Silicon carbide powder synthesis crucible and silicon carbide powder synthesis method

By using step-like structures and graphite sheets to absorb Si atmosphere in the silicon carbide powder synthesis crucible, the Si atmosphere corrosion problem is solved, the equipment life is extended and the powder purity is improved, and the synthesis of high-purity silicon carbide powder is achieved.

CN119080001AActive Publication Date: 2024-12-06SHANDONG UNIV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411212327.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-12-06
Estimated Expiration
2044-08-30

AI Technical Summary

Technical Problem

During the high-temperature self-propagation method synthesis of silicon carbide powder, the escape of Si atmosphere leads to corrosion of crucible and insulation felt, affecting the equipment life and sealing performance, and the imbalance in the silicon-carbon ratio leads to a decrease in the purity of the powder.

Method used

A silicon carbide powder synthesis crucible is designed, including a step-like structure, a ventilation cylinder, a support cylinder and a graphite sheet. The graphite powder is laid between the ventilation cylinder and the support cylinder. The graphite sheet is located on the top of the support cylinder. In order to absorb the Si atmosphere, the corrosion of the crucible is slowed down, and the molar ratio of Si to C is controlled during the synthesis process to ensure sufficient reaction.

Benefits of technology

It effectively slows down the corrosion of Si atmosphere on crucibles and insulation felts, extends the equipment life, maintains the silicon-carbon ratio balance, and improves the purity and product consistency of silicon carbide powder.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119080001A_ABST
    Figure CN119080001A_ABST
Patent Text Reader

Abstract

The invention discloses a silicon carbide powder synthesis crucible and a silicon carbide powder synthesis method. High-purity graphite powder and high-purity silicon powder are evenly mixed in proportion and then laid at the bottom of the crucible; high-purity graphite powder is laid in a containing cavity defined by the supporting cylinder, the ventilation cylinder and the annular support, and the crucible upper cover covers the containing cavity; putting the crucible into a furnace body, vacuumizing, heating, introducing protective gas, and repeatedly pumping, filling and cleaning; and heating, keeping the temperature for 30-50 hours, introducing protective gas during the period, keeping the temperature in the furnace at 2000-2600 DEG C and the pressure at 50-800 mbar, and synthesizing to obtain the silicon carbide powder. The additional graphite powder is placed on the upper portion of the crucible, the Si atmosphere escaping from the powder in the synthesis process preferentially reacts with the graphite powder placed on the outer side of the ventilation cylinder, additional silicon carbide powder is generated, the utilization efficiency of raw materials is improved, and the cost of the raw materials is reduced. In addition, the escaped Si atmosphere preferentially reacts with the graphite powder placed on the outer side of the ventilation cylinder, so that the corrosion possibility of the crucible and the heat preservation felt is reduced, and the estimated service life of the crucible and the heat preservation felt can be remarkably prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the synthesis of silicon carbide powder, in particular to a silicon carbide powder synthesis crucible and a method for synthesizing the silicon carbide powder. Background Art

[0002] The statements herein merely provide background information related to the present invention and do not necessarily constitute prior art.

[0003] As a typical representative of the third generation wide bandgap semiconductor materials, silicon carbide (SiC) has excellent characteristics such as wide bandgap, high electron saturation drift velocity, high critical breakdown voltage, high thermal conductivity and high temperature resistance. Based on the above characteristics, silicon carbide has irreplaceable advantages in electronic application fields such as high temperature, high pressure, high frequency, high power, optoelectronics, radiation resistance, microwave, as well as in extreme environments such as aerospace, military industry, and nuclear energy.

[0004] At present, the high-temperature self-propagating method is the mainstream method for synthesizing silicon carbide powder. The specific process is as follows: high-purity graphite powder and high-purity silicon powder are mixed evenly and placed in a crucible, and heated under the protection of inert gas. When the temperature rises to the melting point of Si, C begins to dissolve in the Si liquid, increasing the ignition contact area and the diffusion rate. When the temperature rises to the ignition temperature, Si and C react exothermically instantly and ignite the surrounding reactants layer by layer, causing more Si to melt, C to continue to dissolve, and the reaction continues, thereby synthesizing silicon carbide powder.

[0005] During the synthesis of silicon carbide powder, as the temperature rises, Si in the mixed powder begins to escape in the form of gas phase, which will cause the following effects: (1) Crucible corrosion and crystallization: The escaping Si atmosphere will seriously corrode the crucible cover and the crucible body. At high temperatures, the Si atmosphere reacts with the crucible material to form atmosphere crystals. These crystalline substances not only adhere to the upper inner wall and upper cover of the crucible, but also cause the crucible cover and the crucible body to stick together, making it impossible to open normally. Long-term corrosion and crystallization will cause cracks in the crucible cover and the upper part of the crucible body, seriously affecting the sealing performance and mechanical strength of the crucible, and ultimately significantly reducing the service life of the crucible. (2) Corrosion and damage of the insulation felt: The Si atmosphere escaping from the outside of the crucible will also corrode the insulation felt. This corrosion will cause structural damage to the insulation felt, thereby reducing its insulation performance and service life. Damage to the insulation felt will increase energy loss, reduce process efficiency, and increase the cost of equipment maintenance and replacement. (3) Imbalance in silicon-carbon ratio and decreased purity of silicon carbide powder: The escape of Si atmosphere will destroy the silicon-carbon ratio balance in the reaction system, reduce the amount of Si in the actual reaction, and leave residual carbon in the prepared silicon carbide product, which will reduce the purity of the final silicon carbide powder and make it difficult to meet the requirements.

[0006] Chinese patent CN109336114B discloses a method for improving the synthesis efficiency of high-purity silicon carbide powder, which includes pretreatment, introduction of mixed gas for high-temperature self-propagating reaction, and cooling to room temperature under the protection of mixed gas. The method is characterized in that the introduction of high-purity silane can effectively inhibit the carbonization of powder caused by the imbalance of carbon-silicon ratio during the synthesis process, thereby improving the quality and synthesis efficiency of silicon carbide powder. However, the introduction of high-purity silane will cause excessive Si atmosphere inside the crucible, aggravating the corrosion of the inner wall of the crucible, and significantly reducing the service life of the crucible.

[0007] Chinese patent CN115520871A discloses a method for synthesizing high-purity silicon carbide powder, the main steps of which are: (1) Batching: Use high-purity silicon powder and graphite powder and mix them in a specific molar ratio. (2) Mixing: Use a three-dimensional motion mixer to mix for 1-24 hours. (3) Crucible pretreatment: Heat the graphite crucible to 1873-2400°C and introduce argon. (4) Synthesis: It is carried out in four stages, including vacuuming, heating, insulation and cooling processes. (5) Post-treatment: ball milling, cleaning and screening. However, the inlaid connection between the crucible cover and the crucible body may not be sufficient to completely seal. Under high temperature conditions, the Si atmosphere escaping from the powder will crystallize with the crucible cover and the crucible body, and the Si atmosphere escaping from the outside of the crucible will corrode the insulation felt, affecting the life of the crucible and the insulation felt.

[0008] The above-disclosed patents all use a high-temperature self-propagating method to synthesize silicon carbide powder. During the high-temperature synthesis process, Si atmosphere will escape, causing severe corrosion of the crucible and insulation felt, affecting the service life and sealing performance of the overall structure, increasing maintenance and replacement costs, and also destroying the silicon-carbon ratio balance in the reaction system, causing the purity of the synthesized silicon carbide to decrease. Summary of the invention

[0009] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a silicon carbide powder synthesis crucible and a method for synthesizing silicon carbide powder. By using the crucible and the synthesis method, high-purity silicon carbide powder can be obtained, and the problem that the crucible is easily corroded by Si atmosphere in the prior art is effectively solved, greatly improving the service life of the crucible and the heat preservation.

[0010] In order to achieve the above object, the present invention is implemented through the following technical solutions:

[0011] In a first aspect, the present invention provides a silicon carbide powder synthesis crucible, comprising a crucible body, a crucible cover, a vent cylinder, a support cylinder and a graphite sheet, wherein:

[0012] The crucible upper cover is used to cover the crucible body;

[0013] The upper part of the inner wall of the crucible body is provided with a step-like structure;

[0014] The ventilation cylinder is installed on the step-shaped structure through an annular support, and the diameter of the ventilation cylinder is smaller than the diameter of the crucible body;

[0015] The outer diameter of the supporting cylinder is smaller than the inner diameter of the crucible body, and the supporting cylinder is mounted on the annular support of the ventilation cylinder, and the height of the supporting cylinder is higher than the height of the ventilation cylinder; a graphite powder containing chamber is formed between the supporting cylinder, the ventilation cylinder and the annular support;

[0016] The graphite sheet is placed on the top of the supporting cylinder and is located between the supporting cylinder and the upper cover of the crucible.

[0017] Since graphite powder has a large specific surface area, carbon atoms can contact silicon atoms more fully. Placing graphite powder between the ventilation cylinder and the support cylinder can make the Si atmosphere escaping from the mixed powder react with the graphite powder first, slowing down the corrosion of the Si component on the graphite sheet or the crucible cover.

[0018] In some embodiments, the crucible cover and the crucible body are made of isostatic graphite and are connected by threads or screws.

[0019] In some embodiments, the graphite sheet is made of isostatic graphite. The presence of the graphite sheet can not only further block the Si atmosphere that has not reacted with the graphite powder, but also effectively prevent the Si atmosphere from reacting with the connection between the crucible cover and the crucible body, thereby reducing corrosion to the crucible and extending the life of the crucible.

[0020] In some embodiments, the support cylinder, the vent cylinder and the annular support are made of tantalum carbide or are plated with tantalum on their surfaces, which can significantly reduce the reaction between the Si atmosphere and the support cylinder and extend the life of the components.

[0021] In some embodiments, the support cylinder has a height of 40-60 mm and a thickness of 10-15 mm.

[0022] Preferably, the support cylinder is 5-15 mm higher than the ventilation cylinder, so that the graphite powder can react with the escaped Si atmosphere.

[0023] In some embodiments, the crucible body has a diameter of 350-400 mm and a wall thickness of 15-30 mm.

[0024] In a second aspect, the present invention provides a method for synthesizing silicon carbide powder, comprising the following steps:

[0025] Using the silicon carbide powder synthesis crucible for synthesis;

[0026] Mix high-purity graphite powder and high-purity silicon powder in proportion and spread them on the bottom of the crucible;

[0027] High-purity graphite powder is laid in a containing chamber formed between the supporting cylinder, the ventilation cylinder and the annular support, and the crucible is covered with an upper cover;

[0028] Place the crucible in the furnace, evacuate it, heat it to 800-1000℃, introduce protective gas, and repeatedly pump and clean it;

[0029] The temperature is continued to be raised to 2000-2600°C and kept at this temperature for 30-50 hours. During this period, protective gas is introduced to maintain the pressure in the furnace at 50-800 mbar to synthesize silicon carbide powder.

[0030] The purpose of repeated pumping and cleaning is to fully remove the nitrogen element inside the crucible.

[0031] In some embodiments, the atomic molar ratio of high-purity graphite powder to high-purity silicon powder is 1:1.05-1.30. As the temperature increases, Si in the mixed powder begins to escape in the form of gas phase, so the molar ratio of Si to C in the gas phase component inside the crucible is greater than 1 to ensure that there is still enough Si to react with C at high temperature. In addition, the purity of graphite powder and silicon powder is high purity (5N, more than 99.999%), which can improve the purity of the synthesized silicon carbide powder.

[0032] In some embodiments, after the synthesis is completed, the temperature is lowered to room temperature, protective gas is introduced, and the pressure in the furnace is raised to 800-1000 mbar.

[0033] In some embodiments, the crucible is placed in the furnace and the vacuum is drawn for 8-10 hours with a vacuum value of 5×10 -5 ~10 -6 mbar.

[0034] In some embodiments, the method of repeated pumping and filling cleaning is: introducing protective gas to make the pressure in the furnace 200-500 mbar, maintaining the time for 0.5-1h, and then evacuating to less than 5×10 -5 mbar, maintain for 1-2h, and repeat this process 3-5 times.

[0035] In some embodiments, high-purity graphite powder is laid in the containing chamber surrounded by the supporting cylinder, the ventilation cylinder and the annular support, and the mass of the laid high-purity graphite powder is 5%-30% of the high-purity graphite powder in the bottom carbon-silicon mixed powder material, so as to ensure that the graphite powder here fully reacts with the Si atmosphere escaping from the bottom of the crucible, thereby improving the utilization rate of raw materials.

[0036] Preferably, high-purity graphite powder is laid in the containing chamber enclosed by the supporting cylinder, the ventilation cylinder and the annular support, and the molar ratio of the laid high-purity graphite powder to excess high-purity silicon powder in the bottom carbon-silicon mixed powder (high-purity silicon powder other than the high-purity silicon powder with a silicon-carbon ratio greater than 1 in the mixed powder) is 0.8-1:1.

[0037] In some embodiments, the protective gas is Ar, H2, He or a mixed gas of Ar / H2 or He / H2; when a mixed gas is used, the volume proportion of H2 is less than 20%.

[0038] In some embodiments, the crucible, insulation felt, etc. are pretreated when used for the first time, the pretreatment temperature is 2200-2600°C, the pretreatment chamber pressure is 1-30mbar, and the pretreatment time is 20-40h, so as to remove the adsorbed nitrogen and impurity elements on the surface, thereby improving the purity of the silicon carbide powder.

[0039] The beneficial effects achieved by one or more embodiments of the present invention are as follows:

[0040] 1. The assembly structure of the ventilation cylinder, the support cylinder and the graphite sheet of the present invention reduces the corrosion of the inner wall of the crucible by the Si atmosphere, and significantly prolongs the service life of the crucible. In addition, the structure reduces the situation where the Si atmosphere escapes into the insulation felt, thereby reducing the corrosion of the insulation felt and increasing its use times. The extension of the life of the crucible and the insulation felt directly reduces the production cost.

[0041] 2. In the process of synthesizing silicon carbide, the present invention adds a slightly excessive amount of silicon to enrich the raw material with silicon. The crucible of the present invention effectively reduces the escape of Si atmosphere, maintains the silicon-carbon ratio balance of the raw material, is conducive to obtaining silicon carbide powder with higher purity, and is more suitable for growing high-quality SiC single crystals; the remaining silicon at the end of the reaction can be sublimated from the silicon carbide to the top of the crucible by heating, and reacts with the graphite powder above to ensure that the synthesized SiC powder does not contain phases such as silicon and carbon, thereby effectively improving the quality of silicon carbide and product consistency.

[0042] 3. In the present invention, additional graphite powder is placed on the upper part of the crucible to fully utilize the characteristics of large specific surface area and high activity of graphite powder. During the synthesis process, the Si atmosphere escaping from the powder reacts preferentially with the graphite powder placed on the outer side of the ventilation cylinder to generate additional silicon carbide powder, which can produce 5% to 30% more SiC powder, thereby improving the utilization efficiency of raw materials and reducing the cost of raw materials; the graphite powder reacts with the excess Si atmosphere in the crucible to reduce the Si component leaking into the insulation layer through the crucible, reduce the corrosion of the crucible and its insulation layer by the Si component, and extend the life of the crucible; since the insulation performance is not affected, energy consumption is also saved to a certain extent.

[0043] 4. The crucible of the present invention has a simple structure, is convenient for taking out materials, is easy to operate and maintain, and is suitable for mass production of silicon carbide powder. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.

[0045] Figure 1 A schematic diagram of the structure of a crucible in an embodiment of the present invention;

[0046] Figure 2 It is an assembly cross-sectional view of the supporting cylinder, the venting cylinder and the graphite sheet in an embodiment of the present invention;

[0047] Figure 3 is a cross-sectional view of a crucible body in an embodiment of the present invention;

[0048] Figure 4 is the Raman spectrum of the silicon carbide powder synthesized in the embodiment of the present invention;

[0049] In the figure, 1-graphite powder; 2-crucible cover; 3-graphite sheet; 4-support cylinder; 5-ventilation cylinder; 6-crucible body; 7-mixed powder. DETAILED DESCRIPTION

[0050] It should be noted that the following detailed descriptions are illustrative and intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used in the present invention have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.

[0051] The present invention will be further described below in conjunction with the embodiments.

[0052] Example 1

[0053] like Figure 1 As shown, the crucible is composed of a crucible cover 2, a graphite sheet 3, a supporting cylinder 4, a vent cylinder 5, and a crucible body 6. The crucible cover is used to cover the crucible body.

[0054] The upper part of the inner wall of the crucible body 6 is provided with a step-like structure;

[0055] The ventilation cylinder 5 is installed on the step-shaped structure through an annular support, and the outer diameter of the ventilation cylinder 5 is smaller than the inner diameter of the crucible body 6;

[0056] The outer diameter of the support cylinder 4 is smaller than the inner diameter of the crucible body 6. The support cylinder 4 is mounted on the annular support of the ventilation cylinder 5. The height of the support cylinder 4 is higher than the height of the ventilation cylinder 5. A graphite powder containing chamber is formed between the support cylinder 4 and the ventilation cylinder 5.

[0057] The graphite sheet 3 is placed on the top of the supporting cylinder 4 and is located between the supporting cylinder 4 and the crucible upper cover 2 .

[0058] Mixed powder 7 is placed at the bottom of the crucible body 6, and graphite powder 1 is placed outside the vent cylinder. In addition, the crucible cover 2 is connected to the crucible body 6 by threads, screws, etc., and the vent cylinder is directly buckled on the step-shaped structure of the crucible body through an annular support.

[0059] like Figure 2 As shown, the graphite sheet 3, the supporting cylinder 4 and the ventilation cylinder 5 are assembled, wherein the inner diameter of the ventilation cylinder 5 is 60-80 mm, the height is 30-50 mm, and the height of the supporting cylinder 4 is 40-60 mm, and the thickness is 10-15 mm. Graphite powder 1 is placed in the space between the ventilation cylinder 5 and the supporting cylinder 4, which can react with the Si atmosphere.

[0060] like Figure 3 As shown, the crucible body 6 has a diameter of 350-400 mm and a wall thickness of 15-30 mm. There is a step-like structure at the top with a step width of 10-15 mm, which is convenient for placing the ventilation cylinder 5. The height of the step-like structure is not higher than 1 / 4 of the total height of the crucible.

[0061] When used for the first time, the crucible and the insulation felt structure are placed in a synthesis furnace for high-temperature pretreatment. The heating temperature is 2200-2600°C, the pretreatment chamber pressure is 1-30mbar, and the insulation time is 20-40h.

[0062] The crucible upper cover 2 and the crucible body 6 are made of isostatic graphite and are connected by threads or screws.

[0063] The support cylinder 4, the ventilation cylinder 5 and the annular support are made of tantalum carbide or are plated with tantalum on their surfaces.

[0064] Example 2

[0065] The synthesis method of silicon carbide powder comprises the following steps:

[0066] (1) High-purity graphite powder and high-purity silicon powder are mixed evenly in a molar ratio of 1:1.05 and placed at the bottom of a graphite crucible, and high-purity graphite powder with a mass of 5% of the high-purity graphite powder in the bottom mixed powder is spread on the outside of the ventilation cylinder.

[0067] (2) Place the assembled graphite crucible into the synthesis furnace and perform vacuum treatment for 8 hours until the vacuum value in the furnace is less than 5×10 -5 mbar.

[0068] (3) The crucible was heated to 800°C, the pressure in the furnace was maintained at 200 mbar for 0.5 h, and then vacuumed to less than 5 × 10 -5 mbar, and maintain for 1 h. This process was repeated 3 times to remove the nitrogen inside the crucible.

[0069] (4) After the pumping and cleaning process is completed, the temperature is raised to 2200°C and kept at this temperature for 50 hours. Protective gas is introduced and the pressure in the furnace is maintained at 50 mbar.

[0070] (5) After the synthesis is completed, the temperature is slowly lowered to room temperature, and the protective gas is continuously introduced to raise the pressure in the furnace to 1000 mbar to obtain the desired high-purity silicon carbide powder.

[0071] Powder X-ray diffractometer, Raman spectrometer and other tests are used, such as Figure 4 As shown, the powder contains only SiC and no impurities such as Si and C. Since the crucible and the insulation felt are not corroded, it is estimated that the service life of the crucible and the insulation felt can reach twice that of an ordinary crucible.

[0072] Example 3

[0073] The synthesis method of silicon carbide powder comprises the following steps:

[0074] (1) High-purity graphite powder and high-purity silicon powder are mixed evenly in a molar ratio of 1:1.15 and placed at the bottom of a crucible. The mass of high-purity graphite powder placed outside the vent cylinder is 15% of the high-purity graphite powder in the bottom mixed powder.

[0075] (2) Place the assembled graphite crucible into the synthesis furnace and evacuate it for 8 hours until the vacuum value in the furnace is less than 5×10 -5 mbar.

[0076] (3) The crucible was heated to 900°C, the pressure in the furnace was maintained at 300 mbar for 0.5 h, and then vacuumed to less than 5 × 10 -5 mbar, and maintain for 1.5 h. This process was repeated 4 times to remove the nitrogen inside the crucible.

[0077] (4) After the pumping and cleaning process is completed, the temperature is raised to 2400°C and kept at this temperature for 40 hours. Protective gas is introduced and the pressure in the furnace is maintained at 300 mbar.

[0078] (5) After the synthesis is completed, the temperature is slowly lowered to room temperature, and the protective gas is continuously introduced to raise the pressure in the furnace to 1000 mbar to obtain the desired high-purity silicon carbide powder.

[0079] The powder X-ray diffractometer, Raman spectrometer and other tests show that the powder contains only SiC and no impurities such as Si and C. It is estimated that the service life of the crucible and insulation felt can reach 2.5 times that of ordinary crucibles.

[0080] Example 4

[0081] The synthesis method of silicon carbide powder comprises the following steps:

[0082] (1) High-purity graphite powder and high-purity silicon powder are mixed evenly in a molar ratio of 1:1.3 and placed at the bottom of the crucible. The mass of the high-purity graphite powder placed outside the ventilation cylinder is 30% of the high-purity graphite powder in the bottom mixed powder.

[0083] (2) Place the assembled graphite crucible into the synthesis furnace and perform vacuum treatment for 9 hours until the vacuum value in the furnace is less than 5×10 -6 mbar.

[0084] (3) The crucible was heated to 1000°C, the pressure in the furnace was maintained at 500 mbar for 0.5 h, and then vacuumed to less than 5 × 10 -5 mbar, and maintain for 1.5 h. This process was repeated 5 times to remove the nitrogen inside the crucible.

[0085] (4) After the pumping and cleaning process is completed, the temperature is raised to 2600°C and kept at this temperature for 30 hours. Protective gas is introduced and the pressure in the furnace is maintained at 800 mbar.

[0086] (5) After the synthesis is completed, the temperature is slowly lowered to room temperature, and the protective gas is continuously introduced to raise the pressure in the furnace to 900 mbar to obtain high-purity silicon carbide powder.

[0087] The powder X-ray diffractometer, Raman spectrometer and other tests show that the powder contains only SiC and no impurities such as Si and C. It is estimated that the service life of the crucible and insulation felt can reach 2.5 times that of ordinary crucibles.

[0088] Comparative Example 1

[0089] Compared with Example 2, the crucible structure of Comparative Example 1 is different. In Comparative Example 1, there is no ventilation cylinder and no high-purity graphite powder is additionally placed on the upper part of the crucible.

[0090] The synthesized SiC powder was tested and characterized, and the test results of powder X-ray diffractometer and Raman spectrometer both found characteristic peaks of carbon, indicating that there are still C impurities in the powder and the powder purity is low.

[0091] At the same time, it was found that the upper part of the crucible was severely corroded, corrosion pits of Si components could be clearly seen on the crucible wall, and SiC powder remained in the insulation felt. This shows that during the synthesis of the powder in Comparative Example 1, the excess Si component corroded the crucible and leaked into the insulation, resulting in a certain degree of carbonization of the powder, which reduced the amount of available powder, and affected the life of the crucible and insulation.

[0092] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A silicon carbide powder synthesis crucible, Features: It includes a crucible body, a crucible cover, a vent cylinder, a support cylinder and a graphite sheet, wherein: The crucible upper cover is used to cover the crucible body; The upper part of the inner wall of the crucible body is provided with a step-like structure; The ventilation cylinder is installed on the step-shaped structure through an annular support, and the diameter of the ventilation cylinder is smaller than the diameter of the crucible body; The outer diameter of the supporting cylinder is smaller than the inner diameter of the crucible body. The supporting cylinder is mounted on the annular support of the ventilation cylinder. The height of the supporting cylinder is higher than the height of the ventilation cylinder. A graphite powder containing chamber is formed between the supporting cylinder, the ventilation cylinder and the annular support. The graphite sheet is placed on the top of the supporting cylinder and is located between the supporting cylinder and the upper cover of the crucible.

2. The silicon carbide powder synthesis crucible according to claim 1, Features: The material of the crucible cover and the crucible body is isostatic graphite, and the two are connected by threads or screws; Preferably, the graphite sheet is made of isostatically pressed graphite.

3. The silicon carbide powder synthesis crucible according to claim 1, Features: The support cylinder, the vent cylinder and the annular support are made of tantalum carbide or are tantalum-plated on the surface thereof.

4. The silicon carbide powder synthesis crucible according to claim 1, Features: The support cylinder has a height of 40-60 mm and a thickness of 10-15 mm; Preferably, the support cylinder is 5-15 mm higher than the ventilation cylinder.

5. The silicon carbide powder synthesis crucible according to claim 1, Features: The diameter of the crucible body is 350-400 mm and the wall thickness is 15-30 mm.

6. A method for synthesizing silicon carbide powder, Features: The steps include: The synthesis is carried out using the silicon carbide powder synthesis crucible according to any one of claims 1 to 5; Mix high-purity graphite powder and high-purity silicon powder in proportion and spread them on the bottom of the crucible; High-purity graphite powder is laid in a containing chamber formed between the supporting cylinder, the ventilation cylinder and the annular support, and the crucible is covered with an upper cover; Place the crucible in the furnace, evacuate it, heat it to 800-1000℃, introduce protective gas, and repeatedly pump and clean it; Then the temperature is raised to 2000-2600°C and kept at this temperature for 30-50 hours, during which time a protective gas is introduced and the pressure in the furnace is maintained at 50-800 mbar to synthesize silicon carbide powder.

7. The method for synthesizing silicon carbide powder according to claim 6, Features: The atomic molar ratio of high-purity graphite powder to high-purity silicon powder is 1:1.05-1.

3.

8. The method for synthesizing silicon carbide powder according to claim 6, Features: After the synthesis is completed, the temperature is lowered to room temperature, protective gas is introduced, and the pressure in the furnace is raised to 800-1000mbar.

9. The method for synthesizing silicon carbide powder according to claim 6, Features: The method of repeated pumping and filling cleaning is: introduce protective gas to make the pressure in the furnace 200-500mbar, maintain it for 0.5-1h, and then evacuate it to less than 5×10 - 5 mbar, maintain for 1-2h, repeat this process 3-5 times; Preferably, the mass of the high-purity graphite powder laid in the containing chamber surrounded by the supporting cylinder, the ventilation cylinder and the annular support is 5%-30% of the high-purity graphite powder in the bottom carbon-silicon mixed powder; Preferably, high-purity graphite powder is laid in the containing chamber surrounded by the support cylinder, the ventilation cylinder and the annular support, and the molar ratio of the laid high-purity graphite powder to the excess high-purity silicon powder in the bottom carbon-silicon mixed powder is 0.8-1:

1.

10. The method for synthesizing silicon carbide powder according to claim 6, Features: The protective gas is Ar, H 2 ,He or Ar / H 2 、He / H 2 Mixed gas; When using mixed gas, H 2 The volume share is less than 20%; Preferably, the crucible and the insulation felt structure are pretreated when used for the first time, the pretreatment temperature is 2200-2600° C., the pretreatment chamber pressure is 1-30 mbar, and the pretreatment time is 20-40 hours.

Citation Information

Patent Citations

  • Method for synthesizing homogeneous nano silicon carbide powder by burning

    CN101125653A

  • Granular polycrystalline silicon granulate and production thereof

    CN103373730A

  • Flow guide cylinder for monocrystal silicon growth furnace and application thereof

    CN105239150A

  • Protective special-shaped graphite crucible

    CN214422782U

  • Method for manufacturing fine-grained silicon monoxide

    US5096685A