Nitrogen-doped metal oxide material and preparation method thereof
Through wet gel method and nitrogen sintering technology, the preparation process of nitrogen-doped metal oxides is simplified, the problems of uneven doping of nitrogen elements and harsh conditions in the existing technology are solved, and efficient dye wastewater degradation and good quality are achieved. cycling performance.
Patent Information
- Application Number
- CN202411199954.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-12-06
AI Technical Summary
The existing nitrogen-doped mesoporous metal oxides have limited nitrogen-doping methods, resulting in uneven doping and harsh conditions, which cannot effectively reduce the band gap, and the preparation process is complicated, making it difficult to achieve efficient dye wastewater degradation.
The nitrogen-containing organic monomer and metal salt were reacted in a solvent by wet gel method, and after freeze-drying and sintering in a nitrogen atmosphere, a diversified nitrogen-doped metal oxide was prepared, which simplified the preparation process and improved doping uniformity. sex.
It realizes the simple and easy preparation of nitrogen-doped metal oxides, has excellent catalytic degradation performance, shows good degradation effect on different cationic dyes, and has good recycling performance.
Smart Images

Figure CN119076038A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of catalyst material preparation, in particular to a nitrogen-doped metal oxide material and a preparation method thereof. Background Art
[0002] With the rapid development of economy, organic pollutants such as dyes and antibiotics have caused harm to drinking water and ecological environment, posing a serious threat to human's normal life and environment.
[0003] The most notable feature of nitrogen-doped metal oxides is that they use organic polymers to form the material skeleton, and then metal atoms are complexed in the skeleton to form a special void structure, which has adsorption and catalytic degradation characteristics. It can efficiently degrade dyes in dye wastewater with hydrogen peroxide and carbonate and has excellent recycling performance, so it has broad application prospects in the field of dye wastewater remediation. At present, although there have been some reports on nitrogen-doped mesoporous metal oxides, nitrogen is generally introduced into mesoporous metal oxides through a gas phase (such as ammonia fumigation) strategy, resulting in nitrogen only being doped on the surface of the sample and unable to effectively reduce the band gap; secondly, the conditions for nitrogen doping are generally harsh (such as high temperature and strong reduction), resulting in the destruction of the mesostructure, and the resulting samples are generally non-porous or have disordered pores.
[0004] Therefore, it is particularly important to develop a simple and easy method to prepare nitrogen-doped metal oxides. Summary of the invention
[0005] The purpose of the present invention is to provide a nitrogen-doped metal oxide material and a preparation method thereof in view of the technical problems existing in the prior art. In the preparation method of the nitrogen-doped metal oxide, the raw materials for preparation are widely available, inexpensive, and the preparation process is simple. The prepared nitrogen-doped metal oxide has a diverse structure and exhibits excellent performance in the application of catalytic degradation of organic dyes.
[0006] In order to achieve the above invention object, the technical solution of the present invention is as follows:
[0007] A method for preparing a nitrogen-doped metal oxide comprises the following steps:
[0008] S1: adding a nitrogen-containing organic monomer to a solvent to prepare a mixed solution, then adding a metal salt to the mixed solution, and obtaining a metal salt mixed solution after the metal salt is evenly dissolved; adding a catalyst to the metal salt mixed solution to obtain a wet gel, aging the wet gel, and performing solvent exchange during the aging process to remove residual reactants;
[0009] S2: freeze-dry the gel obtained in S1 to obtain xerogel;
[0010] S3: The dry gel obtained in S2 is sintered at high temperature in a nitrogen atmosphere to finally obtain nitrogen-doped metal oxide.
[0011] As a preferred embodiment of the present application, in step S1 of the method for preparing a nitrogen-doped metal oxide, the nitrogen-containing organic monomer is chitosan.
[0012] As a preferred embodiment of the present application, in step S1 of the method for preparing a nitrogen-doped metal oxide, the solvent is any one of acetic acid, formamide, N-methylpyrrolidone, dimethyl sulfoxide and N,N-dimethylformamide. When the solvent is acetic acid, the concentration of acetic acid needs to be adjusted to 2wt%. Other solvents can directly use commercially available standard reagents, such as analytical grade.
[0013] As a better embodiment of the present application, in step S1 of the method for preparing a nitrogen-doped metal oxide, the metal salt is any one or two of CoCl2·6H2O, CuCl2·2H2O, NiCl2·6H2O, MnCl2·4H2O or ZnCl2.
[0014] As a better implementation in the present application, in step S1 of the method for preparing a nitrogen-doped metal oxide, the catalyst is 1,2-propylene oxide.
[0015] As a better implementation mode in the present application, in step S1 of the method for preparing a nitrogen-doped metal oxide, a nitrogen-containing organic monomer is added to a solution prepared with a solvent, and the concentration range of the organic monomer is 10-20 g / L; the mass ratio of the organic monomer to the metal ion in the metal salt is 2:1-1:9; and the volume ratio of the catalyst to the solvent is 1:50-4:25.
[0016] As a better implementation in the present application, in step S1 of the method for preparing a nitrogen-doped metal oxide, the aging time is 5-10 days.
[0017] As a better embodiment of the present application, in step S2 of the method for preparing a nitrogen-doped metal oxide, the freeze-drying conditions are: -50°C, vacuum below 10Pa, and the unbound water therein is completely removed directly, and the drying time is usually 3-5 days.
[0018] As a preferred embodiment of the present application, in step S3 of the method for preparing a nitrogen-doped metal oxide, the sintering conditions are: 5-15°C min -1 The temperature is raised to 600-800℃ at a heating rate, kept for 1h~4h, and then cooled naturally.
[0019] Another object of the present invention is to protect the nitrogen-doped metal oxide obtained by any one of the above methods or step combinations.
[0020] The third invention objective of the present invention is to protect the application of the nitrogen-doped metal oxide, which is used to prepare dye wastewater catalytic degradation materials.
[0021] As a better implementation in the present application, the nitrogen-doped metal oxide is used for the catalytic degradation of dye wastewater methylene blue, rhodamine B, and methyl violet.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] (i) In the present preparation method, a wet gel is first prepared by a wet gel method, and then freeze-dried and sintered in a nitrogen atmosphere. The preparation process is simple and easy.
[0024] (ii) The preparation method of the nitrogen-doped metal oxide of the present invention has a wide range of raw materials and is inexpensive; during the preparation, different nitrogen-doped metal oxide catalysts can be prepared according to nitrogen-containing organic monomers and different metal salts.
[0025] (III) The nitrogen-doped metal oxide prepared by the present invention has excellent catalytic degradation effect, has good degradation performance for different cationic dyes (methylene blue, rhodamine B, methyl violet, etc.), has short degradation time and good recycling performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 A schematic diagram of a process for preparing a nitrogen-doped metal oxide according to the present invention;
[0027] Figure 2 This is a product display picture, in which the left is wet gel, the middle is dry gel, and the right is nitrogen-doped metal oxide;
[0028] Figure 3 Activation condition screening and degradation performance diagram of the catalyst in Example 1 of the present invention;
[0029] Figure 4 The cyclic performance result diagram of the catalyst in Example 1 of the present invention;
[0030] Figure 5 Activation condition screening and degradation performance diagram of the catalyst in Example 2 of the present invention;
[0031] Figure 6 The cyclic performance result diagram of the catalyst in Example 2 of the present invention;
[0032] Figure 7 Activation condition screening and degradation performance diagram of the catalyst in Example 3 of the present invention;
[0033] Figure 8 Activation condition screening and degradation performance diagram of the catalyst in Example 4 of the present invention;
[0034] Fig. 9 Graph showing the cyclic performance results of the catalyst in Example 4 of the present invention. DETAILED DESCRIPTION
[0035] The following describes the embodiments of the present invention by specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention. It should be noted that the following embodiments and features in the embodiments can be combined with each other without conflict.
[0036] It should be noted that, in order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Generally, the components of the embodiments of the present invention described and shown in the drawings here can be arranged and designed in various different configurations.
[0037] Therefore, the following detailed description of the embodiments of the present invention provided in the accompanying drawings is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0038] The reagents in this application can all be obtained by purchase.
[0039] Embodiment 1:
[0040] A method for preparing a nitrogen-doped metal oxide comprises the following steps:
[0041] 1) First, 1 g of chitosan was dissolved in 50 mL of 2 wt% acetic acid solution, and then 3.14 g of CoCl2·6H2O was added. After uniform dissolution, 6 mL of 1,2-propylene oxide was added, and the mixture was stirred for 10 min and allowed to stand to obtain a wet gel. The obtained wet gel was solvent exchanged with deionized water for 5 days.
[0042] 2) The wet gel finally obtained in S1 is freeze-dried to obtain a dry gel; the freeze-drying conditions are: freeze-drying at -50°C and a vacuum degree of less than 10 Pa for 4 days.
[0043] 3) The obtained dry gel was heated at 10℃min under nitrogen atmosphere. -1 The temperature is raised to 600°C at a heating rate and kept at 600°C for 2 hours, and finally nitrogen-doped metal oxide (nitrogen-doped metal-based polymer material) is obtained.
[0044] The nitrogen-doped metal oxide prepared in this example was subjected to activation condition screening and performance testing experiments at room temperature. The specific steps are:
[0045] In 50 mL of methylene blue solution (initial concentration 10 mg L -1 ), 10 mg of the nitrogen-doped metal oxide prepared in Example 1, 100 μL of hydrogen peroxide, and 21.2 mg of an activator (sodium bicarbonate or sodium carbonate) were added to the mixture, 2 mL of the solution was sampled every 5 min, and solid-liquid separation was achieved by filtering with a 0.45 μm polypropylene syringe. The absorbance of the solution was tested at 665 nm, and the concentration of methylene blue in the solution was calculated according to the methylene blue solution standard curve. The additives and amounts in A1, A2, and A3 are shown in Table 1.
[0046] Table 1 Nitrogen doped cobalt metal at different ratios
[0047] serial number Chitosan(g) 2wt% acetic acid (mL) <![CDATA[CoCl2·6H2O(g)]]> <![CDATA[Ion mass ratio (Cs:M + )]]> 1,2-Propylene oxide (mL) A1 1.0 50 3.66 1:2 6 A2 1.0 50 1.83 1:1 6 A3 1.0 50 0.91 2:1 6
[0048] The test results are as follows: Figure 3 As shown. Figure 3 It can be seen that when sodium bicarbonate and hydrogen peroxide are selected as activation conditions, the catalyst has good degradation performance; at the same time, when the mass ratio of chitosan to metal cobalt ions is 1:2, the initial concentration of 10 mg L -1 The degradation of methylene blue can reach 96% in 25 min.
[0049] The obtained nitrogen-doped metal-based polymer material was subjected to a cycle performance test. The test results are as follows Figure 4 As shown. Figure 4 It can be seen that after the prepared nitrogen-doped metal oxide is recycled three times, the degradation efficiency is still maintained above 85%, indicating that it has certain recycling performance.
[0050] Embodiment 2:
[0051] A method for preparing a nitrogen-doped metal oxide (catalyst), comprising the following steps:
[0052] 1) First, 1 g of chitosan was dissolved in 50 mL of 2 wt% acetic acid solution, and then 3.14 g of MnCl2·4H2O was added. After the solution was uniformly dissolved, 6 mL of 1,2-propylene oxide was added, and the mixture was stirred for 15 min and allowed to stand to obtain a wet gel. The obtained wet gel was subjected to solvent exchange with deionized water for 7 days.
[0053] 2) The wet gel obtained in S1 is freeze-dried to obtain a dry gel; the freeze-drying conditions are: freeze-drying at -50°C and a vacuum degree of less than 10 Pa for 4 days.
[0054] 3) The obtained dry gel was heated at 10℃min under nitrogen atmosphere. -1 The temperature was raised to 600°C at a heating rate and kept at 600°C for 2.5 hours to finally obtain nitrogen-doped metal oxide (nitrogen-doped metal-based polymer material).
[0055] The nitrogen-doped metal oxide prepared in this example was subjected to activation condition screening and performance testing experiments at room temperature: the specific experimental steps were the same as those in Example 1; the raw materials and amounts used for B1 and B2 are shown in Table 2, and the specific results are shown in Table 2. Figure 5 .
[0056] Table 2 Nitrogen doped metal manganese with different proportions
[0057] serial number Chitosan(g) 2wt% acetic acid (mL) <![CDATA[CoCl2·6H2O(g)]]> <![CDATA[Ion mass ratio (Cs:M + )]]> 1,2-Propylene oxide (mL) B1 1.0 50 3.14 1:2 6 B2 1.0 50 1.57 1:1 6
[0058] from Figure 5 It can be seen that when sodium bicarbonate and hydrogen peroxide are selected as activation conditions, the catalyst has good degradation performance; when the mass ratio of chitosan to manganese ions is 1:2, the initial concentration of 10 mg L -1 The degradation of methylene blue can reach 80% in 210 min.
[0059] The obtained nitrogen-doped metal-based polymer material was subjected to a cycle performance test. The test results are as follows Figure 6 As shown. Figure 6 It can be seen that after the nitrogen-doped metal-based polymer material is cycled three times, the degradation efficiency remains above 60%, indicating that it has certain recycling performance.
[0060] Embodiment 3:
[0061] A method for preparing a nitrogen-doped metal oxide (catalyst), comprising the following steps:
[0062] 1) First, 1 g of chitosan was dissolved in 50 mL of 2 wt% acetic acid solution, and then CuCl2·2H2O was added. After the solution was uniformly dissolved, 6 mL of 1,2-propylene oxide was added, and the mixture was stirred for 12 min and allowed to stand to obtain a wet gel. The obtained wet gel was solvent exchanged with deionized water for 6 days.
[0063] 2) The wet gel obtained in S1 is freeze-dried to obtain a dry gel; the freeze-drying conditions are: freeze-drying at -50°C and a vacuum of less than 10Pa for 5 days.
[0064] 3) The obtained dry gel was heated at 10℃min under nitrogen atmosphere. -1The temperature is raised to 600°C at a heating rate and kept at 600°C for 2 hours, and finally nitrogen-doped metal oxide (nitrogen-doped metal-based polymer material) is obtained.
[0065] The nitrogen-doped metal oxide prepared in this example was subjected to activation condition screening and performance testing experiments at room temperature: the specific experimental steps were the same as those in Example 1; the raw materials and amounts used for C1-C3 are shown in Table 3, and the specific results are shown in Table 3. Figure 7 .
[0066] Table 3 Nitrogen doped metallic copper at different ratios
[0067] serial number Chitosan(g) 2wt% acetic acid (mL) <![CDATA[CuCl2·6H2O(g)]]> <![CDATA[Ion mass ratio (Cs:M + )]]> 1,2-Propylene oxide (mL) C1 1.0 50 2.53 1:2 6 C2 1.0 50 1.26 1:1 6 C3 1.0 50 0.63 2:1 6
[0068] from Figure 7 It can be seen that when sodium bicarbonate and hydrogen peroxide are selected as activation conditions, the catalyst has good degradation performance; when the mass ratio of chitosan to copper ions is 1:2, the initial concentration of 10 mg L -1 The degradation of methylene blue can reach 99.9% in 50 min.
[0069] Embodiment 4:
[0070] A method for preparing a nitrogen-doped metal oxide (catalyst), comprising the following steps:
[0071] 1) First, 1 g of chitosan was dissolved in 50 mL of 2 wt% acetic acid solution, and then CoCl2·6H2O and CuCl2·2H2O were added respectively. After uniform dissolution, 8 mL of 1,2-propylene oxide was added, and the mixture was stirred for 16 min and allowed to stand to obtain a wet gel. The obtained wet gel was solvent exchanged with deionized water for 7 days.
[0072] 2) The wet gel obtained in S1 is freeze-dried to obtain a dry gel; the freeze-drying conditions are: freeze-drying at -50°C and a vacuum of less than 10 Pa for 4 days.
[0073] 3) The obtained dry gel was heated at 10℃min under nitrogen atmosphere. -1 The temperature was raised to 600°C at a heating rate and kept at 600°C for 3 hours, and finally the nitrogen-doped metal-based polymer material was obtained.
[0074] The nitrogen-doped metal oxide prepared in this example was subjected to activation condition screening and performance testing experiments at room temperature: the specific experimental steps were the same as those in Example 1; the raw materials and amounts used for D1-D3 are shown in Table 4, and the specific results are shown in Table 4. Figure 8 .
[0075] Table 4 Nitrogen doped copper-cobalt composite metal oxides in different proportions
[0076]
[0077] from Figure 8 It can be seen that when sodium bicarbonate and hydrogen peroxide are selected as activation conditions, the catalyst has good degradation performance; at the same time, when the mass ratio of chitosan to metal is 1:2 and the mass ratio of copper to cobalt ions is 1:9, the prepared nitrogen-doped copper-cobalt composite metal oxide has good degradation performance for 10 mg L -1 The degradation rate of methylene blue was as high as 100% in 25 min.
[0078] The obtained nitrogen-doped metal-based polymer material was subjected to a cycle performance test. The test results are as follows Fig. 9 As shown. Fig. 9 It can be seen that the degradation efficiency of the nitrogen-doped metal-based polymer material is still as high as 80% after three cycles, indicating that it has certain recycling performance.
[0079] Comparative Example 1:
[0080] 1g sodium alginate was dissolved in 50mL 2wt% acetic acid solution, 1.2679g CuCl2·2H2O was added, and after uniform dissolution, 6mL 1,2-propylene oxide was added, and the mixture was stirred for 15min and allowed to stand, but no wet gel was obtained. No wet gel was obtained after further standing for 5-7 days.
[0081] Comparative Example 2:
[0082] 1 g of chitosan was dissolved in 50 mL of 2 wt% acetic acid solution, 1.2679 g of CuCl2·2H2O was added and dissolved evenly, then 6 mL of 1,2-propylene oxide was added, stirred for 10 min and allowed to stand to obtain a wet gel.
[0083] The obtained wet gel was solvent exchanged with deionized water for 7 days and dried at room temperature and pressure.
[0084] The obtained dry gel was heated at 10 °C min under nitrogen atmosphere. -1 The temperature was raised to 600°C at a heating rate and kept at 600°C for 2h, and finally a nitrogen-doped metal-based polymer material was obtained.
[0085] The performance test of the prepared material was carried out in the same manner as in Example 3 (activation conditions were also the same as those in the best solution in Example 3). The results showed that for an initial concentration of 10 mg L -1 Methylene blue, degradation, the results showed that the degradation rate was 80% at 150min.
[0086] Compared with the catalyst prepared in Example 3, the degradation time is 3 times that of the nitrogen-doped metal oxide in Example 3, and the degradation rate is only 80%.
[0087] Comparative Example 3:
[0088] 1 g chitosan and 1.2679 g CuCl2·2H2O were ground and mixed evenly. -1 The temperature was raised to 600°C at a heating rate of 100°C and kept at 600°C for 2 hours to obtain nitrogen-doped metal oxide (nitrogen-doped metal composite material) by sintering. That is, the gel step was not performed in this case, and the sintering preparation was directly performed.
[0089] The performance of the prepared material was tested in the same manner as in Example 3 (activation conditions were also the same as those in the best solution in Example 3). The results showed that the nitrogen-doped metal oxide had an initial concentration of 10 mg L -1 The degradation rate of methylene blue is 70% in 150 minutes. At the same time, there is precipitation of metal copper ions, which will cause secondary pollution to the environment.
[0090] The above-mentioned embodiments only express the specific implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the protection scope of the present application. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the technical solution concept of the present application, and these all belong to the protection scope of the present application.
[0091] This background section is provided to generally present the context of the invention, and the work of the presently named inventors, the work to the extent described in this background section, and aspects of this section that did not constitute prior art at the time of application are neither explicitly nor implicitly admitted to be prior art to the present invention.
Claims
1. A method for preparing a nitrogen-doped metal oxide, characterized in that The following steps are involved: S1: adding a nitrogen-containing organic monomer to a solvent to prepare a mixed solution, then adding a metal salt to the mixed solution, adding a catalyst after the metal salt is evenly dissolved to obtain a wet gel, aging the wet gel, and performing solvent exchange during the aging process to remove residual reactants; S2: freeze-dry the gel obtained in S1 to obtain xerogel; S3: The dry gel obtained in S2 is sintered at high temperature in a nitrogen atmosphere to finally obtain nitrogen-doped metal oxide.
2. The method for preparing a nitrogen-doped metal oxide according to claim 1, characterized in that: In step S1, the nitrogen-containing organic monomer is chitosan; the solvent is any one of acetic acid, formamide, N-methylpyrrolidone, dimethyl sulfoxide and N,N-dimethylformamide; the metal salt is any one of CoCl2·6H2O, CuCl2·2H2O, NiCl2·6H2O, MnCl2·4H2O or ZnCl2 or a mixture of two thereof; and the catalyst is 1,2-propylene oxide.
3. The method for preparing a nitrogen-doped metal oxide according to claim 2, characterized in that: When the solvent is acetic acid, the concentration of acetic acid is 2 wt %.
4. The method for preparing a nitrogen-doped metal oxide according to claim 1, characterized in that: In step S1, in the prepared mixed solution, the concentration of the organic monomer is 10-20 g / L; the mass ratio of the organic monomer to the metal ion in the metal salt is 2:1-1:9; and the volume ratio of the catalyst to the solvent is 1:50-4:
25.
5. The method for preparing a nitrogen-doped metal oxide according to claim 1, characterized in that: In step S1, the wet gel is aged for 5-10 days.
6. A method for preparing a nitrogen-doped metal oxide according to any one of claims 1 to 5, characterized in that: In step S2, the freeze-drying conditions are: -50°C, vacuum below 10Pa, and drying time of 3-5 days.
7. The method for preparing a nitrogen-doped metal oxide according to claim 6, characterized in that: In step S3, the high temperature sintering conditions are: 5-15℃min -1 The temperature is raised to 600-800℃ at a heating rate, kept for 1h~4h, and then cooled naturally.
8. The nitrogen-doped metal oxide obtained according to the method according to any one of claims 1 to 7.
9. The use of the nitrogen-doped metal oxide according to claim 8, characterized in that: The nitrogen-doped metal oxide is used for preparing dye wastewater catalytic degradation material.
10. The use of the nitrogen-doped metal oxide according to claim 9, characterized in that: The dye wastewater is methylene blue, rhodamine B and methyl violet.