Method for producing copper-clad cable wire rod with excellent surface quality by adopting square billet with section specification of 200mm
By using 200±5mm square billets in the production of copper-clad cable coils and controlling the oxygen content and rolling parameters of the steel in the middle bag, the surface defects and cutting tumor problems in the prior art are solved, and high-quality copper bags are achieved Cable coil production reduces scrap rate and production costs.
Patent Information
- Application Number
- CN202411191093.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-12-06
AI Technical Summary
In the production of copper-clad cable coils, the use of 150mm and 170mm square billets has surface defects, such as scarring, folding and ears, and the large cross-sectional size leads to a low pulling speed and a low cutting temperature during production of the casting machine. The formation of a cutting tumor affects the quality of the product.
Using a square billet with a cross-sectional specification of 200±5mm, the oxygen content of the steel in the middle is controlled to be 40~120PPm, and RH vacuum treatment and standstill to ensure that the length-width ratio of the end cutting tumor at the casting billet is within the appropriate range, and During the rolling process, accurately control the roller slots and outlet blank diameters of each pass to avoid surface defects.
The copper-clad cable coil strips have excellent surface quality, internal grain refinement, and excellent tissue status, which reduces the scrap cutting rate and surface defect rate, and improves production efficiency and cost-effectiveness.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to a method for producing a cable wire rod, in particular to a method for producing a copper-clad cable wire rod with excellent surface quality by using a square billet with a cross-sectional specification of 200 mm. The method is suitable for producing a copper-clad cable wire rod by using a square billet with a cross-sectional specification of 200±5 mm. Background Art
[0002] Cable steel series wire rod is one of the main raw materials for producing copper-clad steel. It is widely used in TV and telephone lines, intelligent wiring, electronic component leads, overhead lines for power transmission, overhead lines for electrified railway and light rail contact networks, braided shielding wires for power cables, grounding rods for the power industry, and other fields. Cable steel combines the excellent properties of copper and steel. It has the high strength and toughness of steel (about twice that of pure copper wire), the excellent conductivity and corrosion resistance of copper, and is light (12% lighter than pure copper wire), has no creep, and has good plasticity, weldability and magnetic properties. At the same time, it can withstand the attack of wind, snow and hail, and can withstand large spans, salt spray and corrosive environments, so it can reduce the distortion and distortion of transmitted information, improve transmission quality, and has the advantages of saving copper materials and reducing costs.
[0003] The process flow of making shielded copper-clad steel wire from cable steel wire rod is as follows: dry drawing → water tank drawing → annealing → copper plating → drawing after copper plating → fine drawing → pipeline annealing → finished wire. Due to the complex deep processing of wire rod and the multiple drawing processes, the wire rod with a general specification of 6.5mm is drawn to the finished product of about 0.1-0.3mm. The deformation during the drawing process is very large, reaching about 98%, so the surface quality requirements of the wire rod are extremely strict, and surface defects such as scarring, folding, and ears are not allowed. Summary of the invention
[0004] The present invention aims to overcome the shortcomings of the prior art using 150mm and 170mm square billets, and provide a method for producing copper-clad cable wire rods with excellent surface quality by using square billets with a cross-sectional specification of 200±5mm. Not only can the internal grains of the finished wire rods be more refined and the organizational state be excellent, but it can also overcome the problem of low pulling speed during casting machine production due to large cross-sectional dimensions, which in turn leads to low temperature during billet cutting and causes a cutting seam ≥5mm, while cutting tumors are easily formed on the upper and lower surfaces of the end portions. The surface of the produced cable wire rods is free of defects such as scars, folds, ears, etc., and the scrap cutting rate can be reduced by at least 2.5% compared with the current situation.
[0005] Measures to achieve the above objectives:
[0006] A method for producing copper-clad cable wire rods with excellent surface quality using square billets with a cross-sectional specification of 200 mm, the steps of which are as follows:
[0007] 1) Conventional converter smelting, during which the oxygen content of molten steel in the tundish is controlled at 40-120 ppm;
[0008] 2) Carry out RH vacuum treatment and control the oxygen content in the molten steel to be 15-30 PPm when the RH leaves the station;
[0009] 3) Allow the molten steel to stand for a period of ≤30 min;
[0010] 4) Casting and heating of billets: Control: Section specifications are 196~205mm×196~
[0011] For a 205mm square billet, the length-to-width ratio of the cutting nodule at the end of the billet is controlled according to the distance between the nodule at the end of the billet and any side of the billet: if it is within ≤70mm, the length-to-width ratio of the cutting nodule is controlled within
[0012] ≤3; when >70mm, it needs to be cut cleanly, and no residual cutting defects are allowed;
[0013] 5) Rolling is carried out. In order to accurately control the precise size of the wire rod at different stages, the control of the roll gap of each pass is achieved as follows:
[0014] The roll gap of the first pass is controlled at 12-13 mm; the roll gap of the second pass is controlled at 10-11 mm; the roll gap of the third pass is controlled at 11-12 mm; the roll gap of the fourth pass is controlled at 10-11 mm;
[0015] The roll gap of the fifth pass is controlled at 9-10mm;
[0016] The roll gap of the sixth pass is controlled at 8-9 mm, and the outlet billet diameter of this pass is controlled at 105-107 mm;
[0017] The roll gap of the seventh pass is controlled at 8-9 mm; the roll gap of the eighth pass is controlled at 5-7 mm; the roll gap of the ninth pass is controlled at 7-8 mm; the roll gap of the tenth pass is controlled at 4-5 mm;
[0018] The roll gap of the eleventh pass is controlled at 3.5-4.5 mm; the roll gap of the twelfth pass is controlled at 5-6 mm;
[0019] The roll gap of the thirteenth pass is controlled at 7.5-8.5 mm;
[0020] The roll gap of the fourteenth pass is controlled at 5-5.5 mm, and the outlet billet diameter of this pass is controlled at 40-41 mm;
[0021] The roll gap of the fifteenth pass is controlled at 3.6-3.7 mm; the roll gap of the sixteenth pass is controlled at 3.9-4.0 mm;
[0022] The roll gap of the 17th pass is controlled at 4.8-5.0 mm; the roll gap of the 18th pass is controlled at 4.4-4.5 mm;
[0023] The roller gap of the 19th pass is controlled at 4.3-4.5 mm;
[0024] The roll gap of the 20th pass is controlled at 3.0-3.1 mm, and the outlet billet diameter of this pass is controlled at 20-20.8 mm;
[0025] The roll gap of the 21st pass is controlled at 2.6-2.9 mm; the roll gap of the 22nd pass is controlled at 2.4-2.5 mm;
[0026] The roll gap of the 23rd pass is controlled at 1.4-1.5mm; the roll gap of the 24th pass is controlled at 1.5-1.6mm;
[0027] The roll gap of the 25th pass is controlled at 1.7-1.75 mm; the roll gap of the 26th pass is controlled at 1.0-1.1 mm;
[0028] The roll gap of the 27th pass is controlled at 1.4-1.45mm;
[0029] The roll gap of the 28th pass is controlled at 1.0-1.1 mm, and the outlet billet diameter of this pass is controlled at 8.4-8.8 mm;
[0030] The roll gap of the 29th pass is controlled at 1.55-1.6 mm; the roll gap of the 30th pass is controlled at 1.05-1.1 mm;
[0031] The roll gap of the 31st pass is controlled at 1.3-1.35mm;
[0032] The roller gap of the 32nd pass is controlled at 1.15-1.2 mm, and the outlet material diameter of this pass is controlled at 6.45-6.75 mm.
[0033] Preferably: the roll gap of the sixth pass is controlled at 8.5-9 mm, and the outlet billet diameter of the sixth pass is controlled at 106-107 mm;
[0034] The roll gap of the fourteenth pass is controlled at 5.2-5.5 mm, and the outlet billet diameter of this pass is controlled at 40.5-41 mm;
[0035] The roll gap of the 20th pass is controlled at 3.05-3.1 mm, and the outlet billet diameter of this pass is controlled at 20.5-20.8 mm;
[0036] The roll gap of the 28th pass is controlled at 1.05-1.1 mm, and the outlet billet diameter of this pass is controlled at 8.5-8.8 mm;
[0037] The roll gap of the 30th pass is controlled at 1.05-1.08 mm;
[0038] The roller gap of the 32nd pass is controlled at 1.17-1.18 mm, and the outlet material diameter of this pass is controlled at 6.5-6.7 mm.
[0039] Functions and mechanisms of each component and main process in the present invention
[0040] The reason why the present invention controls the oxygen content of the molten steel in the middle package to be between 40 and 120 ppm during the pouring of cable steel is that cable steel is a semi-killed steel. In order to remove excess oxygen in the steel, aluminum shots need to be added at RH for deoxidation. During the pouring process of the middle package, the Al in the molten steel is oxidized and remains in the steel, forming Al2O3 inclusions that block the nozzle. When the oxygen in the middle package is less than 40 ppm, the probability of nozzle nodules increases significantly. The reason why the present invention controls the oxygen content of the molten steel in the middle package to be between 40 and 120 ppm is that when the oxygen content in the molten steel is too high, as the solidification process of the molten steel proceeds during the pouring process, the solute elements (carbon, oxygen, nitrogen, and hydrogen) in the liquid phase between the dendrites are gradually enriched. When carbon and oxygen are enriched to a certain extent, exceeding the carbon-oxygen equilibrium value, a carbon-oxygen reaction will occur to generate CO gas. For square billet ultra-low carbon steel, the total pressure of the generated gas is mainly the pressure generated by CO gas:
[0041] P 生 =P CO +P N +P H (1)
[0042] The pressure to stop the gas from being generated: P 阻 =Patm+P 静 (2)
[0043]
C
O
[0044] In the above formula: P 生 : Total pressure of gas generated in steel, Pa;
[0045] P CO : Pressure of CO gas in steel, Pa;
[0046] P N : Pressure generated by N2 in steel, Pa;
[0047] P H : Pressure generated by H2 in steel, Pa;
[0048] P 阻 : The pressure to prevent the gas from being generated, Pa
[0049] Patm: atmospheric pressure, Pa;
[0050] P静 : Static pressure of molten steel, Pa;
[0051] When P 生 >P 阻 Macro bubbles will be generated, thus forming subcutaneous bubble defects on the ingot. If these bubbles are trapped by dendrites or blocked by the solidified surface layer and cannot escape from the steel, subcutaneous bubbles will be formed. Controlling the oxygen content of the molten steel in the tundish to 40-120 ppm can make the concentration product of [C] and [O] in the solidification process of the molten steel below the carbon-oxygen equilibrium value, so that the reaction of [C] + [O] = CO does not occur to form CO gas. Therefore, controlling the oxygen content of the molten steel in the tundish to 40-120 ppm can not only ensure that subcutaneous bubbles are not generated on the surface of the ingot, or generate slight subcutaneous bubbles that will not form surface scar defects after rolling, but also reduce the nozzle nodules during pouring, providing greater convenience for the smelting production of the ingot.
[0052] The reason why the present invention controls the oxygen content of the molten steel of the cable steel leaving the RH station to be 15-30 PPm, and the molten steel standing time after the treatment is controlled to be ≤30 min, is that the oxygen content of the molten steel of the cable steel in the middle package is positively correlated with the oxygen content of the molten steel leaving the RH station. The lower the oxygen content of the molten steel leaving the RH station, the lower the oxygen content of the middle package. As the calming time of the molten steel after the RH treatment increases, the amount of re-oxygenation in the molten steel increases, resulting in an increasing trend of the oxygen in the middle package. Controlling the oxygen content of the molten steel of the cable steel leaving the RH station to be 15-30 PPm, and the molten steel standing time after the treatment is controlled to be ≤30 min, the amount of re-oxygenation in the molten steel after the RH treatment can be reduced, thereby ensuring that the oxygen content of the molten steel in the middle package during continuous casting is mostly within the range of 40-120 PPm.
[0053] The reason why the present invention controls the length-to-width ratio of the cutting nodule within 70 mm of the end of the cable steel ingot to be controlled within ≤3, and residual cutting defects are not allowed to exist beyond 70 mm, is mainly based on the continuous casting and cutting characteristics of the production of 200×200 mm large-section ingots and the process shears are set after rough rolling of the rolling line, and the shearing length is set to 150-180 mm. The length-to-width ratio of the cutting nodule within 70 mm of the end of the ingot is too large, and residual cutting defects are allowed beyond 70 mm, which will result in the cutting nodule not being completely sheared off during the rolling process, forming defects such as scarring and foreign matter pressing on the surface of the wire rod; if the length-to-width ratio of the cutting nodule within 70 mm of the end of the ingot is set too small, the cleaning ratio of the cutting nodule on the ingot section will increase, and even the ingot cutting system will be modified, increasing labor costs and manufacturing costs.
[0054] The reason why the present invention controls the roll gap of each frame and the size of the circular hole of the finished frame of each assembly is that the carbon content of cable steel is extremely low and it is very sensitive to temperature changes. Moreover, this type of steel cools down quickly. The temperature difference between the front and rear halves of a steel bar becomes larger as the rolling time goes by, resulting in large changes in forward slip and width expansion as the temperature changes. In order to ensure that the second flow rates of the front and rear frames are equal during continuous rolling, thereby ensuring stable tension, it is necessary to reasonably set the roll gap of each frame during the production process, thereby ensuring strict control of the export size, ensuring that the second flow rates of the front and rear frames do not fluctuate greatly, stabilizing the tension and cross-sectional size, and preventing defects such as ears, folding and over-dimensioning on the surface.
[0055] Compared with the prior art, the present invention adopts a method for producing copper-clad cable wire rods with excellent surface quality by adopting square billets with a cross-sectional specification of 200 mm, which not only makes the internal grains of the finished wire rods more refined and the organizational state excellent, but also overcomes the problem that the pulling speed of the casting machine is low due to the large cross-sectional size, thereby making the temperature of the billet cutting low and causing the cutting seam ≥5mm, and cutting tumors are easily formed on the upper and lower surfaces of the end, so that the surface of the produced cable wire rods is free of defects such as scars, folds, ears, etc., the correction rate of scar defects in the finished product can be reduced by at least 5%, and the correction rate of defects such as folds and ears in the finished product can be reduced by at least 2%, thereby reducing the production cost.
[0056] Note: The cross-sectional dimensions of the ingot described in the present invention are not limited to 200 mm square ingots. The cross-sectional dimensions of the ingots within the range of 200 ± 5 mm square ingots are suitable for producing copper clad cable wire rods. DETAILED DESCRIPTION
[0057] The present invention is described in detail below:
[0058] Table 1 shows the oxygen content of molten steel in the tundish, the quality of the end cutting edge and the surface control of the wire rod in each embodiment and comparative example;
[0059] Table 2 shows the roll gap of the racks and the outlet dimensions of the last rack and the surface control of the wire rod of each embodiment of the present invention and the comparative example.
[0060] Each embodiment of the present invention is produced according to the following steps
[0061] 1) Conventional converter smelting, during which the oxygen content of molten steel in the tundish is controlled at 40-120 ppm;
[0062] 2) Carry out RH vacuum treatment and control the oxygen content in the molten steel to be 15-30 PPm when the RH leaves the station;
[0063] 3) Allow the molten steel to stand for a period of ≤30 min;
[0064] 4) Casting and heating of billets: Control: Section specifications are 196~205mm×196~
[0065] For a 205mm square billet, the length-to-width ratio of the cutting nodule at the end of the billet is controlled according to the distance between the nodule at the end of the billet and any side of the billet: if it is within ≤70mm, the length-to-width ratio of the cutting nodule is controlled within
[0066] ≤3; when >70mm, it needs to be cut cleanly, and no residual cutting defects are allowed;
[0067] 5) Rolling is carried out. In order to accurately control the precise size of the wire rod at different stages, the control of the roll gap of each pass is achieved as follows:
[0068] The roll gap of the first pass is controlled at 12-13mm; the roll gap of the second pass is controlled at 10-11mm;
[0069] The roll gap of the third pass is controlled at 11-12 mm; the roll gap of the fourth pass is controlled at 10-11 mm;
[0070] The roll gap of the fifth pass is controlled at 9-10mm;
[0071] The roll gap of the sixth pass is controlled at 8-9 mm, and the outlet billet diameter of this pass is controlled at 105-107 mm;
[0072] The roll gap of the seventh pass is controlled at 8-9 mm; the roll gap of the eighth pass is controlled at 5-7 mm;
[0073] The roller gap of the ninth pass is controlled at 7-8 mm; the roller gap of the tenth pass is controlled at 4-5 mm;
[0074] The roll gap of the eleventh pass is controlled at 3.5-4.5 mm; the roll gap of the twelfth pass is controlled at 5-6 mm;
[0075] The roll gap of the thirteenth pass is controlled at 7.5-8.5 mm;
[0076] The roll gap of the fourteenth pass is controlled at 5-5.5 mm, and the outlet billet diameter of this pass is controlled at 40-41 mm;
[0077] The roll gap of the fifteenth pass is controlled at 3.6-3.7 mm; the roll gap of the sixteenth pass is controlled at
[0078] 3.9~4.0mm;
[0079] The roll gap of the seventeenth pass is controlled at 4.8-5.0 mm; the roll gap of the eighteenth pass is controlled at
[0080] 4.4~4.5mm;
[0081] The roller gap of the 19th pass is controlled at 4.3-4.5 mm;
[0082] The roll gap of the 20th pass is controlled at 3.0-3.1 mm, and the outlet billet diameter of this pass is controlled at 20-20.8 mm;
[0083] The roll gap of the 21st pass is controlled at 2.6-2.9 mm; the roll gap of the 22nd pass is controlled at 2.4-2.5 mm;
[0084] The roll gap of the 23rd pass is controlled at 1.4-1.5mm; the roll gap of the 24th pass is controlled at 1.5-1.6mm;
[0085] The roll gap of the 25th pass is controlled at 1.7-1.75 mm; the roll gap of the 26th pass is controlled at 1.0-1.1 mm;
[0086] The roll gap of the 27th pass is controlled at 1.4-1.45mm;
[0087] The roll gap of the 28th pass is controlled at 1.0-1.1 mm, and the outlet billet diameter of this pass is controlled at 8.4-8.8 mm;
[0088] The roll gap of the 29th pass is controlled at 1.55-1.6 mm; the roll gap of the 30th pass is controlled at 1.05-1.1 mm;
[0089] The roll gap of the 31st pass is controlled at 1.3-1.35mm;
[0090] The roller gap of the 32nd pass is controlled at 1.15-1.2 mm, and the outlet material diameter of this pass is controlled at 6.45-6.75 mm.
[0091] Table 1 shows the oxygen content of molten steel in the tundish, the quality of the end cutting edge and the surface control of the wire rod in each embodiment and comparative example.
[0092]
[0093]
[0094] In the present invention, embodiments 1-4 produced about 4,500 tons of cable steel wire rods, of which only 3.3 tons of finished product scar defects were reclassified, with a reclassification rate of 0.07%. In contrast, comparative examples 1-2 produced about 4,400 tons of cable steel wire rods, of which 163 tons of finished product scar defects were reclassified, with a reclassification rate of 3.70%.
[0095] Table 2 The roll gap and the final stand outlet size and the surface control of the wire rod of each embodiment of the present invention and the comparative example
[0096]
[0097]
[0098] Table 2-1 continued
[0099]
[0100]
[0101] Table 2-2
[0102]
[0103]
[0104] In the present invention, embodiments 1-4 produced about 4,500 tons of cable steel wire rods, of which 7.2 tons of finished products were reclassified due to defects such as folds and ears, with a reclassification rate of 0.16%. In contrast, comparative examples 1-2 produced about 4,400 tons of cable steel wire rods, of which 29 tons of finished products were reclassified due to defects such as folds and ears, with a reclassification rate of 2.77%.
[0105] This specific implementation is only the best example and is not a restrictive implementation of the technical solution of the present invention.
Claims
1. A method for producing cable wire rods with excellent surface quality using square billets with a cross-sectional specification of 200 mm, the steps of which are: 1) Conventional converter smelting, during which the oxygen content of molten steel in the tundish is controlled at 40-120 ppm; 2) Carry out RH vacuum treatment and control the oxygen content in the molten steel to be 15-30 PPm when the RH leaves the station; 3) Allow the molten steel to stand for a period of ≤30 min; 4) Casting and heating of billets: Control: For square billets with section specifications of 196-205mm×196-205mm, the length-to-width ratio of the cutting nodule at the end of the billet is controlled according to the distance between the nodule at the end of the billet and any side of the billet: when it is within ≤70mm, the length-to-width ratio of the cutting nodule is controlled to be ≤3; when it is greater than 70mm, it needs to be cut cleanly, and no residual cutting defects are allowed; 5) Rolling is carried out. In order to accurately control the precise size of the wire rod at different stages, the control of the roll gap of each pass is achieved as follows: The roll gap of the first pass is controlled at 12-13mm; the roll gap of the second pass is controlled at 10-11mm; The roll gap of the third pass is controlled at 11-12 mm; the roll gap of the fourth pass is controlled at 10-11 mm; The roll gap of the fifth pass is controlled at 9-10mm; The roll gap of the sixth pass is controlled at 8-9 mm, and the outlet billet diameter of this pass is controlled at 105-107 mm; The roll gap of the seventh pass is controlled at 8-9 mm; the roll gap of the eighth pass is controlled at 5-7 mm; The roller gap of the ninth pass is controlled at 7-8 mm; the roller gap of the tenth pass is controlled at 4-5 mm; The roll gap of the eleventh pass is controlled at 3.5-4.5 mm; the roll gap of the twelfth pass is controlled at 5-6 mm; The roll gap of the thirteenth pass is controlled at 7.5-8.5 mm; The roll gap of the fourteenth pass is controlled at 5-5.5 mm, and the outlet billet diameter of this pass is controlled at 40-41 mm; The roll gap of the fifteenth pass is controlled at 3.6-3.7 mm; the roll gap of the sixteenth pass is controlled at 3.9-4.0 mm; The roll gap of the 17th pass is controlled at 4.8-5.0 mm; the roll gap of the 18th pass is controlled at 4.4-4.5 mm; The roller gap of the 19th pass is controlled at 4.3-4.5 mm; The roll gap of the 20th pass is controlled at 3.0-3.1 mm, and the outlet billet diameter of this pass is controlled at 20-20.8 mm; The roll gap of the 21st pass is controlled at 2.6-2.9 mm; the roll gap of the 22nd pass is controlled at 2.4-2.5 mm; The roll gap of the 23rd pass is controlled at 1.4-1.5mm; the roll gap of the 24th pass is controlled at 1.5-1.6mm; The roll gap of the 25th pass is controlled at 1.7-1.75 mm; the roll gap of the 26th pass is controlled at 1.0-1.1 mm; The roll gap of the 27th pass is controlled at 1.4-1.45mm; The roll gap of the 28th pass is controlled at 1.0-1.1 mm, and the outlet billet diameter of this pass is controlled at 8.4-8.8 mm; The roll gap of the 29th pass is controlled at 1.55-1.6 mm; the roll gap of the 30th pass is controlled at 1.05-1.1 mm; The roll gap of the 31st pass is controlled at 1.3-1.35mm; The roller gap of the 32nd pass is controlled at 1.15-1.2 mm, and the outlet material diameter of this pass is controlled at 6.45-6.75 mm.
2. The method for producing a cable wire rod with excellent surface quality by using a square billet with a cross-sectional specification of 200 mm as claimed in claim 1, characterized in that: The roll gap of the sixth pass is controlled at 8.5-9 mm, and the outlet billet diameter of this pass is controlled at 106-107 mm; The roll gap of the fourteenth pass is controlled at 5.2-5.5 mm, and the outlet billet diameter of this pass is controlled at 40.5-41 mm; the roll gap of the twentieth pass is controlled at 3.05-3.1 mm, and the outlet billet diameter of this pass is controlled at 20.5-20.8 mm; The roll gap of the 28th pass is controlled at 1.05-1.1 mm, and the outlet billet diameter of this pass is controlled at 8.5-8.8 mm; The roll gap of the 30th pass is controlled at 1.05-1.08 mm; The roller gap of the 32nd pass is controlled at 1.17-1.18 mm, and the outlet material diameter of this pass is controlled at 6.5-6.7 mm.
Citation Information
Patent Citations
Electric conduction ultra-low-carbon steel wire rod production method
CN110722330A
Adjusting method for rolling wire rod product with specification phi of 12.3 mm by double-pass system
CN111842480A
Roll gap setting method of wire Morgan rolling mill matched Dalnell reducing sizing mill
CN114160574A