 1 to 4 or the silicon-based adsorption material prepared according to any one of claims 5 to 6 in preparing an extractant for extracting thorium.
9. A method for extracting thorium, comprising the step of contacting a thorium-containing feed liquid with the silicon-based adsorption material according to any one of claims 1 to 4 or the silicon-based adsorption material prepared according to any one of claims 5 to 6 to extract thorium from the feed liquid.
10. The method of claim 9, wherein: The thorium-containing liquid is selected from high-purity rare earth liquid, rare earth leaching liquid, rare earth industrial wastewater liquid; and / or The pH of the thorium-containing liquid is 0 to 4, preferably 1-4; and / or The thorium-containing liquid is a nitric acid, sulfuric acid or hydrochloric acid solution.
Citation Information
Patent Citations
Method for extracting high-purity uranium, thorium and mixed rare earths from excellent molten slag
CN104775026A
Method for adsorbing thorium by utilizing fiber-bridged beta-cyclodextrin derivative
CN105664873A
A method for removing radioactivity from lanthanum chloride solution
CN106148696B
Material capable of enriching and separating thorium and preparation method thereof
CN111841512A
Novel class of calixarene crown ether bond-type silicon-based adsorption materials and preparation method thereof
CN103055816A