Method for improving banded structure of Q355B hot-rolled round steel

Through the controlled rolling and cold control process, the strip structure of Q355B hot-rolled round steel is improved, and the serious problem of strip structure is solved, a low-cost and efficient production process is achieved, and the mechanical properties requirements of steel are met.

CN119076607APending Publication Date: 2024-12-06QINGDAO SPECIAL STEEL CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411171103.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

During the production process of Q355B hot rolled round steel, the strip-like tissue seriously leads to a decline in material performance. Most of the strip-like tissue produced by conventional processes are ≥4.0, which cannot directly meet the tissue performance requirements. Heat treatment is required to increase the processing process and cost.

Method used

Controlled rolling and cooling technology is adopted, including four-stage stepping gas furnace heating, high-pressure water descaling, controlled rolling and controlled cooling. The cooling rate is controlled through cooling water tank and cold bed to prevent grain growth and form high Ferrite and pearlite tissues of diffusion, band-shaped tissue ≤3.

Benefits of technology

Directly improve the strip structure, reduce subsequent heat treatment, reduce production costs, shorten production cycle, improve steel competitiveness, and meet the national standards and user needs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119076607A_ABST
    Figure CN119076607A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of special steel production and processing in the metallurgical industry, and provides a method for improving the banded structure of Q355B hot-rolled round steel, a Q355B continuous casting billet is used as a raw material, the production method sequentially comprises the following steps of gas furnace heating, high-pressure water descaling, controlled rolling, controlled cooling, cooling bed cooling and shearing sizing, and finally a finished product is obtained. Through the on-line controlled rolling and controlled cooling process, the banded structure is directly improved in the round steel rolling process, implementation is easy, and the production cost is low; the subsequent heat treatment process is reduced, the production cost is saved, the production period is shortened, and the market competitiveness of the steel is improved. The metallographic structure of the Q355B hot-rolled round steel produced through the method is ferrite and pearlite, the banded structure is smaller than or equal to grade 3, and the mechanical property reaches the national standard and can meet the requirements of users.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of special steel production and processing in the metallurgical industry, and specifically relates to a method for improving the banded structure of Q355B hot-rolled round steel. Background Art

[0002] During the production process of Q355B hot-rolled round steel, when the round steel is cooled to room temperature after high-temperature rolling, the metal structure transformation characteristics are: during the cooling process, austenite first precipitates proeutectoid ferrite in the carbon and alloy element depleted zone, and discharges excess carbon into the enriched zones on both sides, eventually forming a ferrite-dominated zone, and the carbon and alloy element-enriched zone subsequently forms a pearlite-dominated zone, thus forming a banded structure in which the ferrite-dominated zone and the pearlite-dominated zone alternate with each other.

[0003] The existence of banded structure is a manifestation of uneven internal structure and composition of steel. The more serious the banded structure, the worse the comprehensive performance of the steel. The plasticity, impact performance and fatigue life of the material will decrease to varying degrees. Banded structure is one of the important factors for the failure of parts. The banded structure of Q355B hot-rolled round steel produced by conventional processes is mostly ≥4.0. Users with high requirements for organizational performance cannot directly use the hot-rolled round steel and need to undergo heat treatment before use, which increases the processing flow and use costs. Summary of the invention

[0004] Aiming at the technical problem that the strip structure of hot-rolled round steel produced in the prior art is ≥ level 4, the present invention proposes a method for improving the strip structure of Q355B hot-rolled round steel through a controlled rolling and controlled cooling process.

[0005] To achieve the above object, the present invention provides the following technical solution, which comprises the following steps in sequence:

[0006] A method for improving the banded structure of Q355B hot-rolled round steel, using Q355B continuous casting billet as raw material, the production method sequentially comprises the following steps: gas furnace heating, high-pressure water descaling, controlled rolling, controlled cooling, cooling bed cooling, shearing and sizing;

[0007] The controlled rolling step includes rough rolling, intermediate rolling, water cooling before final rolling, and final rolling, wherein the rough rolling passes are 5 passes, the intermediate rolling passes are 4 to 16 passes, and the final rolling passes are 2 to 5 passes. Before final rolling, the final rolling temperature reaches 780° C. to 850° C. through a cooling water tank;

[0008] The controlled cooling step is to allow the round steel after final rolling to enter a post-rolling cooling water tank and be cooled to 590°C to 630°C at a speed of 3°C / s to 10°C / s.

[0009] Preferably, the gas furnace heating step is divided into four stages of heating, namely, preheating stage, heating stage I, heating stage II and soaking stage, the temperature of the preheating stage is ≤800°C, the heating temperature of the heating stage I is 1000°C~1120°C, the heating temperature of the heating stage II is 1180°C~1200°C, and the temperature of the soaking stage is 1180°C~1200°C; the total heating time in the heating process is 210~300min.

[0010] Preferably, the water pressure in the high-pressure water descaling step is 22 MPa.

[0011] Preferably, the water cooling step before intermediate rolling is to pass the semi-finished product after intermediate rolling through a cooling water tank to cool it to the final rolling temperature of 795°C to 810°C.

[0012] Preferably, the cooling rate in the controlled cooling step is 3.2°C / s, and the temperature is cooled to 602°C to 615°C.

[0013] Preferably, the cooling bed cooling step is to cool the round steel on the cooling bed to 400°C to 430°C.

[0014] The invention also proposes a Q355B hot-rolled round steel, which is prepared by the above method for improving the banded structure of Q355B hot-rolled round steel, and its hot-rolled banded structure is ≤ grade 3.

[0015] Compared with the prior art, the advantages and positive effects of the present invention are:

[0016] The method for improving the banded structure of Q355B hot-rolled round steel of the present invention directly improves the banded structure during the rolling process of round steel through an online controlled rolling and controlled cooling process, which is easy to implement and has low production cost; reduces the subsequent heat treatment process, saves production cost, shortens the production cycle, and improves the market competitiveness of steel; the production process can be fully controlled by PLC, with strong controllability and small quality fluctuation. The metallographic structure of Q355B hot-rolled round steel produced by the method is ferrite + pearlite, the banded structure is ≤3 levels, and the mechanical properties can meet the national standards and user requirements. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 The metallographic structure diagram of Q355B hot-rolled round steel produced in the embodiment of the present invention;

[0018] Figure 2 This is the metallographic structure diagram of Q355B hot-rolled round steel produced in the comparative example of the present invention. DETAILED DESCRIPTION

[0019] In order to make the purpose and technical solution of the present invention clearly and completely described, the embodiments of the present invention are described in detail in conjunction with the accompanying drawings. It should be understood that the specific embodiments described herein are part of the embodiments of the present invention, rather than all of the embodiments, and are only used to explain the embodiments of the present invention, and are not used to limit the embodiments of the present invention. All other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0020] Example

[0021] A method for improving the banded structure of Q355B hot-rolled round steel comprises the following steps:

[0022] (1) Select 240mm*300mm continuous casting billet.

[0023] (2) The continuous casting billet is heated in a four-stage step-beam gas furnace, and the heating temperature is: preheating section 595℃~615℃, heating section I 990℃~1010℃, heating section II 1180℃~1200℃, and soaking section 1180℃~1200℃, and the total heating time is 232min. The heating temperature in this step is higher than that in the traditional process. The four-stage step-beam high-temperature heating not only improves the plasticity of the steel, but also diffuses the C, Si, Mn and other components that are aggregated due to segregation inside the billet to a certain extent, which is beneficial to inhibit the re-aggregation of these elements during the rolling cooling process, thereby optimizing the banded structure.

[0024] (3) High-pressure water descaling: After the continuous casting billet is heated in a gas furnace, high-pressure water is used to remove the iron oxide scale produced by heating in step 2. The high-pressure water pressure is 22 MPa.

[0025] (4) Controlled rolling: After being descaled by high-pressure water, the continuous casting billet enters the rough rolling unit, the intermediate rolling unit, the cooling water tank and the final rolling unit for rolling in sequence. The rough rolling unit includes 5 high-rigidity rolling mills, the intermediate rolling unit includes 6 high-rigidity rolling mills, and the final rolling unit includes 5 high-rigidity rolling mills. There are 2 sets of cooling water tanks. The billet is rolled into a Φ80mm bar. By using the cooling water tank, the final rolling temperature is controlled at 795℃~810℃. At this temperature, the steel is in the austenite + ferrite two-phase region. When rolling at this temperature, the untransformed austenite grains are further elongated, forming deformation bands in the grains, and the transformed ferrite grains form substructures in the grains when they are pressed down. In the subsequent controlled cooling process, the former undergoes phase transformation to form fine polygonal ferrite and pearlite grains, while the latter recovers to become ferrite grains containing subgrains inside.

[0026] (5) Controlled cooling: After controlled rolling, the round steel enters the post-rolling cooling water tank and is cooled to 602°C to 615°C at a rate of 3.2°C / s. By working together with step 4, the grain growth is suppressed, and finally a high dispersion ferrite and pearlite structure is obtained without forming a wide ferrite band structure.

[0027] (6) Cooling on a cooling bed: Cool the round steel obtained in step (5) to 350°C to 450°C on a cooling bed.

[0028] (7) using a cold shearing machine to shear the round steel obtained in step (6) into 6 m fixed lengths to obtain a finished product.

[0029] The method described in this embodiment is used to roll 24 tons of round steel with a specification of Φ80 mm and a chemical composition of 0.19% C, 0.39% Si, 1.50% Mn, and the rest being the balance Fe and unavoidable impurities. Figure 1 The metallographic structure diagram of the Q355B hot-rolled round steel produced in this embodiment shows that the metallographic structure of the round steel produced in this embodiment is ferrite + pearlite. According to "GB / T 34474.1-2017 Evaluation of banded structure in steel Part 1: Standard rating diagram method", the banded structure level of the round steel rolled in this embodiment is 2. The round steel produced by the method described in 1-1 embodiment is randomly selected and tested according to "GBT 228.1-2010 Tensile test of metal materials Part 1: Room temperature test method". The mechanical properties of the above round steel are shown in Table 1. It can be seen from the table that the mechanical properties meet the requirements of GB / T1591-2018.

[0030] Table 1 Mechanical properties of round steel produced in the embodiment

[0031]

[0032] Comparative Example

[0033] The specific steps for processing Q355B hot-rolled round steel by traditional production methods are as follows:

[0034] (1) The same furnace as in the example was used for continuous casting, and the size and chemical composition of the continuous casting were consistent with those in the example.

[0035] (2) The continuous casting billet is heated in a four-stage walking-beam gas furnace at a heating temperature of 535°C to 565°C in the preheating stage, 980°C to 1000°C in the heating stage I, 1080°C to 1100°C in the heating stage II, and 1080°C to 1100°C in the soaking stage. The total heating time is 225 min to improve the plasticity of the steel.

[0036] (3) High-pressure water descaling: After the continuous casting billet is heated in a gas furnace, high-pressure water is used to remove the iron oxide scale generated by heating in step (2). The pressure of the high-pressure water is 22 MPa.

[0037] (4) Rolling: The descaling continuous casting billet is sent to the rough rolling, intermediate rolling and final rolling mills for rolling. The rough rolling mill includes 5 high-rigidity rolling mills, the intermediate rolling mill includes 6 high-rigidity rolling mills, and the final rolling mill includes 5 high-rigidity rolling mills. The final rolling temperature is ≥900°C, and the square billet is finally rolled into Φ80 mm bars.

[0038] (5) Cooling on cooling bed: The rolled round steel is cooled to 630℃~660℃ on the cooling bed.

[0039] (6) Use a cold shear to shear the round steel obtained in step 8 into 6-meter fixed lengths to obtain a finished product.

[0040] The round steel rolled by the above-mentioned traditional method has a specification of Φ80 mm and a chemical composition of 0.20% C, 0.39% Si, 1.50% Mn, and the rest is balanced Fe and inevitable impurities.

[0041] Figure 2 This is the metallographic structure diagram of the Q355B hot-rolled round steel produced in this comparative example. It can be seen from the figure that the metallographic structure of the round steel rolled in this comparative example is ferrite + pearlite. The same detection method as the embodiment is used for detection, and it can be obtained that its banded structure level is 4. By comparison, it can be seen that the banded structure of the embodiment is better. Ten round steels produced in the comparative example were extracted, and their mechanical properties were detected by the same detection method as the embodiment. The results are shown in Table 2. By comparison, it can be seen that the impact performance of the round steel in the embodiment is better than that of the comparative example, and the tensile performance is not significantly different from that of the embodiment.

[0042] Table 2 Mechanical properties of round steel produced in comparative example

[0043]

Claims

1. A method for improving the banded structure of Q355B hot-rolled round steel, characterized in that: The production method uses Q355B continuous casting billet as raw material, and comprises the following steps in sequence: heating with a gas furnace, descaling with high-pressure water, controlled rolling, controlled cooling, cooling on a cooling bed, and shearing to length; The controlled rolling step includes rough rolling, intermediate rolling, water cooling before final rolling and final rolling, wherein the rough rolling passes are 5 passes, the intermediate rolling passes are 4 to 16 passes, the final rolling passes are 2 to 5 passes, and the final rolling temperature reaches 780°C to 850°C through a cooling water tank before final rolling; The controlled cooling step is to allow the round steel after final rolling to enter a post-rolling cooling water tank and be cooled to 590°C to 630°C at a speed of 3°C / s to 10°C / s.

2. The method for improving the banded structure of Q355B hot-rolled round steel according to claim 1, characterized in that: The gas furnace heating step is divided into four stages of heating, namely, preheating stage, heating stage I, heating stage II and soaking stage, the temperature of the preheating stage is ≤800°C, the heating temperature of the heating stage I is 1000°C~1120°C, the heating temperature of the heating stage II is 1180°C~1200°C, and the temperature of the soaking stage is 1180°C~1200°C; the total heating time in the heating process is 210~300min.

3. The method for improving the banded structure of Q355B hot-rolled round steel according to claim 1, characterized in that: The water pressure in the high-pressure water descaling step is 22 MPa.

4. The method for improving the band structure of Q355B hot-rolled round steel according to claim 1, characterized in that: The water cooling step before intermediate rolling is to pass the semi-finished product after intermediate rolling through a cooling water tank to cool it to the final rolling temperature of 795°C to 810°C.

5. The method for improving the band structure of Q355B hot-rolled round steel according to claim 1, characterized in that: The cooling rate in the controlled cooling step is 3.2°C / s, and the temperature is cooled to 602°C to 615°C.

6. The method for improving the band structure of Q355B hot-rolled round steel according to claim 1, characterized in that: The cooling bed cooling step is to cool the round steel to 400°C to 430°C on the cooling bed.

7. A Q355B hot-rolled round steel, characterized in that: It is prepared by the method for improving the banded structure of Q355B hot-rolled round steel according to any one of claims 1 to 6, and its hot-rolled banded structure is ≤ grade 3.0.

Citation Information

Patent Citations

  • Minimizing rolling method of Q345q

    CN102021293A

  • Production method for low cost protection and flaw detection steel middle plate of low alloy structure

    CN112962025A

  • Bar hot rolling production line

    CN114289503A

  • Preparation method of wind power non-quenched and tempered steel bar suitable for cold machining

    CN114657349A

  • Rolling production method of non-quenched and tempered steel

    CN117086102A