Preparation method of tin-based antioxidant solder alloy with core-shell structure
Through the coating technology of antioxidant intermediate alloy-rosin-tin foil-boron nitride coating hollow mold with core-shell structure in tin-based solder alloy, the serious oxidation and insufficient antioxidant performance of the tin-based solder alloy are solved. The problem of this paper has achieved efficient improvement in oxidation resistance and environmentally friendly production process.
Patent Information
- Application Number
- CN202411269396.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-11
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-09-11
AI Technical Summary
During the welding process, the existing tin-based solder alloys have severe oxidation and increased scum, resulting in decreased reliability and poor appearance of solder joints. In addition, the traditional antioxidant element addition method has insufficient dissolution, easy oxidation and safety. Issues such as risks and environmental impact.
The preparation method of tin-based antioxidant solder alloy with core-shell structure is formed by coating the antioxidant intermediate alloy with high softening point rosin and tin foil on the antioxidant intermediate alloy block, and then coated with boron nitride hollow mold to form the antioxidant intermediate alloy-rosin-tin foil -The structure of boron nitride coated hollow mold improves the dissolution and protection effect of antioxidant elements.
Significantly improves the yield of antioxidant elements and the antioxidant properties of the solder, reduces alloy smelting temperature, reduces oxidation and burnout, improves the operating environment, reduces production costs, and improves the static and dynamic mirror maintenance of the solder state.
Smart Images

Figure CN119077221A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of methods for preparing solder alloys for electronic packaging, and in particular relates to a method for preparing a tin-based antioxidant solder alloy with a core-shell structure. Background Art
[0002] Tin-based solder alloys are widely used in electronic soldering processes such as wave soldering and dip soldering due to their low melting point and good comprehensive performance. Compared with reflow soldering and selective soldering, the large molten pool of double-peak wave soldering and dip soldering exposes the solder surface to atmospheric conditions, causing severe oxidation of the solder surface and increased scum, which can easily lead to problems such as reduced reliability of solder joints and poor appearance after soldering. Therefore, in the preparation and use of tin-based solder, it is critical to add sufficient micro-alloy elements with antioxidant properties.
[0003] In the process of preparing solder alloy samples, from the perspective of alloy elements, due to factors such as low solubility or high melting point, the addition of antioxidant elements is divided into single substance form and intermediate alloy form. If the method disclosed in Chinese patent CN106271187A is adopted to directly add antioxidant metal elements to the tin alloy melt, such as Ge, whose melting point is close to 938°C, requires a higher melting temperature and consumes more energy; P is flammable, poses a safety risk, and is easy to burn; Ga's melting point (about 30°C) is much lower than the mainstream lead-free solder alloy melting point (210~230°C), is easy to burn, and P, Ge and Ga elements are easy to enrich on the surface of the solder melt. If they are added directly as single substances, on the one hand, the components are easy to segregate, and on the other hand, the three antioxidant elements are easy to be entrained in the tin slag, resulting in the antioxidant element content in the alloy matrix being far lower than the design value. In addition, if the method disclosed in Japanese patent JP4445046B2 and Chinese patent CN 112322929 A is adopted to simply add the antioxidant intermediate alloy Sn-P-Ge-Ga into the tin pool, because the density of the antioxidant alloy is close to that of the solder alloy melt, and the antioxidant elements are easily enriched on the surface and easily oxidized and burned under high temperature conditions, the antioxidant element content in the actual alloy matrix is lower than the initial addition amount, and the expected static and dynamic antioxidant properties of the solder will be significantly reduced.
[0004] In the actual production process of solder products, in terms of improving the anti-oxidation performance of solder, ammonium chloride (see Chinese patent CN106271187A) and fluoride (see Chinese patent CN114833490A) are usually added to the solder alloy melt and stirred to prepare solder alloy products. However, chemical materials such as chlorine and fluorine are easy to volatilize pungent or toxic gases at high temperatures when the solder is molten, which not only affects the health of operators but also has an adverse impact on the environment. In addition, adding intermediate alloys and covering the alloy surface with rosin (see Chinese patent CN115383349A) is also a way to reduce solder oxidation and increase metal yield, but there are limitations such as the lack of rosin selection and dosage leading to smoke diffusion, excessive carbides on the alloy surface affecting melt purification, or poor anti-oxidation effect of solder. There is also a method of using stainless steel and graphite bell jars to press the metal into the bottom of the melt and keep it for a period of time until it is completely melted, but elements such as Fe and Cr in stainless steel and carbon impurity elements in graphite are easily mixed in the solder alloy, affecting the reliability of the solder joint. Summary of the invention
[0005] The purpose of the present invention is to solve the deficiencies of the above-mentioned prior art and to provide a method for preparing a core-shell structured tin-based antioxidant solder alloy, so as to improve the problems that the antioxidant solder is directly placed on the surface of the antioxidant alloy melt during its preparation, resulting in insufficient dissolution of the alloy elements, the elements being easily oxidized and failing, and thus low antioxidant element yield, high slag production, and the antioxidant performance failing to meet expectations during the use of the solder, so as to effectively improve the antioxidant performance of the static melt surface and enhance the mirror-like retention state of the dynamic melt surface.
[0006] The objective of the present invention is achieved through the following technical solutions: The preparation method of the core-shell structure tin-based anti-oxidation solder alloy is to use an anti-oxidation master alloy block as a matrix, coat the anti-oxidation master alloy block with a high softening point rosin, then wrap tin foil as a secondary outer layer, and then coat a boron nitride hollow mold as the outermost layer to form a core-shell structure of an anti-oxidation master alloy-rosin-tin foil-boron nitride coating hollow mold; the anti-oxidation master alloy block is a SnPGa anti-oxidation master alloy block or a SnPGe anti-oxidation master alloy block. In order to enhance the synergistic anti-oxidation effect of P, Ga, and Ge elements, the mass ratio of P to Ga in the SnPGa anti-oxidation master alloy is 1:5; the mass ratio of P to Ge in the SnPGe anti-oxidation master alloy is 1:2. The mass ratio of the high softening point rosin to the anti-oxidation master alloy is 0.02:1, which can eliminate the oxide layer and promote wetting while reducing the amount of smoke generated when the rosin evaporates. The volume ratio of the anti-oxidation master alloy block to the boron nitride coating hollow mold is 1:1.3. It is convenient to place the anti-oxidation master alloy and protect the mold, so as to obtain the multi-component tin-based anti-oxidation solder master alloy with a core-shell structure.
[0007] The preparation method of the core-shell structure tin-based antioxidant solder alloy comprises the following steps: (1) Under argon protection conditions, an oxygen-resistant master alloy block is prepared in a closed melting furnace; (2) Use a stainless steel hollow mold with a lid, spray a boron nitride coating evenly on the stainless steel surface, and bake the mold at 80°C for 2 hours to obtain a boron nitride coated hollow mold. The boron nitride coated hollow mold not only has high thermal stability against corrosion, but also can overcome the density of the tin alloy melt and automatically sink to the bottom of the alloy melt due to gravity, without manual pressing; (3) Heat the high softening point KE604 rosin to 150°C in a beaker, immerse the anti-oxidation master alloy block in the molten rosin, keep it for 2 seconds, and then quickly lift the anti-oxidation master alloy block. At this time, the surface of the anti-oxidation master alloy block is covered with a rosin layer, and the surface oxide of the anti-oxidation master alloy can be removed. Wrap a layer of tin foil outside the rosin layer, then open the lid of the boron nitride coating hollow mold, put the rosin and tin foil coated anti-oxidation master alloy block into the boron nitride coating hollow mold and cover it, and obtain a core-shell structured multi-component tin-based anti-oxidation master alloy; finally, add the core-shell structured multi-component tin-based anti-oxidation master alloy into a 280°C tin alloy melt and cast it into the mold to prepare the tin-based anti-oxidation solder alloy.
[0008] The present invention has the following advantages: Compared with the direct addition of single Ge metal and SnP, SnGe binary master alloys, the core-shell structured multi-component tin-based antioxidant master alloy of the present invention has a greatly improved antioxidant element yield of more than 90%, that is, the gap between the nominal content and the actual content of the antioxidant elements is further narrowed, and the accuracy of antioxidant element addition is significantly improved.
[0009] The multi-component antioxidant master alloy of the present invention is added to the solder in the form of a core-shell structure, and the antioxidant performance of the solder is significantly improved, including the static melt surface being able to maintain a mirror state, static oxidation weight gain, dynamic mirror retention time, dynamic cycle scraping slag production, etc. are all greatly improved.
[0010] (3) Compared with the single Ge metal and SnP, SnGe binary intermediate alloys directly added at a tin-based alloy melt temperature higher than 320°C, the core-shell structured multi-component tin-based antioxidant intermediate alloy of the present invention only requires a tin alloy melt temperature of 280°C, which further reduces the alloy melting temperature and reduces the energy consumption of solder alloy preparation.
[0011] (4) The shell-structured multi-component tin-based antioxidant master alloy of the present invention is added to the solder and sinks to the bottom of the melt due to gravity, which can effectively reduce oxidation and burning loss and fully dissolve the antioxidant master alloy, shorten the stirring time and melting time, and improve the efficiency of antioxidant solder preparation.
[0012] (5) When the core-shell structured multi-component tin-based antioxidant alloy of the present invention is added to solder, it will not generate irritating gases such as chlorine, thereby improving the operating environment and effectively reducing the amount of tin slag generated, thereby reducing the production cost of the enterprise. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] Figure 1 This is a static oxidation surface picture of the solder of Example 1 of the present invention; Figure 2 This is a static oxidation surface picture of the solder of Example 2 of the present invention; Figure 3 This is a static oxidation surface picture of the solder of Comparative Example 1 of the present invention; Figure 4 This is a static oxidation surface picture of the solder of Comparative Example 2 of the present invention; Figure 5 This is a static oxidation surface picture of the solder of Comparative Example 3 of the present invention; Figure 6 This is a static oxidation surface picture of the solder of Comparative Example 4 of the present invention; Figure 7 It is the TG static oxidation weight gain curve of the solder of Examples 1-2 of the present invention and Comparative Examples 1-4; Figure 8 This is a picture of the dynamic oxidation surface of the solder in Example 1 of the present invention; Fig. 9 This is a picture of the dynamic oxidation surface of the solder according to Example 2 of the present invention; Fig.10 This is a picture of the dynamic oxidation surface of the solder of Comparative Example 3 of the present invention; Fig.11 This is a picture of the dynamic oxidation surface of the solder of Comparative Example 4 of the present invention; Fig.12 This is a picture of the dynamic oxidation surface of the solder of Comparative Example 1 of the present invention; Fig.13 This is a picture of the dynamic oxidation surface of the solder of Comparative Example 2 of the present invention; Fig.14 It is a statistical diagram of the amount of dynamic oxidation slag of solder cycle scraping in Examples 1-2 of the present invention and Comparative Examples 1-4; Fig.15 is a graph showing the surface etching of solder oxidation in Example 1 of the present invention; Fig.16 is a graph showing the surface etching of solder oxidation in Example 2 of the present invention; Fig.17 This is a graph showing the surface etching of solder oxidation in Comparative Example 1 of the present invention; Fig.18 This is a graph showing the surface etching of solder oxidation in Comparative Example 2 of the present invention; Fig.19This is a graph showing the surface etching of solder oxidation in Comparative Example 3 of the present invention; Fig. 20 This is a graph showing the surface etching of solder oxidation in Comparative Example 4 of the present invention; Fig.21 This is a schematic diagram of a boron nitride coated cage-type hollow mold; Fig. 22 yes Fig.21 A-direction view; Fig.23 This is a schematic diagram of a frame-type hollow mold with a boron nitride coating; Fig.24 yes Fig.23 B view. DETAILED DESCRIPTION
[0014] The present invention is further described in detail below by way of examples, but the protection scope of the present invention is not limited to the contents described in the examples.
[0015] The antioxidant element composition of the solder alloy and the antioxidant performance of the solder surface obtained in the following examples and comparative examples are tested to analyze the technical effect of the present invention. The cage-type or frame-type hollow mold used in the present invention is obtained by welding stainless steel bars. Fig.21 , Fig. 22 The cage-type hollow mold shown in the embodiment has an outer diameter of 55 mm, an inner diameter of 50 mm, and an internal volume of 65.45 cm 3 The cage-type hollow mold can be Fig.21 , Fig. 22 As shown, it is composed of two upper and lower hemispherical hollow half molds 1, one side of the two hollow half molds is connected by a hinge shaft 2, and the other side can be fastened by a buckle 3, and the buckle structure can adopt the existing technical structure. The upper hollow half mold is the lid, which can be opened and closed by rotating along the hinge shaft 2. After the lid is closed, the upper and lower hollow half molds can be fastened with the buckle 3. The cage-type structure hollow mold can also adopt other opening structures. Fig.23 , Fig.24 The frame-type hollow mold shown in the embodiment has an inner side length of 50 mm and an inner volume of 125 cm 3 , the frame structure hollow mold can be Fig.23 , Fig.24As shown, it is composed of a square hollow frame 4 and a cover 5 covering the top of the hollow frame. One side of the cover is connected by a hinge shaft 2, and the other side can be fastened by a buckle 3. The cover can be opened and closed by rotating along the hinge shaft 2. After the cover is closed, the top cover can be fastened to the hollow frame by the buckle 3. The frame-type structure hollow mold can also adopt a hollow frame and an opening structure of other structures. The alloy composition testing equipment used in the present invention is a SPECTROLABM10 direct reading spectrometer, and the test sample is a solder alloy cylinder with a diameter and a height of 30 mm and 10 mm, respectively; the composition test standard refers to the YS / T747-20108 standard, and the number of parallel samples is not less than 3. The oxidation resistance of the solder is comprehensively reflected by the alloy melt surface under static atmospheric conditions, TG oxidation weight gain, the slag production of dynamic cycle scraping, the surface state of the dynamic oxidation melt, and the oxidation thickness of the solder surface. The static and dynamic melt surface states of the solder alloy were tested using a solder alloy melt surface oxidation state test device with Chinese patent application number 2024215083379. The static oxidation and dynamic oxidation heating temperatures were 300°C, the static oxidation and dynamic cycle scraping times were both 2 hours, and the cycle scraping rate was 1 minute / time. The amount of dynamic oxidation slag was weighed using a METTLER TOLEDO ME204E analytical balance. The test equipment for solder oxidation weight gain was a STA449F5 weight loss thermal analyzer, and the test sample mass was a solder alloy sphere of 300 mg; the temperature was raised to 300°C under Ar gas conditions, then kept warm for 2 h under O2 conditions, and then cooled to room temperature in an Ar atmosphere. The heating and cooling rates were both 20 K / min, and the temperature range was between 30 and 300°C. The oxide layer on the solder surface was tested using a Thermofisher K-Alpha X-ray photoelectron spectrometer (XPS). The X-ray source was a monochromatic Al target (1486.7 eV). The ion source for sputtering was an Ar single ion beam with an energy resolution of ≤0.5 eV (with the half-peak width of Ag3d as a reference) and an etching rate of 0.54 nm / s. Example 1
[0016] A tin-based antioxidant alloy with a core-shell structure is prepared and added to SnCu0.7 solder as an intermediate alloy to obtain SnCu0.7P0.0032Ga0.016 antioxidant solder alloy. The specific steps are: (1) Under argon protection conditions, a closed melting furnace was used to prepare about 393.19 g of Sn0.32PGa1.6 anti-oxidation master alloy block, with a mass ratio of P to Ga of 1:5; (2) Design and prepare Fig.21 The cage-type stainless steel hollow mold shown has an inner diameter of about 50 mm, and a boron nitride coating is evenly sprayed on the surface of the stainless steel mold. The coating thickness is controlled at 20 μm, and the mold is placed at 80°C and baked for 2 hours to obtain a boron nitride coated cage-type hollow mold; (3) High softening point KE604 rosin (softening point is 124-134°C) was heated to 150°C in a beaker, and the anti-oxidation master alloy block was immersed in the molten rosin. After holding for 2 s, the anti-oxidation master alloy was quickly lifted up. The surface of the alloy was coated with a thin layer of rosin. The amount of rosin wrapped was about 7.86 g, and the mass ratio of rosin to anti-oxidation master alloy was about 0.02:1. A layer of tin foil is wrapped around the solidified rosin layer, and the thickness of the tin foil is 10 μm. Then, the anti-oxidation master alloy block coated with rosin and tin foil is placed in a boron nitride coating hollow mold. The volume ratio of the anti-oxidation master alloy block to the boron nitride coating hollow mold is about 1:1.3, and a ternary tin-based anti-oxidation master alloy with a core-shell structure is obtained. The ternary tin-based anti-oxidation master alloy with a core-shell structure is further added into a SnCu0.7 alloy melt at 280°C to form about 39.32 kg of anti-oxidation solder, which is kept warm for 1 hour and cast into the mold to obtain the SnCu0.7P0.0032Ga0.016 anti-oxidation solder alloy.
[0017] The SnCu0.7P0.0032Ga0.016 solder prepared by adding a core-shell structured ternary tin-based antioxidant master alloy has excellent antioxidant properties. The P element yield is about 90.62%, the Ga element yield is about 93.12%, and under the condition of oxidation at 300°C for 2 hours, the TG oxidation weight gain is 0.36 mg, the dynamic oxidation slag amount is 3.16 g, and the static and dynamic alloy melt surfaces can maintain a mirror state (see Figure 1 The center of the spherical mirror solder and Figure 8 The surface oxygen content of the oxide layer is only 1.29 wt. %, and the oxygen concentration is reduced to 0.67 wt. % after etching for 300 s. See Table 1 to Table 3 and the attached figure for details. Example 2
[0018] A tin-based antioxidant alloy with a core-shell structure is prepared and added to SnCu0.7 solder as an intermediate alloy to obtain SnCu0.7P0.005Ge0.01 antioxidant solder alloy, and its preparation method and adding steps (1) Under argon protection conditions, a closed melting furnace was used to prepare about 750.96 g of SnP0.5Ge1 anti-oxidation master alloy block, with a mass ratio of P to Ge of 1:2; (2) Design and prepare Fig. 22 The frame-type stainless steel hollow mold shown has an inner side length of about 50 mm, and a boron nitride coating is evenly sprayed on the surface of the stainless steel mold. The coating thickness is controlled at 20 μm, and the mold is placed at 80°C and baked for 2 hours to obtain a boron nitride coated frame-type hollow mold; (3) The high softening point KE604 rosin was heated to 150°C in a beaker, and the anti-oxidation master alloy block was immersed in the molten rosin. After holding for 2 s, the anti-oxidation master alloy was quickly lifted up. The surface of the alloy was coated with a thin layer of rosin. The mass ratio of rosin to anti-oxidation master alloy was about 0.02:1, and the amount of rosin wrapped was about 15.02 g. A layer of tin foil is wrapped around the solidified rosin layer, and the thickness of the tin foil is 10 μm. Then, the anti-oxidation intermediate alloy block coated with rosin and tin foil is placed in a boron nitride coating hollow mold. The volume ratio of the anti-oxidation intermediate alloy block and the boron nitride coating hollow mold is about 1:1.3. A ternary tin-based anti-oxidation intermediate alloy with a core-shell structure is obtained. The ternary tin-based anti-oxidation intermediate alloy with a core-shell structure is further added into a SnCu0.7 alloy melt at 280°C to form about 75.10 kg of anti-oxidation solder. The alloy is kept warm for 1 hour and cast into the mold to obtain the SnCu0.7P0.005Ge0.01 anti-oxidation solder alloy.
[0019] The solder prepared by adding the core-shell structured ternary tin-based antioxidant master alloy has excellent antioxidant properties. The P element recovery rate is about 94%, the Ge element recovery rate is about 92%, and under the condition of oxidation at 300°C for 2 hours, the TG oxidation weight gain is 0.38 mg, the dynamic oxidation slag volume is 2.97 g, and the static and dynamic alloy melt surfaces can maintain a mirror state (see Figure 2 The center of the spherical mirror solder and Fig. 9 The oxygen content on the surface of the oxide layer is only 1.96 wt.%, and the oxygen concentration is reduced to 0.98 wt.% after etching for 300 s. Comparative Example 1
[0020] SnP1 master alloy is prepared and metal Ga is directly added to SnCu0.7 solder to obtain SnCu0.7P0.0032Ga0.016 anti-oxidation solder alloy. The steps are as follows: use a closed melting furnace to melt the SnP1 master alloy, put SnP1 and metal Ga into the SnCu0.7 solder melt at a temperature of 330°C, keep the temperature for 2 hours, stir it, and cast it into a mold to obtain the anti-oxidation solder.
[0021] The oxidation-resistant solder prepared by using SnP1 binary master alloy supplemented with metal Ga addition has a P element recovery rate of only 75%, and a Ga element recovery rate of about 73.75%. Under the condition of oxidation at 300°C for 2 hours, the TG oxidation weight increases by 0.44 mg, and the dynamic oxidation slag amount increases to 8.51 g. A large number of yellow oxide film stripes are distributed on the surface of the static and dynamic alloy melts, respectively. The oxygen content on the surface of the oxide layer is as high as 43.97 wt. %, and the oxygen concentration is still 26.04 wt. % after etching for 300 s. Comparative Example 2
[0022] SnP1 master alloy is prepared and metal Ge is directly added to SnCu0.7 solder to obtain SnCu0.7P0.005Ge0.01 anti-oxidation solder alloy. The steps are as follows: use a closed melting furnace to melt the SnP1 master alloy, put SnP1 and metal Ga into the SnCu0.7 solder melt at a temperature of 400°C, keep the temperature for 2 hours, stir it, and cast it into a mold to obtain the anti-oxidation solder.
[0023] The oxidation-resistant solder prepared by using SnP1 binary master alloy supplemented with metal Ga addition has a P element yield of about 80%, a Ga element yield of about 75%, and under the condition of oxidation at 300°C for 2 hours, the TG oxidation weight increases by 0.45 mg, the dynamic oxidation slag amount increases to 7.27 g, and large gray and yellow oxide film stripes are distributed on the surface of the static and dynamic alloy melts, respectively. The oxygen content on the surface of the oxide layer is as high as 45.37 wt. %, and the oxygen concentration is still 29.64 wt. % after etching for 300 s. Comparative Example 3
[0024] SnP1 master alloy is prepared and directly added to SnCu0.7 solder with SnGa1 to obtain SnCu0.7P0.0032Ga0.016 anti-oxidation solder alloy. The steps are as follows: use a closed melting furnace to melt SnP1 and SnGa1 master alloys, put SnP1 and SnGa1 master alloys into SnCu0.7 solder melt at a temperature of 310°C, keep the temperature for 2 hours, stir it, and cast it into a mold to obtain anti-oxidation solder.
[0025] The oxidation-resistant solder prepared by direct addition of SnP1 and SnGa1 binary intermediates has a P element yield of about 78.12%, a Ga element yield of about 74.38%, and under the condition of oxidation at 300°C for 2 hours, the TG oxidation weight increases by 0.41 mg, the dynamic oxidation slag amount increases to 5.86 g, a small amount of gray oxide film stripes appear on the surface of the static and dynamic alloy melts, and the oxygen content on the surface of the oxide layer increases to 32.73 wt. %, and the oxygen concentration is still 13.83 wt. % after etching for 300 s. Comparative Example 4
[0026] SnP1 master alloy is prepared and directly added to SnCu0.7 solder with SnGe1 to obtain SnCu0.7P0.005Ge0.01 anti-oxidation solder alloy. The steps are as follows: use a closed melting furnace to melt SnP1 and SnGe1 master alloys, put SnP1 and SnGe1 master alloys into SnCu0.7 solder melt at a temperature of 330°C, keep the temperature for 2 hours, stir it, and cast it into a mold to obtain anti-oxidation solder.
[0027] The oxidation-resistant solder prepared by direct addition of SnP1 and SnGa1 binary intermediates has a P element yield of about 88%, a Ga element yield of about 83%, and under the condition of oxidation at 300°C for 2 hours, the TG oxidation weight increases by 0.42 mg, the dynamic oxidation slag amount increases to 4.49 g, a small amount of gray oxide film stripes appear on the surface of the static and dynamic alloy melts, and the oxygen content on the surface of the oxide layer increases to 34.92 wt. %, and the oxygen concentration is still 15.28 wt. % after etching for 300 s.
[0028] Table 1 lists the direct reading spectrum component test results of the solder antioxidant elements of Examples 1-2 and Comparative Examples 1-4. Table 2 lists the static TG oxidation weight gain test results of the solder of Examples 1-2 and Comparative Examples 1-4. Table 3 lists the dynamic oxidation slag test results of the solder of Examples 1-2 and Comparative Examples 1-4.
[0029] Figure 1 to Figure 6 The static oxidation surface pictures of the solder are respectively those of Example 1, Example 2, and Comparative Examples 1 to 4; and those of the static oxidation surface of the solder.
[0030] Figure 7 It is the TG static oxidation weight gain curve of the solder of Example 1, Example 2 and Comparative Examples 1 to Comparative Examples 4.
[0031] Figure 8~Figure 13 The dynamic oxidation surface pictures of the solders of Example 1, Example 2, and Comparative Examples 1 to 4 are shown respectively.
[0032] Fig.14 It is a statistical diagram of the dynamic oxidation slag amount of solder cycle scraping in Example 1, Example 2 and Comparative Examples 1 to Comparative Examples 4; Fig.15 ~ for Fig. 20 The solder oxidation surface etching curves of Example 1, Example 2 and Comparative Examples 1 to 4 are shown.
[0033] Table 1 Test results of direct reading spectrum components of solder antioxidant elements of Examples 1-2 and Comparative Examples 1-4
[0034] Table 2 Static TG oxidation weight gain test results of solders of Examples 1-2 and Comparative Examples 1-4
[0035] Table 3 Test results of dynamic oxidation slag of solder in Examples 1-2 and Comparative Examples 1-4
[0036] From Table 1, Table 2, Table 3 and Figure 1 to Figure 20It can be seen that the method of the present invention can significantly improve the alloy element recovery rate, the antioxidant element recovery rate exceeds 90%, and the static melt surface oxidation resistance is effectively improved. The static oxidation weight gain is as low as 0.36-0.38 mg, and the oxygen content at a depth of 300s from the surface is only 0.67-0.98 wt.%. The dynamic melt surface mirror retention state is greatly improved, and the dynamic oxidation slag amount is reduced. The dynamic melt mirror state retention time after cyclic scraping is more than 2 hours, and the dynamic slag weight gain is only 6.40 wt.%, which comprehensively improves the oxidation resistance of the solder alloy. Figure 1 , Figure 2 and Figure 3~Figure 6 By comparison, it can be clearly seen that the static mirror surface of the solders of Examples 1 and 2 is very bright, while the static mirror surface of the solders of Comparative Examples 1 to 4 is obviously dim and is severely oxidized. Figure 8 , Fig. 9 and Figure 10~Figure 12 By comparison, it can be clearly seen that the dynamic mirror surface of the solder of Examples 1 and 2 is very bright and clearly reflects the image of the handheld camera, while the dynamic mirror surface of the solder of Comparative Examples 1 to 4 is very blurry and seriously oxidized. The preparation method of the present invention can also be used to prepare solder sheets, tin powder, tin balls, tin pastes, and tin bars with anti-oxidation properties.
[0037] The closed smelting furnace described in the present invention is a prior art device and will not be described in detail here.
Claims
1. Preparation method of core-shell structure tin-based antioxidant solder alloy, It is characterized in that An anti-oxidation master alloy block is used as a matrix, a high softening point hydrogenated rosin derivative KE604 is used to coat the anti-oxidation master alloy block, tin foil is wrapped as a secondary outer layer, and a boron nitride hollow mold is coated as an outermost layer to form a core-shell structure of an anti-oxidation master alloy-rosin-tin foil-boron nitride coating hollow mold; the anti-oxidation master alloy block is a SnPGa anti-oxidation master alloy block or a SnPGe anti-oxidation master alloy block, in the SnPGa anti-oxidation master alloy, the mass ratio of P to Ga is 1:5; in the SnPGe anti-oxidation master alloy, the mass ratio of P to Ge is 1:2; the mass ratio of the high softening point rosin to the anti-oxidation master alloy is 0.02:1, and the volume ratio of the anti-oxidation master alloy block to the boron nitride coating hollow mold is 1:1.
3.
2. The method for preparing the core-shell structure tin-based antioxidant solder alloy according to claim 1, It is characterized in that The preparation method comprises the following steps: (1) Under argon protection conditions, an oxygen-resistant master alloy block is prepared in a closed melting furnace; (2) Designing and preparing a cage-type or frame-type stainless steel hollow mold with a cover, spraying a boron nitride coating evenly on the stainless steel surface, and baking the hollow mold at 80°C for 2 hours to obtain a boron nitride coated hollow mold; (3) The high softening point KE604 rosin was heated to 150°C in a beaker, and the antioxidant master alloy block was immersed in the molten rosin. After holding for 2 s, the antioxidant master alloy block was lifted up. The surface of the antioxidant master alloy block was covered with a rosin layer. A layer of tin foil was wrapped around the outer layer of rosin. The lid of the boron nitride coating hollow mold was opened, and the antioxidant master alloy block coated with rosin and tin foil was placed into the boron nitride coating hollow mold and the lid was closed to obtain a core-shell structured multi-component tin-based antioxidant master alloy. The core-shell structured multi-component antioxidant master alloy was then added into a 280°C tin alloy melt and cast into the mold to prepare a tin-based antioxidant solder alloy.
3. The method for preparing the core-shell structure tin-based antioxidant solder alloy according to claim 1, It is characterized in that The cage-type stainless steel hollow mold with a cover is composed of a hollow upper hemisphere and a lower hemisphere.
Citation Information
Patent Citations
Lead-free high-temperature antioxidant solder and preparation method thereof
CN106271187A
Intermediate alloy for improving solder oxidation resistance
CN112322929A
Method for improving oxidation resistance of tin raw material or tin-based solder
CN114833490A
Method for obtaining high-toughness lead-tin-bismuth-free solder through microalloying regulation and control of microstructure
CN115383349A
Solder alloy melt surface oxidation state testing device
CN222439397U