Polyacrylate spherical material, drop ball forming method and application thereof, and fixed bed CO2 adsorbent

Polyacrylate spherical materials were prepared by drop ball forming method, which solved the particle size distribution and yield problems of emulsion suspension polymerization and precipitation polymerization, and achieved efficient and uniform preparation of polyacrylate spherical materials, suitable for CO2 adsorbents , improves mechanical strength and industrial production potential.

CN119075932AActive Publication Date: 2024-12-06PETROCHINA CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202310658162.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-06-05
Publication Date
2024-12-06
Estimated Expiration
2043-06-05

AI Technical Summary

Technical Problem

In the prior art, the particle size distribution range of polyacrylate spherical materials is prepared by emulsion suspension polymerization method, with a narrow yield and low production efficiency, and the precipitation polymerization method is low, making it not suitable for large-scale industrial production.

Method used

By using the drip ball forming method, a uniform organic phase is formed by mixing the organic monomer, an emulsifier, an initiator and a co-emulsifier, and then mixed with a silica sol solution and deionized water to form an aqueous phase, and after sufficient emulsification, the reducing agent is added. A spherical shape is formed under surface tension in water using a drop ball forming device to achieve polymerization and initial curing, and then aged and dried under mild conditions to produce a spherical polyacrylate material.

Benefits of technology

It has achieved a spherical polyacrylate material with high yield, uniform particle size and high mechanical strength. It is suitable for fixed bed CO2 adsorbents, reducing production costs, simplifying processes, and improving industrial application potential.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119075932A_ABST
    Figure CN119075932A_ABST
Patent Text Reader

Abstract

The invention provides a polyacrylate spherical material, a drop ball forming method and application thereof, and a fixed bed CO2 adsorbent, the drop ball forming method comprises the following steps: firstly adding two or three organic monomers into an organic dispersion phase, and then sequentially adding an emulsifier, an initiator and a co-emulsifier to form a uniform organic phase; mixing the silica sol solution and deionized water to form a water phase; dropwise adding the water phase into the organic phase, fully emulsifying, and adding a reducing agent to obtain a formed emulsion; and carrying out drop ball forming and aging on the formed emulsion by using a drop ball forming device, and drying the aged small balls to obtain a finished product. The drop ball forming method realizes one-step ball forming, and is simple in operation process, green, environment-friendly, easy to industrialize and high in yield, the yield can be improved by more than 30% compared with that of an emulsion suspension polymerization method, and the production cost is reduced; the prepared polyacrylate spherical material has the characteristics of high bulk density, large particle size, high mechanical strength and the like, and is suitable for being used as a solid adsorbent carrier for fixed bed CO2 adsorption.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a polyacrylate spherical material and a drop ball forming method and application thereof, a fixed bed CO 2 Adsorbent, CO 2 The field of adsorption capture technology. Background Art

[0002] Greenhouse effect and climate warming are hot issues in the world today. 2 It is the anthropogenic gas that contributes most to the greenhouse effect. 2 Capture is the main way to significantly reduce greenhouse gas emissions.

[0003] About CO 2 For capture, the more mature technology at this stage is chemical absorption, which has the advantages of fast absorption, mature process, and large processing capacity, but it has many defects such as high regeneration energy consumption, limited space for further energy saving and consumption reduction, complex process, and easy corrosion of equipment. In comparison, chemical adsorption has many advantages such as low energy consumption, simple process, and no equipment corrosion. Solid adsorbents include calcium-based adsorbents, metal organic framework materials (MOFs), zeolites, hyper-cross-linked polymers, carbon materials, alkali metal carbonates, amine-functionalized adsorbents, etc. Among them, the polymer material prepared by the emulsion template method has a higher porosity and a certain mechanical strength. The internal pores are a three-dimensional interconnected pore structure with a pore size of 0.1-300μm. The pore size can be adjusted to be appropriate and the pore size distribution is uniform. The above characteristics make the emulsion template polymer have outstanding advantages as a solid adsorbent carrier.

[0004] CN106589201A discloses a hydrophilic modification method for polystyrene materials and its products, which can reduce the specific adsorption of biomacromolecules by chloromethylating the surface of polystyrene microspheres and bonding PVA to the surface of polystyrene microspheres. PVA contains a large number of hydroxyl groups, which is convenient for coupling specific ligands to meet different separation mode requirements. However, the hydrophilic modification process is complicated, the steps are cumbersome, and it is difficult to control.

[0005] CN111825796A discloses a method for using CO 2 The invention relates to a polyacrylate composite material for CO adsorption and a preparation method thereof. In the preparation process, a polymer emulsion is added to a dispersed phase, dispersed into balls at a certain speed, a reducing agent is added after stabilization, and the balls are separated and dried after solidification to obtain spherical porous polyacrylate balls, which are then subjected to amination grafting and epoxy resin surface end-capping treatment to obtain a spherical porous polyacrylate ball for CO adsorption. 2 Adsorbed polyacrylate composites.

[0006] CN114213581A discloses a method for preparing hydrophilic polyacrylate crosslinked microspheres, in which the hydrophilic substance is connected to the comonomer by chemical bonding, and then copolymerized with the crosslinking agent in an aqueous phase containing a stabilizer to form polymer microspheres.

[0007] The above methods all adopt emulsion suspension polymerization to prepare polyacrylate beads. Although emulsion suspension polymerization has been widely used in industry, the particle size of the microspheres obtained mainly depends on the stirring speed during polymerization. Therefore, the particle size distribution range is wide and can only be regulated within a narrow range, and there is a problem of low yield. In addition, polyacrylate beads can also be prepared by precipitation polymerization in the prior art, but the production efficiency of precipitation polymerization is very low and does not have the prospect of industrial large-scale production.

[0008] Therefore, a novel polyacrylate spherical material (polyacrylate cross-linked porous spherical granular material) and its drop ball forming method and application, fixed bed CO 2 Adsorbents have become a technical problem that needs to be solved urgently in this field. Summary of the invention

[0009] In order to solve the above-mentioned shortcomings and deficiencies, an object of the present invention is to provide a drop ball forming method of polyacrylate spherical material.

[0010] Another object of the present invention is to provide a polyacrylate spherical material, which is prepared by the above-mentioned polyacrylate spherical material drop ball forming method.

[0011] Another object of the present invention is to provide the above-mentioned polyacrylate spherical material as a fixed bed CO 2 Application of solid adsorbent carriers used for adsorption.

[0012] Another object of the present invention is to provide a fixed bed CO 2 Adsorbent, wherein the adsorption carrier is the polyacrylate spherical material mentioned above.

[0013] In order to achieve the above objectives, on the one hand, the present invention provides a drop ball forming method of a polyacrylate spherical material, wherein the drop ball forming method of the polyacrylate spherical material comprises:

[0014] Step 1: First, two or three organic monomers are added to the organic dispersed phase, and then an emulsifier, an initiator and an emulsifier are added in sequence to form a uniform organic phase;

[0015] Step 2: Mixing the silica sol solution and deionized water to form an aqueous phase;

[0016] Step 3: dropping the aqueous phase into the organic phase for full emulsification and then adding a reducing agent to obtain a formed emulsion;

[0017] Step 4: using a drop ball forming device to perform drop ball forming and aging on the formed latex, and then drying the aged small balls to obtain the polyacrylate spherical material.

[0018] As a specific embodiment of the drop ball forming method described above in the present invention, the organic monomer includes two or three organic monomers selected from the group consisting of glycidyl methacrylate, tert-butyl methacrylate, trimethylolpropane triacrylate, tert-butyl acrylate, methyl methacrylate, ethyl methacrylate, methyl acrylate, ethyl acrylate, styrene, and ethylene glycol dimethacrylate.

[0019] As a specific embodiment of the drop ball forming method described above, the organic monomers include glycidyl methacrylate, tert-butyl methacrylate and trimethylolpropane triacrylate in a mass ratio of 2-3.5:0.5-1.5:1.5-3.

[0020] In the present invention, the amount of the organic dispersed phase affects the yield, dispersion and mechanical strength of the polyacrylate spherical material finally obtained. As for the volume fraction of the organic dispersed phase, it is sufficient to ensure that each organic monomer is fully dissolved and dispersed. As a specific embodiment of the drop ball forming method described above of the present invention, the volume fraction of the organic dispersed phase is 30-50% based on the total volume of the organic phase as 100%.

[0021] As a specific embodiment of the drop ball forming method described above in the present invention, the organic dispersed phase includes one or a combination of cyclohexane, toluene, carbon tetrachloride, dichloromethane, 1-2-dichloroethane, ethyl acetate, etc.; preferably, one or a combination of toluene, cyclohexane, and ethyl acetate.

[0022] As a specific embodiment of the drop ball forming method described above, based on the total weight of the two or three organic monomers as 100%, the amounts of the emulsifier, initiator and co-emulsifier are 3-15%, 1-5% and 1-3% respectively.

[0023] As a specific embodiment of the drop ball forming method described above in the present invention, the emulsifier includes one or a combination of span80 (Span 80), span60 (Span 60), span20 (Span 20), polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer (P123), etc.

[0024] As a specific embodiment of the drop ball forming method described above in the present invention, the initiator includes one or a combination of ammonium persulfate, potassium persulfate, benzoyl peroxide, diisopropylbenzene peroxide, tert-butyl peroxide, azobisisobutyronitrile, azobisisovaleronitrile, etc.

[0025] As a specific embodiment of the drop ball forming method described above, the co-emulsifier includes one or a combination of hexadecanol, hexanol, octanol, p-nonylphenol, etc.

[0026] As a specific embodiment of the drop ball forming method described above, in step 1, a uniform organic phase can be formed by ultrasound, and the present invention does not make specific requirements on the ultrasound time, etc., which can be reasonably adjusted according to the actual operation conditions on site. For example, in some embodiments of the present invention, the ultrasound time can be 5-10 minutes.

[0027] As a specific embodiment of the drop ball forming method described above, the mass ratio of the silica sol solution to deionized water is 1:1-1:4, and the mass concentration of the silica sol solution is 25-35%, preferably 30%.

[0028] As a specific embodiment of the drop ball forming method described above, the aqueous phase is dropped into the organic phase for full emulsification according to the aqueous phase accounting for 55-62% of the total volume of the emulsion obtained after full emulsification.

[0029] As a specific embodiment of the drop ball forming method described above, in step 3, the step of dropping the aqueous phase into the organic phase for sufficient emulsification and then adding the reducing agent specifically comprises:

[0030] Under the condition of stirring at a speed of 1000-3000r / min in a high-speed stirrer, the aqueous phase is dropped into the organic phase. After the dropping is completed, the speed is increased to 5000-10000r / min and stirred for 5-10min to fully emulsify. Then, the reducing agent is added to the fully emulsified emulsion and stirring is continued for 1-2min.

[0031] As a specific embodiment of the drop ball forming method described above, the amount of the reducing agent is 5-15%, based on the total weight of the two or three organic monomers being 100%.

[0032] As a specific embodiment of the drop ball forming method described above in the present invention, the reducing agent includes one or a combination of N,N-dimethylaniline, N,N,N,N-tetramethylethylenediamine, ferrous sulfate, sodium sulfite, etc.

[0033] As a specific embodiment of the drop ball molding method described above in the present invention, in order to delay the occurrence of the polymerization reaction before molding, the process of preparing the molding emulsion must be carried out under low temperature conditions, that is, step three is carried out in a low temperature environment so that the temperature of the molding emulsion drops below 5°C; preferably, steps one to three are all carried out in a low temperature environment.

[0034] As a specific embodiment of the drop ball forming method described above in the present invention, the drop ball forming device includes a forming emulsion storage tank, a peristaltic pump and a forming column, the forming column is a jacketed glass tube with upper and lower ends opening, a drip tray is arranged on the upper end opening of the jacketed glass tube, a plurality of drop ball forming needles are arranged on the drip tray facing the upper end opening, the lower end opening of the jacketed glass tube is connected to the forming tank; the outlet of the forming emulsion storage tank is connected to the inlet of the drip tray through a pipeline via a peristaltic pump.

[0035] As a specific embodiment of the drop ball forming method described above, a valve is provided between the lower end opening of the jacketed glass tube and the inlet of the forming tank.

[0036] As a specific embodiment of the drop ball forming method described above, the forming emulsion storage tank, peristaltic pump, jacketed glass tube, drip tray, drop ball forming needle and forming tank are all conventional equipment and can be obtained by commercial purchase or self-production. For example, in some embodiments of the present invention, the forming tank can be a conical flask.

[0037] As a specific embodiment of the drop ball forming method described above, in step 4, the drop ball forming and aging of the forming emulsion using a drop ball forming device comprises:

[0038] Adding an aqueous solution of a dispersant, preferably an aqueous solution of a dispersant, into the jacketed glass tube so that both the jacketed glass tube and the molding tank are filled with the aqueous solution of the dispersant, and heating to 55-70° C. by connecting a water bath device through the jacket;

[0039] The molding emulsion is transported to the drip tray by a peristaltic pump and dripped into the jacketed glass tube through a ball-dropping molding needle. The molding emulsion forms a sphere under the action of surface tension in water and undergoes polymerization reaction and preliminary solidification to quickly form small balls. The small balls after preliminary solidification fall into a molding tank and are aged at 55-65°C, that is, sufficient polymerization reaction is carried out in the molding tank to ensure that the small balls are completely formed to obtain aged small balls.

[0040] In some embodiments of the present invention, in step 4, the forming emulsion is subjected to drop ball forming and aging using a drop ball forming device, specifically comprising:

[0041] Open the valve provided between the lower end opening of the jacketed glass tube and the inlet of the forming tank, add an aqueous solution of a dispersant, preferably an aqueous solution of a dispersant, into the jacketed glass tube, so that both the jacketed glass tube and the forming tank are filled with the aqueous solution of the dispersant, and heat to 55-70° C. by connecting a water bath device through the jacket;

[0042] The molding emulsion is transported to the drip tray by a peristaltic pump and dripped into the jacketed glass tube by a ball-dropping molding needle. The molding emulsion forms a sphere under the surface tension of water and undergoes polymerization reaction and preliminary solidification to quickly form small balls. The small balls after preliminary solidification fall into the molding tank and are aged at 55-65°C, that is, sufficient polymerization reaction is carried out in the molding tank to ensure that the small balls are completely formed, and the aged small balls are obtained;

[0043] After the aging is completed, the valve provided between the lower end opening of the jacketed glass tube and the inlet of the molding tank is closed, the molding tank is removed, and the aged balls are taken out therefrom, and then the balls are dried.

[0044] In the drop ball forming method described above, the forming emulsion can be formed into a sphere by surface tension in pure water or an aqueous solution of a dispersant, but the use of a dispersant can further prevent the formed small spheres from sticking to each other. If a dispersant is not used, monodisperse spheres cannot be obtained.

[0045] As a specific embodiment of the drop ball forming method described above, the mass concentration of the aqueous solution of the dispersant is 0.13-0.3%, preferably 0.13-0.23%.

[0046] As a specific embodiment of the drop ball forming method described above, the dispersant includes organic dispersants such as polyvinyl alcohol (PVA) and / or polyethylene glycol, preferably polyvinyl alcohol (PVA).

[0047] As a specific embodiment of the drop ball forming method described above, the height of the jacketed glass tube is 1-2 m.

[0048] As a specific embodiment of the drop ball forming method described above, the inner diameter of the drop ball forming needle is 0.3-1 mm.

[0049] As a specific embodiment of the above-mentioned drop ball forming method of the present invention, the dripping rate is 1-3 drops / second.

[0050] In the above drop ball forming method of the present invention, the temperature in the forming tank needs to be controlled at 55-65°C to age the preliminarily solidified balls at this temperature. The aging time can be reasonably adjusted according to the actual needs of the on-site operation. In some embodiments of the present invention, the aging time can be, for example, 15-20 minutes.

[0051] As a specific embodiment of the drop ball forming method described above, the drying is performed at 40-80° C. for 4-8 hours. Drying is a conventional operation and can be performed in an oven.

[0052] On the other hand, the present invention further provides a polyacrylate spherical material, wherein the polyacrylate spherical material is prepared by the above-mentioned polyacrylate spherical material drop ball forming method.

[0053] As a specific embodiment of the above-mentioned polyacrylate spherical material of the present invention, the particle size of the polyacrylate spherical material is 0.85-2 mm, and the bulk density is >0.2 g / mL.

[0054] In another aspect, the present invention also provides the above-mentioned polyacrylate spherical material as a fixed bed CO 2 Application of solid adsorbent carriers used for adsorption.

[0055] In another aspect, the present invention also provides a fixed bed CO 2 The solid adsorbent comprises a solid adsorption carrier and an adsorption active component loaded on the surface of the solid adsorption carrier, wherein the solid adsorption carrier is the above-mentioned polyacrylate spherical material.

[0056] The present invention is to fix the bed CO 2 There is no specific requirement for the adsorption active component and the amount thereof used in the solid adsorbent, and they can be reasonably adjusted according to the actual operation needs on site. For example, in some embodiments of the present invention, the adsorption active component can be an organic amine such as pentaethylenehexamine.

[0057] Compared with the prior art, the beneficial technical effects that can be achieved by the present invention include:

[0058] The drop ball forming method of the polyacrylate spherical material provided by the present invention first adds two or three organic monomers into an organic dispersed phase, then sequentially adds an emulsifier, an initiator and an emulsifier co-emulsifier to form a uniform organic phase, then mixes a silica sol solution and deionized water to form an aqueous phase, then drops the aqueous phase into the organic phase for full emulsification, and then adds a reducing agent to obtain an oil-in-water forming emulsion with a density greater than that of water, and finally forms the forming emulsion by a top-down drop ball forming method, and obtains the polyacrylate spherical material by utilizing the surface tension of the forming emulsion in water and the polymerization reaction occurring in the forming emulsion itself.

[0059] Compared with the traditional precipitation polymerization and suspension polymerization methods, the drop ball forming method of the polyacrylate spherical material provided by the present invention has the following advantages:

[0060] (1) One-step ball forming, no need for secondary molding, simple operation process, green and environmentally friendly, easy to industrialize, high yield. Its yield can be increased by more than 30% compared with the emulsion suspension polymerization method, reducing production costs;

[0061] (2) The operating conditions are mild, and polymerization can be achieved at a relatively low temperature without the need for high-temperature calcination;

[0062] (3) The prepared polyacrylate spherical material has the characteristics of high bulk ratio and large particle size, with a particle size of 0.85-2 mm and a bulk density of >0.2 g / mL, which is suitable for use as a fixed bed CO 2 Solid adsorbent carrier used for adsorption;

[0063] (4) The polyacrylate spherical material has high sphericity, easy to control particle size and uniform particle size distribution;

[0064] (5) Due to the addition of hydrophilic silica sol, the obtained polyacrylate spherical material has higher mechanical strength. Compared with the currently used emulsion suspension polymerization method, the mechanical strength of the polyacrylate spherical material can be increased by more than 15%, and it is not easy to wear during fixed bed operation. BRIEF DESCRIPTION OF THE DRAWINGS

[0065] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0066] Figure 1 Schematic diagram of the structure of the drop ball forming device used in the embodiment of the present invention.

[0067] Figure 2 This is a physical picture of the polyacrylate spherical material provided in Example 2 of the present invention.

[0068] Figure 3 This is a physical picture of the polyacrylate spherical material provided in Example 5 of the present invention.

[0069] Figure 4 This is a physical picture of the polyacrylate spherical material provided for Comparative Example 2 of the present invention.

[0070] Figure 5 This is a physical picture of the polyacrylate spherical material provided for Comparative Example 5 of the present invention.

[0071] Figure 6 This is a physical picture of the polyacrylate spherical material provided in Comparative Example 7 of the present invention.

[0072] Figure 7 This is a scanning electron microscope image (500 μm) of the polyacrylate spherical material provided in Example 1 of the present invention.

[0073] Figure 8 This is a scanning electron microscope image (3.00 μm) of the polyacrylate spherical material provided in Example 1 of the present invention.

[0074] Description of main figures:

[0075] 1. Molding emulsion storage tank;

[0076] 2. Peristaltic pump;

[0077] 3. Drip tray;

[0078] 31. Drop ball forming needle

[0079] 4. Molding column;

[0080] 5. Molding tank;

[0081] 6. Aqueous solution of dispersant. DETAILED DESCRIPTION

[0082] It should be noted that the term "comprises" and any variations thereof in the specification and claims of the present invention and the above-mentioned drawings are intended to cover non-exclusive inclusions. For example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.

[0083] "Scope" disclosed in the present invention is given in the form of lower limit and upper limit. It can be one or more lower limits, and one or more upper limits respectively. A given range is defined by selecting a lower limit and an upper limit. The selected lower limit and upper limit define the boundaries of a particular range. All ranges defined in this way are combinable, i.e. any lower limit can be combined with any upper limit to form a range. For example, for a specific parameter, a range of 60-120 and 80-110 is listed, and it is understood that a range of 60-110 and 80-120 is also expected. In addition, if the minimum range values ​​listed are 1 and 2, and the maximum range values ​​listed are 3, 4 and 5, then the following ranges can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5.

[0084] In the present invention, unless otherwise specified, the numerical range "ab" represents an abbreviation of any real number combination between a and b, where a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" have been listed in the present invention, and "0-5" is just an abbreviation of these numerical combinations.

[0085] In the present invention, unless otherwise specified, all embodiments and preferred embodiments mentioned in the present invention can be combined with each other to form a new technical solution.

[0086] In the present invention, unless otherwise specified, all technical features and preferred features mentioned in the present invention can be combined with each other to form a new technical solution.

[0087] In the present invention, if not specifically stated, the term "two" used in this specification means "at least two".

[0088] In the present invention, unless otherwise specified, all steps mentioned herein may be performed sequentially or randomly, but are preferably performed sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0089] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with the attached table, drawings and examples. The following described embodiments are some embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention, and should not be regarded as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present invention. If the specific conditions are not specified in the embodiments, they are carried out according to the normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified in the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0090] Example 1

[0091] This embodiment provides a polyacrylate spherical material, which is prepared by a drop ball forming method comprising the following specific steps:

[0092] Step 1: Weigh 2.1g of glycidyl methacrylate, 0.8g of tert-butyl methacrylate and 2.1g of trimethylolpropane triacrylate and add them into toluene accounting for 30% of the total volume of the organic phase, then add 0.3g of P123, 0.2g of benzoyl peroxide (BPO) and 0.1g of hexadecanol in sequence, and then ultrasonicate in an ultrasonic cleaner for 5min to dissolve and mix them evenly, as the oil phase, i.e., the uniform organic phase;

[0093] Step 2: Weigh 7 g of 35% silica sol solution and stir with 13 g of deionized water to form the aqueous phase;

[0094] Step 3: Place the dissolved oil phase in an ice bath, and slowly drop the uniformly stirred water phase into the oil phase at a high-speed stirrer speed of 3000 r / min, so that the water phase accounts for 56% of the total volume of the emulsion obtained after full emulsification. After the drop is completed, increase the speed to 7000 r / min and stir for 5 minutes to fully emulsify, then add 0.3 g of reducing agent N, N-dimethylaniline and continue stirring for 1 minute to obtain a stable water-in-oil emulsion, i.e., a formed emulsion;

[0095] Step 4: Using a drop ball forming device to perform drop ball forming and aging on the formed emulsion, wherein the structure diagram of the drop ball forming device is as follows: Figure 1 As shown, from Figure 1 As can be seen from the figure, it includes a molding emulsion storage tank 1, a peristaltic pump 2 and a molding column 4 with a height of 1.2m, wherein the molding column 4 is a jacketed glass tube with openings at both ends, a drip tray 3 is arranged on the upper opening of the jacketed glass tube, and a plurality of drop ball molding needles 31 are arranged on the drip tray 3 toward the upper opening, and the lower opening of the jacketed glass tube is connected to the molding tank 5; the outlet of the molding emulsion storage tank 1 is connected to the inlet of the drip tray 3 through a pipeline via the peristaltic pump 2;

[0096] Droplet forming and aging specifically include:

[0097] Prepare an aqueous solution 6 of a dispersant, which in this embodiment is an aqueous solution of polyvinyl alcohol with a mass concentration of 0.13%, and pour it into a molding column, and then connect a water bath device such as a water bath circulation heater to 60° C. through a jacket, and heat the molding tank, such as a conical flask, at a temperature of 55° C. using a magnetic stirring heater to ensure that the pellets are fully formed;

[0098] The molding emulsion is transported to a drip tray by a peristaltic pump at a pump speed of 5.5 r / min, and the molding emulsion is dripped into a polyvinyl alcohol aqueous solution contained in a jacketed glass tube at a dripping speed of 1 drop / second through a drop ball molding needle with an inner diameter of 0.3 mm. The molding emulsion forms a spherical shape under the action of surface tension in water and undergoes polymerization reaction and preliminary solidification. The preliminary solidified small balls fall into a molding tank and are aged at 55° C. for 15 minutes to obtain aged small balls.

[0099] The small balls were taken out and placed in an oven at 50° C. to dry for 6 hours, thereby preparing macroporous polymer balls, namely the polyacrylate spherical material.

[0100] Example 2

[0101] This embodiment provides a polyacrylate spherical material, which is prepared by a drop ball forming method comprising the following specific steps:

[0102] Step 1: Weigh 2.2g of glycidyl methacrylate, 1.0g of tert-butyl methacrylate and 1.6g of trimethylolpropane triacrylate and add them into toluene accounting for 35% of the total volume of the organic phase, then add 0.4g of span80, 0.1g of ammonium persulfate and 0.12g of hexanol in sequence, and then ultrasonicate in an ultrasonic cleaner for 7min to dissolve and mix them evenly, as the oil phase, i.e., the uniform organic phase;

[0103] Step 2: Weigh 7 g of 32% silica sol solution and stir with 13 g of deionized water to form the aqueous phase;

[0104] Step 3: Place the dissolved oil phase in an ice bath, and slowly drop the uniformly stirred water phase into the oil phase at a high-speed stirrer speed of 2000 r / min, so that the water phase accounts for 57% of the total volume of the emulsion obtained after full emulsification. After the drop is completed, increase the speed to 8000 r / min and stir for another 6 minutes to fully emulsify, then add 0.4 g of reducing agent N,N,N,N-tetramethylethylenediamine and continue stirring for 1 minute to obtain a stable water-in-oil emulsion, i.e., a formed emulsion;

[0105] Step 4: Using a drop ball forming device to perform drop ball forming and aging on the formed emulsion, wherein the structure diagram of the drop ball forming device is as follows: Figure 1 As shown, from Figure 1 As can be seen from the figure, it includes a molding emulsion storage tank 1, a peristaltic pump 2 and a molding column 4 with a height of 1.2m, wherein the molding column 4 is a jacketed glass tube with openings at both ends, a drip tray 3 is arranged on the upper opening of the jacketed glass tube, and a plurality of drop ball molding needles 31 are arranged on the drip tray 3 toward the upper opening, and the lower opening of the jacketed glass tube is connected to the molding tank 5; the outlet of the molding emulsion storage tank 1 is connected to the inlet of the drip tray 3 through a pipeline via the peristaltic pump 2;

[0106] Droplet forming and aging specifically include:

[0107] Prepare an aqueous solution of a dispersant 6, which in this embodiment is an aqueous solution of polyethylene glycol with a mass concentration of 0.15%, and pour it into the molding column, and then connect it to a water bath through a jacket, such as a water bath circulation heater, and heat it to 70° C. The molding tank, such as a conical flask, is heated at a temperature of 58° C. using a magnetic stirring heater to ensure that the pellets are fully formed;

[0108] The molding emulsion is transported to a drip tray by a peristaltic pump at a pump speed of 4.5 r / min, and the molding emulsion is dripped into the aqueous solution of polyethylene glycol contained in the jacketed glass tube at a dripping speed of 1 drop / second through a drop ball molding needle with an inner diameter of 0.3 mm. The molding emulsion forms a spherical shape under the action of surface tension in water and undergoes polymerization reaction and preliminary solidification. The preliminary solidified small balls fall into a molding tank and are aged at 58° C. for 15 minutes to obtain aged small balls.

[0109] The small balls were taken out and placed in an oven at 65° C. to dry for 6 hours, thereby preparing macroporous polymer balls, namely the polyacrylate spherical material.

[0110] Example 3

[0111] This embodiment provides a polyacrylate spherical material, which is prepared by a drop ball forming method comprising the following specific steps:

[0112] Step 1: Weigh 2.3g of glycidyl methacrylate, 1.2g of tert-butyl methacrylate and 2.5g of trimethylolpropane triacrylate and add them into toluene accounting for 40% of the total volume of the organic phase, then add 0.2g of span60, 0.24g of diisopropylbenzene peroxide and 0.18g of octanol in sequence, and then ultrasonicate in an ultrasonic cleaner for 8min to dissolve and mix them evenly, as the oil phase, i.e., the uniform organic phase;

[0113] Step 2: Weigh 8 g of a silica sol solution with a mass concentration of 28% and stir it with 12 g of deionized water to form the aqueous phase;

[0114] Step 3: Place the dissolved oil phase in an ice bath, and slowly drop the uniformly stirred water phase into the oil phase at a high-speed stirrer speed of 3000 r / min, so that the water phase accounts for 59% of the total volume of the emulsion obtained after full emulsification. After the drop is completed, increase the speed to 9000 r / min and stir for another 7 minutes to fully emulsify, then add 0.6 g of reducing agent ferrous sulfate and continue stirring for 1 minute to obtain a stable water-in-oil emulsion, i.e., a formed emulsion;

[0115] Step 4: Using a drop ball forming device to perform drop ball forming and aging on the formed emulsion, wherein the structure diagram of the drop ball forming device is as follows: Figure 1 As shown, from Figure 1As can be seen from the figure, it includes a molding emulsion storage tank 1, a peristaltic pump 2 and a molding column 4 with a height of 1.2m, wherein the molding column 4 is a jacketed glass tube with openings at both ends, a drip tray 3 is arranged on the upper opening of the jacketed glass tube, and a plurality of drop ball molding needles 31 are arranged on the drip tray 3 toward the upper opening, and the lower opening of the jacketed glass tube is connected to the molding tank 5; the outlet of the molding emulsion storage tank 1 is connected to the inlet of the drip tray 3 through a pipeline via the peristaltic pump 2;

[0116] Droplet forming and aging specifically include:

[0117] Prepare an aqueous solution of a dispersant 6, which in this embodiment is an aqueous solution of polyvinyl alcohol with a mass concentration of 0.18%, and pour it into the molding column, and then connect it to a water bath through a jacket, such as a water bath circulation heater, and heat it to 55° C. The molding tank, such as a conical flask, is heated at a temperature of 60° C. using a magnetic stirring heater to ensure that the pellets are fully formed;

[0118] The molding emulsion is transported to a drip tray by a peristaltic pump at a pump speed of 7.5 r / min, and the molding emulsion is dripped into a polyvinyl alcohol aqueous solution contained in a jacketed glass tube at a dripping speed of 2 drops / second through a drop ball molding needle with an inner diameter of 0.8 mm. The molding emulsion forms a spherical shape under the action of surface tension in water and undergoes polymerization reaction and preliminary solidification. The preliminary solidified small balls fall into a molding tank and are aged at 60° C. for 15 minutes to obtain aged small balls.

[0119] The small balls were taken out and placed in an oven at 70° C. to dry for 6 hours, thereby preparing macroporous polymer balls, namely the polyacrylate spherical material.

[0120] Example 4

[0121] This embodiment provides a polyacrylate spherical material, which is prepared by a drop ball forming method comprising the following specific steps:

[0122] Step 1: Weigh 2.6g of glycidyl methacrylate, 1.3g of tert-butyl methacrylate and 2.8g of trimethylolpropane triacrylate and add them to a mixture of cyclohexane and ethyl acetate accounting for 45% of the total volume of the organic phase, then add 0.3g of span20, 0.2g of BPO and 0.08g of p-nonylphenol in sequence, and then ultrasonicate in an ultrasonic cleaner for 9 minutes to dissolve and mix them evenly, as the oil phase, that is, the uniform organic phase;

[0123] Step 2: Weigh 7 g of 30% silica sol solution and mix with 20 g of deionized water to form the aqueous phase;

[0124] Step 3: Place the dissolved oil phase in an ice bath, and slowly drop the uniformly stirred water phase into the oil phase at a high-speed stirrer speed of 3000 r / min, so that the water phase accounts for 61% of the total volume of the emulsion obtained after full emulsification. After the drop is completed, increase the speed to 10000 r / min and stir for 8 minutes to fully emulsify, then add 0.5 g of reducing agent N, N-dimethylaniline and continue stirring for 1 minute to obtain a stable water-in-oil emulsion, i.e., a formed emulsion;

[0125] Step 4: Using a drop ball forming device to perform drop ball forming and aging on the formed emulsion, wherein the structure diagram of the drop ball forming device is as follows: Figure 1 As shown, from Figure 1 As can be seen from the figure, it includes a molding emulsion storage tank 1, a peristaltic pump 2 and a molding column 4 with a height of 1.8m, wherein the molding column 4 is a jacketed glass tube with openings at both ends, a drip tray 3 is provided on the upper opening of the jacketed glass tube, and a plurality of drop ball molding needles 31 are provided on the drip tray 3 facing the upper opening, and the lower opening of the jacketed glass tube is connected to the molding tank 5; the outlet of the molding emulsion storage tank 1 is connected to the inlet of the drip tray 3 through a pipeline via the peristaltic pump 2;

[0126] Droplet forming and aging specifically include:

[0127] Prepare an aqueous solution 6 of a dispersant, which in this embodiment is a mixed aqueous solution of polyvinyl alcohol and polyethylene glycol with a mass concentration of 0.2%, and pour it into a molding column, and then connect a water bath device such as a water bath circulation heater to 65° C. through a jacket, and heat the molding tank, such as a conical flask, at a temperature of 62° C. using a magnetic stirring heater to ensure that the pellets are fully formed;

[0128] The molding emulsion is transported to a drip tray by a peristaltic pump at a pump speed of 5.5 r / min, and the molding emulsion is dripped into a mixed aqueous solution of polyvinyl alcohol and polyethylene glycol contained in a jacketed glass tube by a drop ball molding needle with an inner diameter of 0.3 mm at a drip speed of 2 drops / second. The molding emulsion forms a spherical shape under the action of surface tension in water and undergoes polymerization reaction and preliminary solidification. The preliminary solidified small balls fall into a molding tank and are aged at 62° C. for 15 minutes to obtain aged small balls.

[0129] The small balls were taken out and placed in an oven at 75° C. to dry for 6 hours, thereby preparing macroporous polymer balls, namely the polyacrylate spherical material.

[0130] Example 5

[0131] This embodiment provides a polyacrylate spherical material, which is prepared by a drop ball forming method comprising the following specific steps:

[0132] Step 1: Weigh 3.0g of glycidyl methacrylate, 1.5g of tert-butyl methacrylate and 2.1g of trimethylolpropane triacrylate and add them to a mixture of cyclohexane and ethyl acetate accounting for 50% of the total volume of the organic phase, then add a combined emulsifier formed by 0.4g of P123 and 0.3g of span80, and a combined co-emulsifier formed by 0.2g of BPO and 0.05g of hexadecanol and 0.05g of hexanol, and then ultrasonicate in an ultrasonic cleaning machine for 10 minutes to dissolve and mix evenly, as the oil phase, that is, the uniform organic phase;

[0133] Step 2: Weigh 7 g of 25% silica sol solution and stir with 9 g of deionized water to form the aqueous phase;

[0134] Step 3: Place the dissolved oil phase in an ice bath, and slowly drop the uniformly stirred water phase into the oil phase at a high-speed stirrer speed of 3000 r / min, so that the water phase accounts for 62% of the total volume of the emulsion obtained after full emulsification. After the drop is completed, increase the speed to 7000 r / min and stir for 9 minutes to fully emulsify, then add 0.7 g of a combined reducing agent (i.e., 0.3 g of N,N-dimethylaniline, 0.2 g of N,N,N,N-tetramethylethylenediamine and 0.2 g of sodium sulfite), and continue stirring for 1 minute to obtain a stable water-in-oil emulsion, i.e., a formed emulsion;

[0135] Step 4: Using a drop ball forming device to perform drop ball forming and aging on the formed emulsion, wherein the structure diagram of the drop ball forming device is as follows: Figure 1 As shown, from Figure 1 As can be seen from the figure, it includes a molding emulsion storage tank 1, a peristaltic pump 2 and a molding column 4 with a height of 1.8m, wherein the molding column 4 is a jacketed glass tube with openings at both ends, a drip tray 3 is provided on the upper opening of the jacketed glass tube, and a plurality of drop ball molding needles 31 are provided on the drip tray 3 facing the upper opening, and the lower opening of the jacketed glass tube is connected to the molding tank 5; the outlet of the molding emulsion storage tank 1 is connected to the inlet of the drip tray 3 through a pipeline via the peristaltic pump 2;

[0136] Droplet forming and aging specifically include:

[0137] Prepare an aqueous solution 6 of a dispersant, which in this embodiment is an aqueous solution of polyethylene glycol with a mass concentration of 0.3%, and pour it into the molding column, and then connect it to a water bath through a jacket, such as a water bath circulation heater, and heat it to 70° C. The molding tank, such as a conical flask, is heated at a temperature of 65° C. using a magnetic stirring heater to ensure that the pellets are fully formed;

[0138] The molding emulsion is transported to a drip tray by a peristaltic pump at a pump speed of 5.5 r / min, and the molding emulsion is dripped into the aqueous solution of polyethylene glycol contained in the jacketed glass tube at a dripping speed of 3 drops / second through a drop ball molding needle with an inner diameter of 0.45 mm. The molding emulsion forms a spherical shape under the action of surface tension in water and undergoes polymerization reaction and preliminary solidification. The preliminary solidified small balls fall into a molding tank and are aged at 65° C. for 15 minutes to obtain aged small balls.

[0139] The small balls were taken out and placed in an oven at 80° C. to dry for 6 hours, thereby preparing macroporous polymer balls, namely the polyacrylate spherical material.

[0140] Comparative Example 1

[0141] This comparative example provides a polyacrylate material, which is also prepared by a drop ball forming method. The difference between this comparative example and Example 1 is only that:

[0142] The amount of emulsifier P123 used was 0.1 g.

[0143] Comparative Example 2

[0144] This comparative example provides a polyacrylate material, which is also prepared by a drop ball forming method. The difference between this comparative example and Example 2 is only that:

[0145] The amount of deionized water used is 30 g.

[0146] Comparative Example 3

[0147] This comparative example provides a polyacrylate material, which is also prepared by a drop ball forming method. The difference between this comparative example and Example 3 is only that:

[0148] The amount of silica sol solution with a mass concentration of 28% is 1 g.

[0149] Comparative Example 4

[0150] This comparative example provides a polyacrylate material, which is also prepared by a drop ball forming method. The difference between this comparative example and Example 4 is only that:

[0151] Connect the jacket to a water bath, such as a water bath circulation heater, and heat to 50°C.

[0152] Comparative Example 5

[0153] This comparative example provides a polyacrylate material, which is also prepared by a drop ball forming method. The difference between this comparative example and Example 5 is only that:

[0154] The inner diameter of the drop ball forming needle is 1.2mm.

[0155] Comparative Example 6

[0156] This comparative example provides a polyacrylate material, which is prepared by an emulsion suspension polymerization method comprising the following specific steps:

[0157] Step 1: Weigh 2.1g of glycidyl methacrylate, 0.8g of tert-butyl methacrylate and 2.1g of trimethylolpropane triacrylate and add them into toluene accounting for 30% of the total volume of the organic phase, then add 0.3g of P123, 0.2g of benzoyl peroxide (BPO) and 0.1g of hexadecanol in sequence, and then ultrasonicate in an ultrasonic cleaner for 5min to dissolve and mix them evenly, as the oil phase, i.e., the uniform organic phase;

[0158] Step 2: Weigh 13 g of deionized water as the aqueous phase;

[0159] Step 3: Place the dissolved oil phase in an ice bath, and slowly add the water phase to the oil phase at a high-speed stirrer speed of 3000 r / min, so that the water phase accounts for 56% of the total volume of the emulsion obtained after full emulsification. After adding, increase the speed to 7000 r / min and stir for 5 minutes to fully emulsify. Then, add 0.3 g of reducing agent N,N-dimethylaniline and continue stirring for 1 minute to obtain a shaped emulsion.

[0160] Step 4: Measure 150 mL of water and add it to a 250 mL three-necked flask, add 0.15 g of ammonium persulfate and 1.5 mL of polyvinyl alcohol dispersant, stir with an electric stirrer at a speed of 300 rpm and heat in a constant temperature water bath at 45°C; after the temperature is kept constant for 10 minutes, add the formed emulsion prepared in step 3 to the three-necked flask, and the emulsion will be dispersed into spheres under the action of its own interfacial tension. After continuing to stir for 10 minutes, take out the balls and place them in an oven at 60°C to dry for 6 hours to prepare macroporous polymer balls, i.e., the polyacrylate material.

[0161] Comparative Example 7

[0162] This comparative example provides a polyacrylate material, which is also prepared by a drop ball forming method. The difference between this comparative example and Example 1 is only that:

[0163] No dispersant polyvinyl alcohol is added to the molding liquid, and pure water is used as the molding liquid.

[0164] The appearance of the polyacrylate spherical materials obtained in Examples 1 to 5 of the present invention is basically the same, and they are all regular spherical particles, that is, they have a high sphericity. Here, only the appearance pictures of the polyacrylate spherical materials obtained in Examples 2 and 5 are provided, respectively. Figure 2 and Figure 3 shown.

[0165] The physical pictures of the polyacrylate materials provided in Comparative Examples 2, 5 and 7 are as follows: Figure 4-Figure 6 As shown. Figure 4 and Figure 5 It can be seen that the appearance of the polyacrylate materials provided in Comparative Examples 2 and 5 is quite different, and most of them are ellipsoidal or irregularly shaped particles with poor sphericity. Figure 6 It can be seen that since Comparative Example 7 uses pure water as the forming liquid and no dispersant is used, the droplets adhere to each other into large lumps during the polymerization process and cannot be formed into monodisperse spheres.

[0166] In addition, the scanning electron microscope image of the polyacrylate spherical material prepared in Example 1 of the present invention is as follows: Figure 7 and Figure 8 As shown. Figure 7 and Figure 8 As can be seen from the figure, the internal details of the polyacrylate spherical material show that there are a large number of macroporous structures inside.

[0167] In addition, the molding effects of Examples 1 to 5 and Comparative Examples 1 to 7 of the present invention, the bulk density of the prepared polyacrylate spherical materials or polyacrylate material samples, and the mechanical strength data are all shown in Table 1 below.

[0168] Table 1

[0169]

[0170] From the molding effect data shown in Table 1 above, it can be seen that Examples 1 to 5 of the present invention have higher yields, good molding effects, and uniform particle sizes (the higher the yield, the more uniform the particle size), and polyacrylate spherical materials with higher bulk density that are suitable for fixed bed processes can be obtained.

[0171] It can also be seen from Table 1 that the amount of emulsifier in Comparative Example 1 was reduced to 2% of the total mass fraction of the organic monomers, resulting in emulsion demulsification and failure to form in the molding liquid, indicating that the amount of emulsifier should be controlled at 3-15% of the total mass fraction of the organic monomers, and should not be too little.

[0172] Comparative Examples 2 and 3 investigated the mass ratio of silica sol solution and deionized water. The results showed that if the amount of deionized water was too much, the oil and water phases in the emulsion would be unstable and difficult to form, and the yield would drop to 20%; when the amount of silica sol solution was too little, the density of the emulsion was small and it could not fall to form and polymerize, but floated to the liquid surface and broke, and could not be formed. This shows that the mass ratio of silica sol solution and deionized water should be controlled at 1:1-1:4.

[0173] In Comparative Example 4, the polymerization temperature in the molding column is 50°C. The low polymerization temperature causes the droplets to not be completely formed and the experiment fails, indicating that the polymerization temperature of the present invention should be controlled at 55-65°C.

[0174] The needle size used in Comparative Example 5 is 1.2 mm. As shown in Table 1, the yield of 0.85-2 mm in Comparative Example 5 is only 13.6%, indicating that the larger inner diameter of the droplet forming needle leads to a larger droplet size and a wider distribution range, and the sphericity is poor (e.g. Figure 5 As shown), the yield is reduced, indicating that in order to ensure that the carrier particle size is as uniform as possible, the needle size should be controlled at 0.3-1mm.

[0175] Comparative Example 6 was prepared by traditional emulsion suspension polymerization, and the results showed that its yield was only 41%, indicating that the drop ball forming method provided by the present invention can effectively improve the yield of the prepared polyacrylate spherical material sample and ensure good sphericity.

[0176] It can also be seen from Table 1 above that the polyacrylate spherical materials prepared in Examples 1 to 5 of the present invention all have higher mechanical strength, and compared with the existing emulsion suspension polymerization method, the mechanical strength of the polyacrylate spherical materials can be increased by more than 15%, and they are not easy to wear during the fixed bed operation. The higher mechanical strength of the polyacrylate spherical materials prepared in Examples 1 to 5 of the present invention can be attributed to the addition of hydrophilic silica sol.

[0177] Application Examples

[0178] To further evaluate the polyacrylate spherical material samples prepared in the examples and comparative examples of the present invention as fixed bed CO 2 The performance of the solid adsorbent carrier used for adsorption, this application example adopts the physical impregnation method, a certain amount of organic amine is loaded on the polyacrylate spherical material samples prepared in Examples 1 to 5 and Comparative Examples 1 to 6 of the present invention, and its adsorption performance is evaluated. The specific loading steps are: weigh 2g of the polyacrylate spherical material samples prepared in Examples 1 to 5 and Comparative Examples 1 to 6, respectively, and place them in a round-bottom flask, add 15g of pentaethylenehexamine, and use a rotary evaporator to rotate and impregnate for 6h at a temperature of 60°C. After the impregnation, wash with a small amount of alcohol, and then dry at a temperature of 40°C for 10h. Finally, a physical adsorption instrument is used to test the CO absorption of the polyacrylate spherical material samples loaded with pentaethylenehexamine at a temperature of 25°C and a pressure of 1 bar. 2 The specific results of adsorption capacity are shown in Table 2 below.

[0179] Table 2

[0180] project Adsorption capacity (mmol / g) project Adsorption capacity (mmol / g) Example 1 4.1 Comparative Example 1 Unformed Example 2 3.6 Comparative Example 2 2.5 Example 3 3.7 Comparative Example 3 Unformed Example 4 3.5 Comparative Example 4 Unformed Example 5 3.4 Comparative Example 5 2.9 Comparative Example 6 3.0 Comparative Example 7 Unformed

[0181] It can be seen from Table 2 above that under the same conditions, the polyacrylate spherical material sample prepared in the embodiment of the present invention is used as a fixed bed CO 2 CO adsorption on solid adsorbent carrier 2The adsorption capacity is significantly higher than that of the polyacrylate spherical material sample prepared in the comparative example, indicating that the polyacrylate spherical material sample prepared by the drop ball forming method provided by the present invention has a better CO 2 Adsorption performance.

[0182] The above is only a specific embodiment of the present invention, and cannot be used to limit the scope of the invention. Therefore, the replacement of equivalent components, or equivalent changes and modifications made according to the protection scope of the patent of the present invention, should still fall within the scope of this patent. In addition, the technical features of the present invention can be freely combined with each other, with each other and with each other, and with each other.

Claims

1. A drop ball forming method for polyacrylate spherical material, It is characterized in that The drop ball forming method of the polyacrylate spherical material comprises: Step 1: First, two or three organic monomers are added to the organic dispersed phase, and then an emulsifier, an initiator and an emulsifier are added in sequence to form a uniform organic phase; Step 2: Mixing the silica sol solution and deionized water to form an aqueous phase; Step 3: dropping the aqueous phase into the organic phase for full emulsification and then adding a reducing agent to obtain a formed emulsion; Step 4: using a drop ball forming device to perform drop ball forming and aging on the formed latex, and then drying the aged small balls to obtain the polyacrylate spherical material.

2. The drop ball forming method according to claim 1, It is characterized in that The organic monomers include two or three of the group consisting of glycidyl methacrylate, tert-butyl methacrylate, trimethylolpropane triacrylate, tert-butyl acrylate, methyl methacrylate, ethyl methacrylate, methyl acrylate, ethyl acrylate, styrene, and ethylene glycol dimethacrylate.

3. The drop ball forming method according to claim 2, It is characterized in that The organic monomers include glycidyl methacrylate, tert-butyl methacrylate and trimethylolpropane triacrylate in a mass ratio of 2-3.5:0.5-1.5:1.5-3.

4. The drop ball forming method according to claim 1, It is characterized in that Taking the total volume of the organic phase as 100%, the volume fraction of the organic dispersed phase is 30-50%.

5. The drop ball forming method according to claim 1 or 4, It is characterized in that The organic dispersed phase includes one or a combination of cyclohexane, toluene, carbon tetrachloride, dichloromethane, 1-2-dichloroethane, and ethyl acetate; preferably, one or a combination of toluene, cyclohexane, and ethyl acetate.

6. The drop ball forming method according to any one of claims 1 to 3, It is characterized in that Based on the total weight of the two or three organic monomers being 100%, the amounts of the emulsifier, the initiator and the co-emulsifier are 3-15%, 1-5% and 1-3% respectively.

7. The drop ball forming method according to claim 6, It is characterized in that The emulsifier includes one or a combination of span80, span60, span20, and a polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer.

8. The drop ball forming method according to claim 6, It is characterized in that The initiator includes one or a combination of ammonium persulfate, potassium persulfate, benzoyl peroxide, dicumyl peroxide, tert-butyl peroxide, azobisisobutyronitrile, and azobisisovaleronitrile.

9. The drop ball forming method according to claim 6, It is characterized in that The auxiliary emulsifier includes one or a combination of hexadecanol, hexanol, octanol, and p-nonylphenol.

10. The drop ball forming method according to claim 1, It is characterized in that The mass ratio of the silica sol solution to deionized water is 1:1-1:4, and the mass concentration of the silica sol solution is 25-35%.

11. The drop ball forming method according to claim 1, It is characterized in that The aqueous phase is dripped into the organic phase to fully emulsify the emulsion according to the aqueous phase accounting for 55-62% of the total volume of the emulsion obtained after full emulsification.

12. The drop ball forming method according to claim 1, It is characterized in that Based on the total weight of the two or three organic monomers being 100%, the amount of the reducing agent used is 5-15%.

13. The drop ball forming method according to claim 1 or 12, It is characterized in that The reducing agent includes one or a combination of N,N-dimethylaniline, N,N,N,N-tetramethylethylenediamine, ferrous sulfate, and sodium sulfite.

14. The drop ball forming method according to claim 1, It is characterized in that The entire step 3 is carried out in a low temperature environment to reduce the temperature of the formed emulsion to below 5°C.

15. The drop ball forming method according to claim 1, It is characterized in that The drop ball forming device comprises a forming emulsion storage tank, a peristaltic pump and a forming column. The forming column is a jacketed glass tube with upper and lower ends opened. A drip tray is arranged on the upper end opening of the jacketed glass tube. A plurality of drop ball forming needles are arranged on the drip tray facing the upper end opening. The lower end opening of the jacketed glass tube is connected to the forming tank. The outlet of the forming emulsion storage tank is connected to the inlet of the drip tray through a pipeline via the peristaltic pump.

16. The drop ball forming method according to claim 1 or 15, It is characterized in that In step 4, the forming emulsion is subjected to drop ball forming and aging by using a drop ball forming device, which comprises: Add the aqueous solution of dispersant into the jacketed glass tube so that both the jacketed glass tube and the molding tank are filled with the aqueous solution of dispersant and heat to 55-70° C. by connecting a water bath device through the jacket; The molding emulsion is transported to a drip tray by a peristaltic pump and dripped into a jacketed glass tube by a ball-dropping molding needle. The molding emulsion forms a spherical shape under the action of surface tension in water and undergoes polymerization and preliminary solidification. The preliminary solidified small balls fall into a molding tank and are aged at 55-65°C to obtain aged small balls.

17. The drop ball forming method according to claim 16, It is characterized in that The mass concentration of the aqueous solution of the dispersant is 0.13-0.3%; Preferably, the dispersant comprises polyvinyl alcohol and / or polyethylene glycol.

18. The drop ball forming method according to claim 16, It is characterized in that The height of the jacketed glass tube is 1-2 m; preferably, the inner diameter of the drop ball forming needle is 0.3-1 mm; also preferably, the dripping rate of the dripping is 1-3 drops / second.

19. A polyacrylate spherical material, It is characterized in that The polyacrylate spherical material is prepared by the drop ball forming method of the polyacrylate spherical material according to any one of claims 1 to 18; Preferably, the particle size of the polyacrylate spherical material is 0.85-2 mm, and the bulk density is >0.2 g / mL.

20. The polyacrylate spherical material according to claim 19 is used as a fixed bed CO 2 Application of solid adsorbent carriers used for adsorption.

21. A fixed bed CO 2 The solid adsorbent comprises a solid adsorption carrier and an adsorption active component loaded on the surface of the solid adsorption carrier. It is characterized in that The solid adsorption carrier is the polyacrylate spherical material as described in claim 19.

Citation Information

Patent Citations

  • Preparation method and use of polyacrylate / silica solution composite material

    CN102140217A

  • In situ polymerization micro-crosslinking sodium polyacrylate modified polyether sulfone microspheres as well as preparation method and application thereof

    CN104479354A

  • Silica sol / polyacrylic ester emulsion with high silicon content and preparation method of silica sol / polyacrylic ester emulsion

    CN104530302A

  • Preparation method of amino functionalized macroporous polymer sphere for adsorbing CO2

    CN107552019A

  • Vermiculite polyacrylamide composite for fluidized bed adsorption technology

    CN109225166A