Preparation method of high-plasticity pure titanium foil for bipolar plate of proton exchange membrane fuel cell
Through electron beam smelting, hot rolling and annealing treatment of high-purity titanium materials, the problem of poor plasticity of the bipolar foil of the proton exchange membrane fuel cell is solved, which improves the elongation rate, simplifies the production process and reduces costs, and promotes pure Commercial application of titanium bipolar plate.
Patent Information
- Application Number
- CN202411230239.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-04
- Publication Date
- 2024-12-06
AI Technical Summary
The pure titanium foil for bipolar plates of proton exchange membrane fuel cell have poor plasticity, which is difficult to meet production needs, and limits the widespread application of materials.
High-purity titanium material is used to mold through electron beam smelting, hot rolling, rough rolling, thin plate annealing and finish rolling, and control the annealing temperature and time, improve the elongation of the foil, reduce internal stress, and enhance plasticity.
It improves the elongation of pure titanium foil, meets the performance requirements of bipolar plates, simplifies production processes, reduces costs, and promotes large-scale commercial applications.
Smart Images

Figure CN119076624A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of proton exchange membrane fuel cells, and in particular to a method for preparing a high-plasticity pure titanium foil material for a proton exchange membrane fuel cell bipolar plate. Background Art
[0002] Proton exchange membrane fuel cells have broad application prospects in the fields of automobiles, aircraft and stationary power sources due to their outstanding features such as environmental friendliness, high energy efficiency and low operating temperature. Bipolar plates are one of the key components of proton exchange membrane fuel cells, accounting for 60%-80% of the weight and 25%-40% of the total cost. They support the stack, collect and transmit current and distribute reactant gases in proton exchange membrane fuel cells.
[0003] Metal bipolar plates have been widely used in the field of bipolar plate manufacturing due to their unique advantages such as ultra-low thickness, easy manufacturing, outstanding mechanical strength and low cost. Compared with other metal materials, pure titanium foil has the characteristics of low density and high specific strength. As a bipolar plate material, it can greatly reduce the total weight of proton exchange membrane fuel cells. In addition, pure titanium is composed of α phase and has excellent corrosion resistance, which can well resist H in the proton exchange membrane fuel cell environment. - 、F - Therefore, pure titanium is an ideal material for manufacturing bipolar plates of proton exchange membrane fuel cells.
[0004] However, common grades of pure titanium have low plasticity at room temperature, and the thickness of the metal foil used to make bipolar plates is required to be no more than 0.1 mm. Under extreme thickness conditions, the plasticity of pure titanium will be further reduced. Therefore, it is urgent to develop a preparation method for high-plasticity pure titanium foil to meet the production needs of pure titanium bipolar plates and promote large-scale commercial applications of pure titanium bipolar plates. Summary of the invention
[0005] The purpose of the present invention is to solve the problem of poor plasticity of pure titanium foil for bipolar plates of proton exchange membrane fuel cells, and to provide a method for preparing high-plasticity pure titanium foil for bipolar plates of proton exchange membrane fuel cells.
[0006] The technical solution of the present invention is as follows: A method for preparing a high-plasticity pure titanium foil for a proton exchange membrane fuel cell bipolar plate comprises the following steps:
[0007] 1) Melting: High-purity titanium is used as raw material, and then electron beam melting is used to form a pure titanium ingot, whose composition is Ti and inevitable impurities;
[0008] 2) Hot rolling: The ingot is forged into a block, heated to 900℃-1000℃, and kept warm for 2-12h. After completion, the block ingot is hot rolled by a rolling mill to obtain a pure titanium plate;
[0009] 3) Rough rolling: Use a rolling mill to cold roll the pure titanium sheet to obtain a thin plate with a thickness of 0.3-0.8 mm;
[0010] 4) Sheet annealing: The sheet is annealed in a heat treatment furnace at a temperature of 400°C-600°C for 5-10 minutes, and air-cooled to room temperature. Argon gas is used for protection during the sheet annealing process.
[0011] 5) Finish rolling: The thin plate is cold rolled using a rolling mill to obtain a foil with a thickness of 0.06-0.1 mm;
[0012] 6) Foil annealing: The foil is annealed in a heat treatment furnace at a temperature of 490°C-510°C for 4-6 minutes, and air-cooled to room temperature. The vacuum degree of the foil annealing process is <10Pa.
[0013] The total content of the inevitable impurities in step 1) is less than 0.005%, including C, N, O, H, Fe, etc.
[0014] The reduction ratio of the rough rolling in step 3) is 60%-85%.
[0015] The elongation of the thin plate after annealing in step 4) is 44%-74%.
[0016] The reduction ratio of the finishing rolling in step 5) is 66%-93%.
[0017] The foil after annealing in step 6) has an elongation of 34%-52% and a grain size of 2-10 μm.
[0018] The thin plate cold-rolled to 0.3-0.8 mm is annealed at 400°C-600°C for 5-10 minutes, and the grains inside the thin plate begin to grow. The migration and rearrangement of the grain boundaries gradually release the internal stress, avoiding the phenomenon of foil cracking caused by stress concentration during the finishing rolling process. In addition, the internal stress is released, the stress concentration is greatly reduced, the plasticity of the thin plate is improved, and it is more conducive to the foil forming in the subsequent finishing rolling process. If the annealing is performed below this temperature or time range, the internal stress of the thin plate will not be fully released and the expected effect cannot be achieved. If the annealing is performed above this temperature or time range, the internal stress of the thin plate cannot be further released, resulting in a waste of energy and an increase in production costs. Therefore, the thin plate annealing temperature in step 4) is 400°C-600°C, and the annealing time is 5-10 minutes.
[0019] The foil cold rolled to 0.06-0.1mm is annealed at 490℃-510℃ for 4-6min, and the deformed grains inside the foil are recrystallized into small equiaxed grains. The small equiaxed grains can promote the plastic deformation of the foil, making the foil have higher plasticity. If the annealing is performed below this temperature or time range, the deformed grains inside the foil cannot be completely transformed into small equiaxed grains, and there are still a large number of deformed grains, and the plasticity of the foil is poor. If the annealing is performed above this temperature or time range, the equiaxed grains inside the foil grow rapidly and become coarse. Coarse grains are not conducive to improving the plasticity of the foil. Therefore, the annealing temperature of the foil in step 6) is 490℃-510℃, and the annealing time is 4-6min.
[0020] Compared with the prior art, the present invention has the following beneficial effects:
[0021] The present invention provides a method for preparing a high-plasticity pure titanium foil for a proton exchange membrane fuel cell bipolar plate, which solves the problem of poor plasticity of existing grades of pure titanium foil. The pure titanium foil produced by the preparation method provided by the present invention can have an elongation of 34%-52%, which is at least 60% higher than the elongation of existing grades of pure titanium foil, meeting the performance requirements of room temperature stamping of bipolar plates. There is no need to adopt multi-stage stamping or high-temperature stamping processes due to poor material plasticity, thereby simplifying the bipolar plate production process and reducing production costs. In addition, the preparation method has low equipment dependence, and production can be completed on a two-roll rolling mill. It has the economy and feasibility of large-scale industrial production, can promote the large-scale commercial application of pure titanium bipolar plates, and contains huge economic potential. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1(a)-Figure 1(c) The metallographic phases of pure titanium foils prepared in Examples 1-3; FIG. 1( a ) corresponds to Example 1, FIG. 1( b ) corresponds to Example 2, and FIG. 1( c ) corresponds to Example 3.
[0023] Figure 2(a)-Figure 2(c) The microstructures of pure titanium foils prepared in Examples 1-3; FIG. 2( a ) corresponds to Example 1, FIG. 2( b ) corresponds to Example 2, and FIG. 2( c ) corresponds to Example 3.
[0024] Figure 3 The engineering stress-strain curve of the pure titanium foil prepared for Example 1-3;
[0025] Figure 4 The engineering stress-strain curves of pure titanium foil prepared in Comparative Examples 1-4. DETAILED DESCRIPTION
[0026] In order to better illustrate the present invention and facilitate understanding of the technical solution of the present invention, the specific implementation methods of the present invention are further described in detail:
[0027] Example 1
[0028] High-purity titanium is used as raw material, and then formed by electron beam melting. Its composition is Ti and inevitable impurities such as C, N, O, H, Fe, etc., and the total impurity content is less than 0.005%, to obtain a pure titanium ingot;
[0029] The ingot was forged into a block, heated to 900°C, and kept warm for 8 hours. After completion, the ingot was hot rolled using a rolling mill to obtain a 2mm thick pure titanium plate;
[0030] The 2 mm thick plate was cold rolled using a rolling mill with a reduction rate of 60% to obtain a 0.8 mm thick sheet;
[0031] The thin plate was annealed in a heat treatment furnace at a temperature of 600°C for 10 minutes, and then air-cooled to room temperature. Argon gas was used for protection during the annealing process.
[0032] The rolling mill cold-rolls the 0.8 mm thick sheet with a reduction of 87.5% to obtain a 0.1 mm thick foil;
[0033] The foil is annealed in a heat treatment furnace at a temperature of 500° C. for 5 minutes, and then air-cooled to room temperature. The vacuum degree during the foil annealing process is less than 10 Pa. The elongation of the foil at room temperature is 52.1%.
[0034] Example 2
[0035] The other operations are the same as those of Example 1 except for the following changes.
[0036] The rolling mill cold-rolls the 0.8 mm thick sheet with a reduction of 90% to obtain a 0.08 mm thick foil;
[0037] The foil is annealed in a heat treatment furnace at a temperature of 500° C. for 5 minutes, and then air-cooled to room temperature. The vacuum degree during the foil annealing process is less than 10 Pa. The elongation of the foil at room temperature is 38.6%.
[0038] Example 3
[0039] The other operations are the same as those of Embodiment 1 except for the following changes.
[0040] The 0.8 mm thick sheet was cold rolled using a rolling mill with a reduction ratio of 92.5% to obtain a 0.06 mm thick foil;
[0041] The foil is annealed in a heat treatment furnace at a temperature of 500° C. for 5 minutes, and then air-cooled to room temperature. The vacuum degree during the foil annealing process is less than 10 Pa. The elongation of the foil at room temperature is 34.2%.
[0042] Comparative Example 1
[0043] The operation is the same as that of Embodiment 1 except for the following changes.
[0044] The foil is annealed in a heat treatment furnace at a temperature of 550° C. for 30 minutes, and then air-cooled to room temperature. The vacuum degree during the foil annealing process is less than 10 Pa. The elongation of the foil at room temperature is 34%.
[0045] Comparative Example 2
[0046] The operation is the same as that of Embodiment 1 except for the following changes.
[0047] The foil is annealed in a heat treatment furnace at a temperature of 600° C. for 30 minutes, and then air-cooled to room temperature. The vacuum degree during the foil annealing process is less than 10 Pa, and the elongation of the foil at room temperature is 25%.
[0048] Comparative Example 3
[0049] The operation is the same as that of Embodiment 1 except for the following changes.
[0050] The foil is annealed in a heat treatment furnace at a temperature of 650° C. for 30 minutes, and then air-cooled to room temperature. The vacuum degree during the foil annealing process is less than 10 Pa. The elongation of the foil at room temperature is 22%.
[0051] Comparative Example 4
[0052] The operation is the same as that of Embodiment 1 except for the following changes.
[0053] The foil is annealed in a heat treatment furnace at a temperature of 700° C. for 30 minutes, and then air-cooled to room temperature. The vacuum degree during the foil annealing process is less than 10 Pa. The elongation of the foil at room temperature is 17%.
Claims
1. A method for preparing a high-plasticity pure titanium foil for a proton exchange membrane fuel cell bipolar plate, characterized in that: The following steps are involved: 1) Melting: High-purity titanium is used as raw material, and then electron beam melting is used to form a pure titanium ingot, whose composition is Ti and inevitable impurities; 2) Hot rolling: The ingot is forged into a block, heated to 900℃-1000℃, and kept warm for 2-12h. After completion, the block ingot is hot rolled by a rolling mill to obtain a pure titanium plate; 3) Rough rolling: Use a rolling mill to cold roll the pure titanium sheet to obtain a thin plate with a thickness of 0.3-0.8 mm; 4) Sheet annealing: The sheet is annealed in a heat treatment furnace at a temperature of 400°C-600°C for 5-10 minutes, and air-cooled to room temperature. Argon gas is used for protection during the sheet annealing process. 5) Finish rolling: The thin plate is cold rolled using a rolling mill to obtain a foil with a thickness of 0.06-0.1 mm; 6) Foil annealing: The foil is annealed in a heat treatment furnace at a temperature of 490°C-510°C for 4-6 minutes, and air-cooled to room temperature. The vacuum degree of the foil annealing process is <10Pa.
2. The method for preparing a high-plasticity pure titanium foil for a proton exchange membrane fuel cell bipolar plate according to claim 1, characterized in that: The total content of the unavoidable impurities in step 1) is less than 0.005%.
3. The method for preparing a high-plasticity pure titanium foil for a proton exchange membrane fuel cell bipolar plate according to claim 1, characterized in that: The reduction ratio of the rough rolling in step 3) is 60%-85%.
4. The method for preparing a high-plasticity pure titanium foil for a proton exchange membrane fuel cell bipolar plate according to claim 1, characterized in that: The elongation of the thin plate after annealing in step 4) is 44%-74%.
5. The method for preparing a high-plasticity pure titanium foil for a proton exchange membrane fuel cell bipolar plate according to claim 1, characterized in that: The reduction ratio of the finishing rolling in step 5) is 66%-93%.
6. A method for preparing a high-plasticity pure titanium foil for a proton exchange membrane fuel cell bipolar plate according to any one of claims 1 to 5, characterized in that: The foil after annealing in step 6) has an elongation of 34%-52% and a grain size of 2-10 μm.
Citation Information
Patent Citations
Preparation method of ultrathin titanium strip for bipolar plate of hydrogen fuel cell
CN114589213A
High-efficiency low-cost micron-sized titanium and titanium alloy foil preparation method with ultra-large width-to-thickness ratio
CN117960786A
Preparation method of wide pure titanium foil strip
CN118403896A
Titanium alloy plate and method for producing the same
JP2023040457A