Method for preparing metal iron powder by using vanadium extraction tailings
By using reducing agents and additives in vanadium extraction tailings for high-temperature roasting and magnetic separation processes, the problems of low iron recovery efficiency and high cost in vanadium extraction tailings are solved, and efficient and low-cost metal iron powder recycling is achieved, reducing the number of Environmental pollution has important resource utilization value.
Patent Information
- Application Number
- CN202411190216.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-12-06
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The problem of low efficiency and high cost of iron recovery technology in vanadium tail slag.
The mixture of vanadium-elevating tailings, graphite powder, lignite powder or anthracite powder and additives such as calcium carbonate and calcium fluoride is used for high-temperature reduction and roasting, and then the iron grade is gradually improved through grinding-magnetic separation technology to reach 90~ 95% of metal iron powder is recycled.
It has achieved efficient recycling of iron powder, with iron grade reaching 90.31%, and a recovery rate of 91.98%, reducing production costs, reducing environmental pollution, alleviating the shortage of iron concentrates, and promoting the recycling and utilization of valuable metals.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of recycling vanadium extraction tailings, and in particular relates to a method for preparing metallic iron powder by utilizing vanadium extraction tailings. Background Art
[0002] Vanadium tailings are a type of solid waste from steel companies. They contain high levels of alkaline oxides and sulfur, and are produced in large quantities each year. Open-air stacking not only occupies a large amount of land, but also causes serious pollution to the surrounding soil and water environment. The iron content in vanadium tailings exceeds 30%, which has a high recycling value. However, due to its complex composition, people pay little attention to the technology of extracting iron from it.
[0003] The iron in vanadium extraction tailings mainly exists in the form of ferrous oxide, which has no magnetism and cannot be directly enriched by magnetic separation. The traditional method of recovering iron from vanadium extraction tailings has problems such as low recovery efficiency and high cost.
[0004] Therefore, developing an efficient and low-cost iron recovery technology for vanadium extraction tailings has important practical application value. Summary of the invention
[0005] The technical problem to be solved by the present invention is the low efficiency and high cost of the existing iron recovery technology in vanadium extraction tailings.
[0006] The technical solution adopted by the present invention to solve the technical problem is: a method for preparing metallic iron powder using vanadium extraction tailings, comprising the following steps:
[0007] a. After uniformly mixing the vanadium extraction tailings, the reducing agent and the additive, the reduction product is obtained by reduction roasting and cooling;
[0008] b. The reduced product is subjected to a first-stage grinding-magnetic separation to obtain an intermediate product with a TFe content of 80-85%, and the intermediate product is subjected to a second-stage grinding-magnetic separation to obtain a metallic iron powder with a TFe content of 90-95%.
[0009] In the above step a, the mass of the reducing agent accounts for 25-35% of the mass of the vanadium extraction tailings, and the mass of the additive accounts for 5-15% of the mass of the vanadium extraction tailings.
[0010] Furthermore, the main chemical components of the vanadium extraction tailings are TFe 25-35%, SiO2 10-20%, MnO 5-15%, Al2O3 5-15%, CaO 5-20%, S2-5%, and TiO2 5-20% by mass percentage; the particle size of the vanadium extraction tailings is less than 200 mesh, accounting for 100%, and less than 250 mesh, accounting for 85%.
[0011] Furthermore, the reducing agent is at least one of graphite powder, lignite powder and anthracite powder; the particle size of the reducing agent is less than 3 mm, and the carbon content is greater than 80%.
[0012] Furthermore, the additive is at least one of calcium carbonate, CaO and calcium fluoride; and the particle size of the additive is less than 1 mm.
[0013] In the above step a, the reduction roasting is carried out in a high temperature reduction device at 1150-1350° C. for 1-2 hours.
[0014] Furthermore, the high-temperature reduction equipment is at least one of a high-temperature rotary kiln, a push-plate kiln and a vertical furnace.
[0015] In the above step a, the calcined product is cooled to room temperature by a water quenching process.
[0016] In the above step b, the concentration of the first grinding stage is 65-75%, the fineness of -74 μm accounts for 50-100%; the magnetic field strength of the first magnetic separation stage is 130-150 KA / m, and the selection ratio is 20-30%.
[0017] In the above step b, the concentration of the second-stage grinding is 65-75%, the fineness of -45 μm accounts for 50-100%; the magnetic field strength of the second-stage magnetic separation is 40-50 KA / m, and the selection ratio is 70-80%.
[0018] The beneficial effects of the present invention are as follows: the present invention provides a method for preparing metallic iron powder by roasting-magnetic separation process of vanadium extraction tailings, reducing iron oxide to metallic iron by coal-based direct reduction method, and then realizing iron recovery by magnetic separation. The present invention has the following advantages: (1) High efficiency recovery: through roasting and magnetic separation process, metallic iron can be effectively recovered from vanadium extraction tailings, the iron grade reaches 90.31%, and the recovery rate is 91.98%; (2) Low cost: using cheap lignite and CaO as reducing agent and flux, reducing production cost; (3) Environmental protection benefit: reducing the accumulation of vanadium extraction tailings and avoiding pollution to the environment. The method of the present invention can not only alleviate the shortage of iron ore concentrate, but also realize the recovery and utilization of valuable metals in vanadium extraction tailings, which is of great significance for the effective utilization of resources in my country and has broad application prospects and practical value. DETAILED DESCRIPTION
[0019] The technical solution of the present invention can be specifically implemented in the following manner.
[0020] The method for preparing metallic iron powder using vanadium extraction tailings comprises the following steps:
[0021] a. After uniformly mixing the vanadium extraction tailings, the reducing agent and the additive, the reduction product is obtained by reduction roasting and cooling;
[0022] b. The reduced product is subjected to a first-stage grinding-magnetic separation to obtain an intermediate product with a TFe content of 80-85%, and the intermediate product is subjected to a second-stage grinding-magnetic separation to obtain a metallic iron powder with a TFe content of 90-95%.
[0023] In the above step a, the mass of the reducing agent accounts for 25-35% of the mass of the vanadium extraction tailings, and the mass of the additive accounts for 5-15% of the mass of the vanadium extraction tailings. Among them, the main chemical components of the vanadium extraction tailings are TFe 25-35% (all iron exists in the form of FeO, and the FeO content is 30-50%), SiO2 10-20%, MnO 5-15%, Al2O3 5-15%, CaO 5-20%, S2-5%, TiO2 5-20% by mass percentage; the particle size of the vanadium extraction tailings <200 mesh accounts for 100%, and <250 mesh accounts for 85%. The reducing agent is at least one of graphite powder, lignite powder and anthracite powder; the reducing agent particle size is <3mm, and the carbon content is >80%. The additive is at least one of calcium carbonate, CaO and calcium fluoride; the additive particle size is <1mm. The type of flux has a great influence on the type, melting point, density and viscosity of the slag after reduction, and is an important factor affecting smelting. In the roasting and reduction process of the present invention, selecting a suitable additive can promote the reduction of the vanadium-extracting tailings, thereby saving a large amount of roasting and reduction costs.
[0024] In the above step a, the reduction roasting is carried out in a high temperature reduction device at 1150-1350° C. for 1-2 hours; wherein the high temperature reduction device is at least one of a high temperature rotary kiln, a push plate kiln and a vertical furnace. The cooling adopts a water quenching process to cool the roasted product to room temperature.
[0025] In the above step b, the concentration of the first grinding is 65-75%, the fineness is -74μm accounting for 50-100%; the magnetic field strength of the first magnetic separation is 130-150KA / m, and the selection ratio is 20-30%, that is, after the first magnetic separation of 100 tons of vanadium tailings, 20-30 tons of metal iron powder with a TFe content of 80-85% are obtained. The concentration of the second grinding is 65-75%, the fineness is -45μm accounting for 50-100%; the magnetic field strength of the second magnetic separation is 40-50KA / m, and the selection ratio is 70-80%, that is, after the second magnetic separation of the original 100 tons of vanadium tailings, 15-25 tons of metal iron powder with a TFe content of 90-95% are obtained.
[0026] The technical solution and effects of the present invention are further illustrated below through practical examples.
[0027] Example
[0028] The present invention provides three groups of Examples 1 to 3 for preparing metallic iron powder using vanadium extraction tailings by the method of the present invention. The chemical composition of the vanadium extraction tailings used in Examples 1 to 3 is shown in Table 1. The specific preparation method is as follows.
[0029] Table 1 Main chemical composition of titanium slag smelting dust removal ash (by mass percentage / %)
[0030] Example 1 Example 2 Example 3 TFe 30 35 35 FeO 40 45 45 <![CDATA[SiO2]]> 15 20 10 MnO 10 15 10 <![CDATA[Al2O3]]> 10 5 15 CaO 15 5 10 S 4 3 5 <![CDATA[TiO2]]> 6 7 5
[0031] Example 1
[0032] (1) Using brown coal powder as a reducing agent, the addition ratio is 30% (that is, adding 30 grams of brown coal powder to every 100 grams of vanadium extraction tailings); selecting calcium carbonate as an additive, the addition ratio is 10% (that is, adding 10 grams of calcium carbonate to every 100 grams of vanadium extraction tailings).
[0033] (2) performing reduction in a high-temperature rotary kiln, wherein the reduction temperature is set to 1200° C. and the holding time is 1.5 hours; and using a water quenching process to cool the reduced product to room temperature.
[0034] (3) In the grinding-magnetic separation process, the magnetic field strength of the first magnetic separation is 140KA / m, and the magnetic field strength of the second magnetic separation is 45KA / m. After two stages of grinding-magnetic separation, a metal iron powder with a TFe content of 92% and a selection ratio of 20% is obtained, that is, 20 tons of metal iron powder with a TFe content of 92% is obtained from 100 tons of vanadium extraction tailings.
[0035] Example 2
[0036] (1) Anthracite powder is used as a reducing agent at a ratio of 25%; CaO is selected as an additive at a ratio of 15%.
[0037] (2) Reduction is carried out in a push plate kiln, the reduction temperature is set to 1150° C., and the insulation time is 2 hours; the reduced product is placed in high-speed circulating water and quickly cooled to room temperature.
[0038] (3) In the grinding-magnetic separation process, the magnetic field strength of the first magnetic separation is 130KA / m, and the magnetic field strength of the second magnetic separation is 50KA / m. After two stages of grinding-magnetic separation, a metal iron powder with a TFe content of 95% and a selection ratio of 22% is obtained, that is, 22 tons of metal iron powder with a TFe content of 95% is obtained from 100 tons of vanadium tailings.
[0039] Example 3
[0040] (1) Graphite powder and lignite powder are used as reducing agents in combination, with the addition ratio being 15% and 20% respectively; calcium fluoride is selected as an additive, with the addition ratio being 5%.
[0041] (2) performing reduction in a vertical furnace, with the reduction temperature set at 1350° C. and the holding time being 1 hour; and using a water quenching process to cool the reduced product to room temperature.
[0042] (3) In the grinding-magnetic separation process, the magnetic field strength of the first magnetic separation is 150KA / m, and the magnetic field strength of the second magnetic separation is 40KA / m. After two stages of grinding-magnetic separation, a metal iron powder with a TFe content of 90% and a selection ratio of 25% is obtained, that is, 25 tons of metal iron powder with a TFe content of 90% is obtained from 100 tons of vanadium tailings.
Claims
1. A method for preparing metallic iron powder using vanadium extraction tailings, characterized in that: The steps include: a. After uniformly mixing the vanadium extraction tailings, the reducing agent and the additive, the reduction product is obtained by reduction roasting and cooling; b. The reduced product is subjected to a first-stage grinding-magnetic separation to obtain an intermediate product with a TFe content of 80-85%, and the intermediate product is subjected to a second-stage grinding-magnetic separation to obtain a metallic iron powder with a TFe content of 90-95%.
2. The method for preparing metallic iron powder using vanadium extraction tailings according to claim 1, characterized in that: In step a, the mass of the reducing agent accounts for 25-35% of the mass of the vanadium extraction tailings, and the mass of the additive accounts for 5-15% of the mass of the vanadium extraction tailings.
3. The method for preparing metallic iron powder using vanadium extraction tailings according to claim 2, characterized in that: The main chemical components of the vanadium extraction tailings are TFe 25-35%, SiO2 10-20%, MnO 5-15%, Al2O3 5-15%, CaO 5-20%, S2-5%, and TiO2 5-20% by mass percentage; the particle size of the vanadium extraction tailings is less than 200 mesh, accounting for 100%, and less than 250 mesh, accounting for 85%.
4. The method for preparing metallic iron powder using vanadium extraction tailings according to claim 2, characterized in that: The reducing agent is at least one of graphite powder, lignite powder and anthracite powder; the particle size of the reducing agent is less than 3 mm, and the carbon content is greater than 80%.
5. The method for preparing metallic iron powder using vanadium extraction tailings according to claim 2, characterized in that: The additive is at least one of calcium carbonate, CaO and calcium fluoride; and the particle size of the additive is less than 1 mm.
6. The method for preparing metallic iron powder using vanadium extraction tailings according to claim 1, characterized in that: In step a, the reduction roasting is carried out in a high temperature reduction device at 1150-1350° C. for 1-2 hours.
7. The method for preparing metallic iron powder using vanadium extraction tailings according to claim 6, characterized in that: The high temperature reduction equipment is at least one of a high temperature rotary kiln, a push plate kiln and a vertical furnace.
8. The method for preparing metallic iron powder using vanadium extraction tailings according to claim 1, characterized in that: In step a, the calcined product is cooled to room temperature by a water quenching process.
9. The method for preparing metallic iron powder using vanadium extraction tailings according to claim 1, characterized in that: In step b, the concentration of the first grinding stage is 65-75%, the fineness of -74 μm accounts for 50-100%; the magnetic field strength of the first magnetic separation stage is 130-150 KA / m, and the selection ratio is 20-30%.
10. The method for preparing metallic iron powder using vanadium extraction tailings according to claim 9, characterized in that: In step b, the concentration of the second-stage grinding is 65-75%, the fineness is -45 μm accounting for 50-100%; the magnetic field strength of the second-stage magnetic separation is 40-50 KA / m, and the selection ratio is 70-80%.
Citation Information
Patent Citations
Process method of tailings in vanadium extraction
CN101280361A
Technique method for directly producing sponge iron by carrying out deep reduction on extracted vanadium tailings
CN101713007A
Technology for producing vanadium chromium manganese alloyed pig iron by melting vanadium extraction tailings
CN102337444A
Lead slag and coal-based direct reduction method for producing metal iron powder
CN102658369A
Treatment system and method for vanadium extraction tailings
CN106636628A
Cited By
Method for preparing wear-resistant alloy containing vanadium, chromium and iron by using vanadium extraction tailings
CN121896475A