Iron-containing small-grain ZSM-5 molecular sieve as well as preparation method and application thereof
By introducing peroxide into hydrothermal reaction, the synthesis of ZSM-5 molecular sieve with iron-containing small crystals was solved, and the problem of metal packaging in silicon-aluminum MFI molecular sieve was achieved, effective metal packaging in alkaline environments was improved, and catalytic performance was improved. Low carbon olefin yield.
Patent Information
- Application Number
- CN202310640156.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-31
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2043-05-31
AI Technical Summary
The prior art is difficult to effectively encapsulate metals in silicon-aluminum MFI molecular sieves, especially in alkaline environments. Metals are prone to form hydroxide precipitation and interact with phosphorus, resulting in the problems of high synthesis and low activity.
By using the template agent method, ZSM-5 molecular sieve with small iron-containing grains is synthesized in hydrothermal reaction by introducing peroxides, free radical initiators are used to promote metal encapsulation into the molecular sieve, and the distribution of iron active components on the molecular sieve framework is controlled. Avoid free iron ions and ferrous ions to improve catalytic performance.
The prepared iron-containing small-grain ZSM-5 molecular sieve has a small grain size and excellent catalytic properties, which improves the yield of low-carbon olefins and the conversion of saturated hydrocarbons in the catalytic cracking reaction of light hydrocarbons.
Smart Images

Figure CN119080020A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to a ZSM-5 molecular sieve containing small iron crystals and a preparation method and application thereof. Background Art
[0002] Catalytic cracking refers to the process of converting hydrocarbons into low-carbon olefins such as ethylene, propylene and butene under the action of a catalyst, and producing light aromatics at the same time. The process of producing low-carbon olefins by catalytic cracking of heavy oil has always occupied a large share of the low-carbon olefin market due to its strong raw material adaptability and low production cost. Since the mid-1980s, Sinopec Research Institute of Petroleum and Chemical Industry (Sinopec Research Institute) has been tracking and studying this technology. In 1994, the Research Institute of Petroleum and Chemical Industry developed a catalytic cracking (DCC) process for producing low-carbon olefins using heavy oil (vacuum distillate oil, coking gas oil and residual oil, etc.) as raw materials. After the successful industrialization of DCC technology, the Research Institute of Petroleum and Chemical Industry developed a catalytic thermal cracking (CPP) process for directly producing ethylene and propylene from heavy oil, which has multiple production schemes such as maximum ethylene, maximum propylene and simultaneous production of ethylene and propylene. Compared with the steam cracking process, the CPP process broadens the source of ethylene raw materials and reduces the cost of ethylene raw materials. At the same time, the reaction temperature is lower than that of the steam cracking process, so the energy consumption of the device is significantly reduced. Light oil catalytic cracking mainly refers to the process of producing ethylene and propylene from light gasoline or naphtha in the presence of a catalyst. This process can realize the transformation of petroleum resources into basic chemical raw materials and will play an important role in future chemical refineries.
[0003] The metal component can be introduced into the molecular sieve by encapsulation. This method can not only make the metal component uniformly dispersed in the molecular sieve, but also use the shape selectivity of the molecular sieve for selective dehydrogenation, thereby reducing the methane content and increasing the selectivity of light olefins. Some studies have used ethylenediamine as a ligand to directly synthesize MFI molecular sieves encapsulating metal Pd, realizing the direct synthesis of high-silicon molecular sieves encapsulating metals. The characterization results show that the metal Pd particles after hydrogen reduction are about 1.5nm and are distributed at the intersection of two sets of ten-membered ring channels of the MFI molecular sieve. However, there are currently many studies on encapsulating metals into all-silicon or high-silicon MFI molecular sieves, but there are relatively few studies on encapsulating metals into silicon-aluminum MFI molecular sieves, because if the metal is directly introduced into the synthesis system, it is easy for the metal to form hydroxide precipitation in an alkaline environment. In addition, the metal easily interacts with phosphorus, resulting in difficult synthesis or low activity. Summary of the invention
[0004] The purpose of the present disclosure is to provide a ZSM-5 molecular sieve containing small iron crystals and a preparation method and application thereof. The method of the present disclosure can prepare a ZSM-5 molecular sieve containing small iron crystals with a smaller molecular sieve grain size, which can be used for catalytic cracking reactions of light hydrocarbons and has a better yield of light olefins.
[0005] In order to achieve the above object, the present disclosure provides a method for preparing a ZSM-5 molecular sieve containing small iron crystals in a first aspect, the method comprising:
[0006] S1, mixing a silicon source, an aluminum source, an alkali source, a seed crystal, a template and water to obtain a first mixture;
[0007] S2, mixing the iron source, peroxide, water and the first mixture and performing a hydrothermal reaction;
[0008] Wherein, the peroxide is selected from one or more of sodium persulfate, hydrogen peroxide and Fenton's reagent.
[0009] Optionally, step S2 includes:
[0010] SS1. Mixing the iron source, peroxide and water to obtain a second mixture; the molar ratio of the iron source, peroxide and water in terms of Fe2O3 is 1:(0.2-2.5):(100-1500); preferably 1:(0.2-2):(500-800);
[0011] SS2. The first mixture and the second mixture are mixed and then subjected to the hydrothermal reaction; the molar ratio of the first mixture calculated as Al2O3 to the second mixture calculated as Fe2O3 is 1:(0.01-2.5), preferably 1:(0.4-1.8).
[0012] Optionally, in step S1, the molar ratio of the silicon source calculated as SiO2, the aluminum source calculated as Al2O3, the alkali source calculated as alkali metal oxide, the template and the water is (20-300):1:(1-10):(1-30):(400-2500), preferably (30-100):1:(2-8):(2-10):(500-1200);
[0013] Calculated as SiO2, the amount of the seed crystal used is 3-12 wt%, preferably 8-10 wt%, relative to the total weight of the silicon source.
[0014] Optionally, in step S2, the conditions of the hydrothermal reaction include: temperature of 150-220° C., and time of 8-32 h.
[0015] Optionally, the method further comprises: subjecting the solid product obtained by the hydrothermal treatment to ammonium exchange and calcination treatment; the conditions of the calcination treatment comprise: a temperature of 400-800° C., a time of 0.5-8 h, and an atmosphere of air or water vapor.
[0016] Optionally, the silicon source includes one or more of silica gel, silicon dioxide, white carbon black and silicate;
[0017] The aluminum source includes one or more of sodium metaaluminate, SB powder, aluminum alcoholate, aluminum oxide, aluminum hydroxide and aluminum sulfate;
[0018] The alkali source includes sodium hydroxide and / or potassium hydroxide;
[0019] The seed crystals include one or more ZSM-5 molecular sieves with a silicon-aluminum ratio of 20-50, and the average particle size of the ZSM-5 molecular sieve is 0.5-2 μm;
[0020] The iron source is selected from one or more of ferric nitrate, ferric oxalate, ferric sulfate and ferric hydroxide;
[0021] The template agent includes an organic nitrogen-containing template agent, preferably one or more of n-butylamine, tetrapropylammonium hydroxide and tetrapropylammonium bromide.
[0022] The second aspect of the present disclosure provides a ZSM-5 molecular sieve containing small iron crystals prepared by the method provided in the first aspect of the present disclosure.
[0023] Optionally, the ZSM-5 molecular sieve containing small iron crystals has a structure in which an iron active component is encapsulated inside the ZSM-5 molecular sieve;
[0024] The iron active component is distributed on the framework of the ZSM-5 molecular sieve, and the grain size of the iron-containing small-grain ZSM-5 molecular sieve is 0.5-1 μm.
[0025] Optionally, the specific surface area of the ZSM-5 molecular sieve containing small iron crystals is 240-550 m 2 / g, with a total pore volume of 0.150-0.28 cm 3 ·g -1 , the micropore volume is 0.140-0.20cm 3 ·g -1 , the mesopore volume is 0.010-0.120cm 3 ·g -1 , relative crystallinity is 82-100%;
[0026] In the ZSM-5 molecular sieve containing small iron crystals, the molar ratio of SiO2 to Al2O3 is 20-300;
[0027] Relative to the total weight of the ZSM-5 molecular sieve containing small iron crystals, the content of the iron active component calculated as Fe2O3 is 0.8-1.5 wt%.
[0028] The third aspect of the present disclosure provides an application of the iron-containing small-grain ZSM-5 molecular sieve provided by the second aspect of the present invention in a catalytic cracking reaction of light hydrocarbons.
[0029] Optionally, the conditions for the catalytic cracking reaction include: a temperature of 500-680°C, a reaction mass space velocity of 20-40h -1 , the reaction pressure is 0.8-1.2MPa, and the agent-oil weight ratio is 1-2.
[0030] Through the above technical scheme, the method disclosed in the present invention synthesizes ZSM-5 molecular sieve containing small iron crystals by introducing peroxide into the template system. The prepared molecular sieve has a small crystal size and is used for catalytic cracking reactions of light hydrocarbons with a better yield of low-carbon olefins.
[0031] Other features and advantages of the present disclosure will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] The accompanying drawings are used to provide a further understanding of the present disclosure and constitute a part of the specification. Together with the following specific embodiments, they are used to explain the present disclosure but do not constitute a limitation of the present disclosure. In the accompanying drawings:
[0033] Figure 1 is an X-ray diffraction spectrum of the iron-containing small-grain ZSM-5 molecular sieve A prepared in Example 1 of the present disclosure;
[0034] Figure 2 is a scanning electron microscope photograph of the iron-containing small-grain ZSM-5 molecular sieve A prepared in Example 1 of the present disclosure;
[0035] Figure 3 is a transmission electron microscope photograph of the iron-containing small-grain ZSM-5 molecular sieve A prepared in Example 1 of the present disclosure;
[0036] Figure 4 This is a mapping photo of the iron-containing small-grain ZSM-5 molecular sieve A prepared in Example 1 of the present disclosure;
[0037] Figure 5 is an X-ray diffraction spectrum of the iron-containing small-grain ZSM-5 molecular sieve B prepared in Example 2 of the present disclosure;
[0038] Figure 6 This is a scanning electron microscope photograph of the iron-containing small-grain ZSM-5 molecular sieve B prepared in Example 2 of the present disclosure. DETAILED DESCRIPTION
[0039] The specific implementation of the present disclosure is described in detail below in conjunction with the accompanying drawings. It should be understood that the specific implementation described herein is only used to illustrate and explain the present disclosure, and is not used to limit the present disclosure.
[0040] The first aspect of the present disclosure provides a method for preparing a ZSM-5 molecular sieve containing small iron crystals, the method comprising:
[0041] S1, mixing a silicon source, an aluminum source, an alkali source, a seed crystal, a template and water to obtain a first mixture;
[0042] S2, mixing the iron source, peroxide, water and the first mixture and performing a hydrothermal reaction;
[0043] Wherein, the peroxide is selected from one or more of sodium persulfate, hydrogen peroxide and Fenton's reagent.
[0044] The present invention adopts a template method and introduces a free radical initiator to prepare an iron-containing small-grain ZSM-5 molecular sieve. The prepared iron-containing small-grain ZSM-5 molecular sieve has a small grain size and has a good catalytic effect when used in the catalytic cracking reaction of light hydrocarbons, and can further improve the conversion rate of saturated hydrocarbons and the selectivity of light olefins.
[0045] In a preferred embodiment of the present disclosure, the peroxide is sodium persulfate or hydrogen peroxide, more preferably sodium persulfate. The peroxide can interact with the metal and the molecular sieve precursor at the same time, promote the nucleation of the molecular sieve around the metal, and encapsulate the metal into the interior of the molecular sieve.
[0046] In a specific embodiment of the present disclosure, step S2 comprises: SS1, mixing the iron source, peroxide and water to obtain a second mixture; the molar ratio of the iron source, peroxide and water in terms of Fe2O3 is 1:(0.2-2.5):(100-1500); preferably 1:(0.2-2):(500-800); SS2, mixing the first mixture with the second mixture and then performing the hydrothermal reaction; the molar ratio of the first mixture in terms of Al2O3 to the second mixture in terms of Fe2O3 is 1:(0.01-2.5), preferably 1:(0.4-1.8). Within the above-mentioned dosage ratio, the second mixture can be free of free iron ions or ferrous ions, thereby avoiding the presence of aggregated iron active components in the prepared molecular sieve and further improving its catalytic performance.
[0047] In a specific embodiment of the present disclosure, in step S1, the molar ratio of the silicon source calculated as SiO2, the aluminum source calculated as Al2O3, the alkali source calculated as alkali metal oxide, the template and the water is (20-300):1:(1-10):(1-30):(500-1500), preferably (30-100):1:(2-8):(2-10):(500-1200); calculated as SiO2, relative to the total weight of the silicon source, the amount of the seed crystal used is 3-12% by weight, preferably 8-10% by weight.
[0048] According to the present disclosure, hydrothermal treatment is well known to those skilled in the art and can be carried out in equipment well known to those skilled in the art, such as a closed heat-resistant and pressure-resistant reactor. In a specific embodiment of the present disclosure, in step S2, the conditions of the hydrothermal reaction include: a temperature of 150-220°C and a time of 8-32h; preferably, a temperature of 150-180°C and a time of 8-20h. The present disclosure does not specifically limit the pressure of the hydrothermal reaction, for example, it can be carried out under the autogenous pressure of the reaction system or under an applied pressure, preferably, under the autogenous pressure of the reaction system.
[0049] In a specific embodiment of the present disclosure, the method further includes: exchanging ammonium and calcining the solid product obtained by the hydrothermal treatment; the conditions of the calcination treatment include: a temperature of 400-800°C, a time of 0.5-8h, and an atmosphere of air atmosphere or water vapor atmosphere; preferably, the temperature is 500-600°C and the time is 2-4h. The calcination treatment is well known to those skilled in the art, and can be carried out in a muffle furnace, a tubular furnace, etc. In a preferred embodiment, the solid product is washed to neutrality before exchanging ammonium, and the liquid used for washing can be any type of liquid that does not react with the solid product, for example, it can be deionized water. In another preferred specific embodiment, the solid obtained by the ammonium exchange is dried before calcination, and the drying conditions can include: a temperature of 100-150°C and a time of 5-20h.
[0050] In a specific embodiment of the present disclosure, the solid product obtained by the hydrothermal treatment can be taken out by centrifugal separation, precipitation and the like.
[0051] According to the present disclosure, the silicon source, aluminum source and alkali source are well known to those skilled in the art. In a specific embodiment of the present disclosure, the silicon source includes one or more of silica gel, silicon dioxide, white carbon black and silicate; the aluminum source includes one or more of sodium aluminate, SB powder, aluminum alcoholate, aluminum oxide, aluminum hydroxide and aluminum sulfate; the alkali source includes sodium hydroxide and / or potassium hydroxide.
[0052] According to the present disclosure, the iron source may be a water-soluble iron salt and / or ferrous salt. In a specific embodiment of the present disclosure, the iron source is selected from one or more of ferric nitrate, ferric sulfate and ferric hydroxide.
[0053] In a specific embodiment of the present disclosure, the seed crystal includes one or more of the ZSM-5 molecular sieves with a silicon-aluminum ratio of 20-50, for example, including but not limited to ZPR molecular sieve, ZSP molecular sieve, etc.; the average particle size of the ZSM-5 molecular sieve is 0.5-2μm, preferably 1-2μm. The average particle size of the ZSM-5 molecular sieve in the present disclosure refers to the average particle size of the molecular sieve estimated by SEM analysis of the molecular sieve and measuring the particle size of 50 particles randomly selected in the SEM photo to obtain the average value, and the SEM instrument model is HITACHI S-4800.
[0054] According to the present disclosure, the template is an organic nitrogen-containing template, preferably including one or more of aminoalkanes, nitrogen-containing organic hydroxides and organic ammonium bromides; further preferably including one or more of n-butylamine, tetrapropylammonium hydroxide and tetrapropylammonium bromide.
[0055] The second aspect of the present disclosure provides a ZSM-5 molecular sieve containing small iron crystals prepared by the method provided in the first aspect of the present disclosure.
[0056] In a specific embodiment of the present disclosure, the ZSM-5 molecular sieve containing small iron grains has a structure in which the iron active component is encapsulated inside the ZSM-5 molecular sieve; the iron active component is distributed on the skeleton of the ZSM-5 molecular sieve, and the grain size of the ZSM-5 molecular sieve containing small iron grains is 0.3-0.8 μm.
[0057] The grain size of the iron-containing small-grain ZSM-5 molecular sieve disclosed in the present invention is further preferably 0.5-0.8 μm.
[0058] In the present disclosure, "iron active components are distributed on the framework of the ZSM-5 molecular sieve" means that at least part of the Si and Al on the framework of the ZSM-5 molecular sieve are replaced by Fe. The introduction of iron elements can adjust the acid properties of the ZSM-5 molecular sieve, improve its catalytic function of cracking and dehydrogenation, and introduce the iron active components into the interior of the molecular sieve in an encapsulated manner, further reducing the severity of the catalytic cracking reaction of light hydrocarbons, and improving the conversion rate of saturated hydrocarbons and the selectivity of light olefins. In the present disclosure, "the outer surface of the particles of the iron-containing small-grain ZSM-5 molecular sieve does not contain iron active components" means that the iron active components are not distributed on the outer surface of the molecular sieve, and the outer surface of the iron active components is not connected to the outer surface of the ZSM-5 molecular sieve. Compared with the presence of iron active components on the outer surface of the molecular sieve, the iron active components of the molecular sieve disclosed in the present disclosure are more evenly distributed inside the molecular sieve, which is more conducive to the selective dehydrogenation of alkanes into olefins in the pores of the molecular sieve, rather than dehydrogenation on the outer surface of the molecular sieve.
[0059] In the present disclosure, the iron active component may include framework iron and / or Fe2O3.
[0060] In a specific embodiment of the present disclosure, the specific surface area of the ZSM-5 molecular sieve containing small iron crystals is 240-550 m 2 / g, preferably 320-370m 2 / g, with a total pore volume of 0.150-0.28 cm 3 ·g -1 , preferably 0.16-0.24cm 3 ·g -1 , the micropore volume is 0.140-0.200cm 3 ·g -1 , preferably 0.15-0.18cm 3 ·g -1 , the mesopore volume is 0.010-0.120cm 3 ·g -1 , preferably 0.01-0.015cm 3 ·g -1 , the relative crystallinity is 82-100%, preferably 85-100%; in the ZSM-5 molecular sieve containing small iron grains, the molar ratio of SiO2 to Al2O3 is 20-300; relative to the total weight of the ZSM-5 molecular sieve containing small iron grains, the content of iron active components calculated as Fe2O3 is 0.3-3% by weight, preferably 0.8-1.5% by weight.
[0061] Wherein, the molar ratio of SiO2 to Al2O3 can be obtained by X-ray fluorescence spectroscopy. The relative crystallinity is measured by Siemens D5005 X-ray diffractometer based on the standard sample of ZSM-5 molecular sieve of Petrochemical Research Institute of Petrochemicals (i.e., the relative crystallinity of the standard sample of ZSM-5 molecular sieve of Petrochemical Research Institute of China Petrochemical Corporation is 100%). The specific surface area and pore volume parameters can be determined by using a specific surface area tester according to the principle of N2 adsorption and the BET calculation method (see petrochemical analysis method (RIPP test method), RIPP151-90, Science Press, published in 1990). The content of the active iron component in terms of Fe2O3 is measured by X-ray fluorescence spectroscopy.
[0062] The third aspect of the present disclosure provides an application of the iron-containing small-grain ZSM-5 molecular sieve provided by the second aspect of the present disclosure in the catalytic cracking reaction of n-tetradecane and the catalytic cracking reaction of light hydrocarbons.
[0063] In a specific embodiment of the present disclosure, the conditions of the catalytic cracking reaction include: a temperature of 500-680°C, a reaction pressure of 0.8-1.2 MPa, and a catalyst-oil weight ratio of 1-1.8; preferably, the temperature is 540-600°C, the reaction pressure is 1-1.2 MPa, and the catalyst-oil weight ratio is 1.28-1.92.
[0064] The present disclosure is further illustrated below by way of examples, but the present disclosure is not limited thereby.
[0065] Silicon-aluminum molar ratio: that is, the molar ratio of SiO2 to Al2O3, tested by X-ray fluorescence spectrometry, the instrument model is Japan Rigaku Electric Co., Ltd. 3013 X-ray fluorescence spectrometer; test conditions: tungsten target, excitation voltage 40kV, excitation current 50mA;
[0066] Grain size: The molecular sieve is analyzed by SEM, and 50 particles are randomly selected from the SEM photo to measure the particle size and calculate the average value to estimate the grain size. The SEM instrument model is HITACHI S-4800.
[0067] Relative crystallinity: measured by Siemens D5005 X-ray diffractometer, with ZSM-5 molecular sieve standard sample of Petrochemical Research Institute as the benchmark (i.e., the relative crystallinity of ZSM-5 molecular sieve standard sample of Petrochemical Research Institute of China Petrochemical Corporation is 100%);
[0068] Specific surface area: determined by using a specific surface area tester based on the N2 adsorption principle and the BET calculation method (see Petrochemical Analysis Method (RIPP Test Method), RIPP151-90, Science Press, published in 1990);
[0069] Pore volume test method: The sample was vacuumed to 1.33×10 at 350°C. -2 Pa, constant temperature and pressure for 15 hours. Tests were conducted at liquid nitrogen temperature of -196°C to measure the adsorption and desorption of N2 under different relative pressures (p / p0). The desorption branch data were calculated using the BJH (Barrett-Joyner-Halenda) method to obtain the pore size distribution data of the sample;
[0070] The scanning electron microscope instrument model is HITACHI S-4800 scanning electron microscope; the test conditions are: the acceleration voltage is 20.0 kV, and after the sample is processed, the grain morphology and size of the molecular sieve sample are observed at a magnification of 5000-30000;
[0071] The transmission electron microscope instrument model is JEM-2100 (200 kV) transmission electron microscope of JEOL Ltd.; the test conditions are: the acceleration voltage is 200 kV, and after the sample is processed, the grain morphology and size of the molecular sieve sample are observed at a magnification of 5000-30000;
[0072] STEM-Mapping test method and instrument: JEOL Ltd. JEM-2100 (200kV) transmission electron microscope. The accelerating voltage of the electron microscope is 200kV. Anhydrous ethanol is dispersed in the sample, and then dripped on the sample net with a diameter of 3mm for observation and testing;
[0073] Test method for the content of active iron components in terms of Fe2O3: Semi-quantitative analysis of iron is performed by measuring the intensity of characteristic spectral lines of each element through XRF.
[0074] Example 1
[0075] This example uses the following steps to prepare iron-containing small-grain ZSM-5 molecular sieve A:
[0076] (1) adding 0.99 g of sodium hydroxide, 40.8 g of deionized water, 20 g of silica gel, 6.77 g of low-alkali sodium aluminate (Na2O: 156.3 g / L, Al2O3: 103.8 g / L), 1.97 g of ZSM-5 seed crystals, and 1.98 g of n-butylamine in sequence under stirring, and stirring well to obtain a first mixture;
[0077] The molar ratio of silicon source calculated as SiO2, aluminum source calculated as Al2O3, alkali source calculated as alkali metal oxide, n-butylamine and water is 55:1:4.675:4.95:589; the amount of ZSM-5 seed crystals used is 10 wt% relative to the total weight of the silicon source calculated as SiO2; the silicon-aluminum ratio of the ZSM-5 seed crystals is 27, and the average particle size is 1-2 μm;
[0078] (2) dissolving 1.13 g of ferric nitrate nonahydrate in 10 g of deionized water, adding 0.14 g of sodium persulfate, and stirring until the mixture becomes clear and transparent to obtain a second mixture; wherein the molar ratio of the iron source calculated as Fe2O3, sodium persulfate and water is 1:0.2:200, and the molar ratio of the aluminum source calculated as Al2O3 to the iron source calculated as Fe2O3 is 1:0.40;
[0079] (3) adding the second mixture to the first mixture, mixing thoroughly and then transferring to a stainless steel kettle for hydrothermal treatment at 170° C. for 12 h;
[0080] (4) The product obtained by the hydrothermal treatment in step (3) was filtered, washed to pH=7-8, and then dried at 120°C for 12 hours after ammonium exchange, and then calcined at 550°C for 2 hours in an air atmosphere to obtain a small-grain ZSM-5 molecular sieve encapsulated with iron, denoted as A, with structural parameters listed in Table 1 and an X-ray diffraction spectrum shown in Figure 1 , SEM photos are shown in Figure 2 , STEM and Mapping photos see Figure 3 and Figure 4 .
[0081] Example 2
[0082] In this embodiment, the same method as in embodiment 1 is used to prepare iron-containing small-grain ZSM-5 molecular sieve B, except that in step (2), 1.13 g of ferric nitrate nonahydrate is dissolved in 10 g of deionized water, 0.28 g of sodium persulfate is added, and the mixture is stirred until it becomes clear and transparent to obtain a second mixture; wherein the molar ratio of the iron source calculated as Fe2O3, sodium persulfate and water is 1:0.4:200, and the molar ratio of the aluminum source calculated as Al2O3 to the iron source calculated as Fe2O3 is 1:0.40; and the small-grain ZSM-5 molecular sieve encapsulating iron is obtained, which is denoted as B, and the structural parameters are listed in Table 1. Its X-ray diffraction spectrum is shown in Table 1. Figure 5 , SEM photos are shown in Figure 6 .
[0083] Example 3
[0084] This embodiment adopts the same method as that of embodiment 1 to prepare iron-containing small-grain ZSM-5 molecular sieve C, except that, in step (1), 1.53 g of sodium hydroxide, 105 g of deionized water, 20 g of silica gel, 3.38 g of low-alkali sodium aluminate (Na2O: 156.3 g / L, Al2O3: 103.8 g / L), 1.97 g of ZSM-5 seed crystals, and 1.43 g of n-butylamine are added in sequence under stirring, and stirred well to obtain a first mixture;
[0085] Among them, the molar ratio of silicon source calculated as SiO2, aluminum source calculated as Al2O3, alkali source calculated as alkali metal oxide, n-butylamine and water is 110:1:9.35:11:2420; calculated as SiO2, the amount of ZSM-5 seeds used is 10 weight% relative to the total weight of the silicon source; the silicon-to-aluminum ratio of the ZSM-5 seeds is 27, and the average particle size is 1-2μm.
[0086] Example 4
[0087] This embodiment adopts the same method as that of embodiment 1 to prepare iron-containing small-grain ZSM-5 molecular sieve D, except that: (1) 1.23 g of sodium hydroxide, 41.9 g of deionized water, 20 g of silica gel, 5.33 g of low-alkali sodium aluminate (Na2O: 156.3 g / L, Al2O3: 103.8 g / L), 1.97 g of ZSM-5 seed crystals, and 1.98 g of n-butylamine are added in sequence under stirring and stirred well to obtain a first mixture;
[0088] The molar ratio of silicon source calculated as SiO2, aluminum source calculated as Al2O3, alkali source calculated as alkali metal oxide, n-butylamine and water is 70:1:4.675:9.9:589; the amount of ZSM-5 seed crystals used is 10 wt% relative to the total weight of the silicon source calculated as SiO2; the silicon-aluminum ratio of the ZSM-5 seed crystals is 27, and the average particle size is 1-2 μm;
[0089] (2) dissolving 1.08 g of ferric nitrate nonahydrate in 10 g of deionized water, adding 0.56 g of sodium persulfate, and stirring thoroughly until the mixture becomes clear and transparent to obtain a second mixture; wherein the molar ratio of the iron source calculated as Fe2O3, sodium persulfate and water is 1:0.8:200, and the molar ratio of the aluminum source calculated as Al2O3 to the iron source calculated as Fe2O3 is 1:0.40.
[0090] Example 5
[0091] This embodiment adopts the same method as that of Embodiment 1 to prepare small iron-containing grains, except that, in step (2), 1.13 g of ferric nitrate nonahydrate is dissolved in 22.5 g of deionized water, 1.61 g of sodium persulfate is added, and the mixture is stirred until it becomes clear and transparent to obtain a second mixture; wherein the molar ratio of the iron source calculated as Fe2O3, sodium persulfate and water is 1:2.3:450, and the molar ratio of the aluminum source calculated as Al2O3 to the iron source calculated as Fe2O3 is 1:0.4.
[0092] Comparative Example 1
[0093] The iron-containing small-grain ZSM-5 molecular sieve D1 was prepared in the same manner as in Example 2, except that sodium persulfate, a free radical initiator, was not added.
[0094] (1) adding 0.99 g of sodium hydroxide, 40.8 g of deionized water, 20 g of silica gel, 6.77 g of low-alkali sodium aluminate (Na2O: 156.3 g / L, Al2O3: 103.8 g / L), 1.97 g of ZSM-5 seed crystals, and 1.98 g of n-butylamine in sequence under stirring, and stirring well to obtain a first mixture;
[0095] The molar ratio of silicon source calculated as SiO2, aluminum source calculated as Al2O3, alkali source calculated as alkali metal oxide, n-butylamine and water is 55:1:4.675:4.95:589; the amount of ZSM-5 seed crystals used is 10 wt% relative to the total weight of the silicon source calculated as SiO2; the silicon-aluminum ratio of the ZSM-5 seed crystals is 27, and the average particle size is 1-2 μm;
[0096] (2) 1.13 g of ferric nitrate nonahydrate was dissolved in 10 g of deionized water and stirred thoroughly until the mixture was clear and transparent to obtain a second mixture; after high temperature crystallization, an iron-containing ZSM-5 molecular sieve was obtained, which was denoted as D1 and whose structural parameters are listed in Table 1.
[0097] Test Case
[0098] The iron-containing ZSM-5 molecular sieves prepared in the examples and comparative examples were subjected to aging treatment. The specific aging treatment method is as follows: the aging furnace is a hydrothermal aging device made by the Institute of Petroleum Science and Technology, and the state after aging at 800°C for 17 hours is used to simulate the balance agent in industrial operation.
[0099] The iron-containing ZSM-5 molecular sieve prepared in the embodiment and the comparative example was used as a catalyst in the catalytic cracking reaction of light hydrocarbons to carry out the catalytic cracking reaction of n-tetradecane. The specific method is as follows: the reaction is carried out in a fixed bed reactor, the feed oil is n-tetradecane, the carrier gas is nitrogen, the flow rate is 30 mL / min, the reaction temperature is 550°C, the regeneration temperature is 600°C, the reaction pressure is 0.1 MPa, and the weight space velocity is 20 hr -1 The molecular sieve was sieved into 20-40 mesh particles after tableting, the loading amount was 2.0 g, the agent-oil ratio was 1.28, and the sample was analyzed after 900 seconds of reaction, and the material balance calculation was performed. The product distribution is shown in Table 1.
[0100] The following formula is used to calculate the micro-reverse conversion rate X of the raw material and the yield S of the product: i :
[0101]
[0102]
[0103]
[0104]
[0105] Table 1
[0106]
[0107] According to the data in Table 1, the iron-containing small-grain ZSM-5 molecular sieve prepared by the template method and the introduction of a free radical initiator in the present disclosure has a high relative crystallinity of about 80-105%, and a small grain size of 0.5-0.8 μm. It can be seen from the scanning electron microscope photos of the iron-containing ZSM-5 molecular sieve prepared by Examples 1-3 that the grain size of the iron-containing ZSM-5 molecular sieve prepared by the method of the present disclosure is 0.5-1 μm, which belongs to a small-grain molecular sieve; it can be seen from the STEM-Mapping photos of the iron-containing ZSM-5 molecular sieve prepared by Examples 1-3 that the iron active component in the iron-containing ZSM-5 molecular sieve prepared by the method of the present disclosure is evenly distributed.
[0108] And according to the data in Tables 1 and 2, when the iron-containing small-grain ZSM-5 molecular sieve prepared by the method disclosed in the present invention is used for the catalytic cracking reaction of light hydrocarbons, a higher micro-reverse conversion rate and a better light olefin yield can be obtained, and the yield of propylene can be improved; according to the comparison between Example 1-2 and Example 3, when the molar ratio of the silicon source calculated as SiO2, the aluminum source calculated as Al2O3, the alkali source calculated as alkali metal oxide, the template agent and water is (30-100): 1: (2- 8): (2-10): (500-1200), a higher micro-reverse conversion rate and propylene yield can be obtained; according to the comparison between Example 1 and Example 5, when the molar ratio of the iron source, peroxide and water calculated as Fe2O3 is 1: (0.2-2): (500-800), a higher micro-reverse conversion rate and propylene yield can be obtained; according to the comparison between Examples 1 and 2, when the silicon-aluminum ratio is relatively low, the acidity of the molecular sieve is stronger and a higher micro-reverse conversion rate can be obtained.
[0109] The preferred embodiments of the present disclosure are described in detail above in conjunction with the accompanying drawings; however, the present disclosure is not limited to the specific details in the above embodiments. Within the technical concept of the present disclosure, a variety of simple modifications can be made to the technical solution of the present disclosure, and these simple modifications all fall within the protection scope of the present disclosure.
[0110] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present disclosure will not further describe various possible combinations.
[0111] In addition, various embodiments of the present disclosure may be arbitrarily combined, and as long as they do not violate the concept of the present disclosure, they should also be regarded as the contents disclosed by the present disclosure.
Claims
1. A method for preparing a ZSM-5 molecular sieve containing small iron crystals, the method comprising: S1, mixing a silicon source, an aluminum source, an alkali source, a seed crystal, a template and water to obtain a first mixture; S2, mixing the iron source, peroxide, water and the first mixture and performing a hydrothermal reaction; Wherein, the peroxide is selected from one or more of sodium persulfate, hydrogen peroxide and Fenton's reagent.
2. The method according to claim 1, wherein: Step S2 includes: SS1. Mixing the iron source, peroxide and water to obtain a second mixture; the molar ratio of the iron source, peroxide and water in terms of Fe2O3 is 1:(0.2-2.5):(100-1500); preferably 1:(0.2-2):(500-800); SS2. The first mixture and the second mixture are mixed and then subjected to the hydrothermal reaction; the molar ratio of the first mixture calculated as Al2O3 to the second mixture calculated as Fe2O3 is 1:(0.01-2.5), preferably 1:(0.4-1.8).
3. The method according to claim 1, wherein: In step S1, the molar ratio of the silicon source calculated as SiO2, the aluminum source calculated as Al2O3, the alkali source calculated as alkali metal oxide, the template and the water is (20-300):1:(1-10):(1-30):(400-2500), preferably (30-100):1:(2-8):(2-10):(500-1200); Calculated as SiO2, the amount of the seed crystal used is 3-12 wt%, preferably 8-10 wt%, relative to the total weight of the silicon source.
4. The method according to claim 1, wherein: In step S2, the conditions of the hydrothermal reaction include: temperature of 150-220° C. and time of 8-32 h.
5. The method according to claim 1, wherein: The method further comprises: subjecting the solid product obtained by the hydrothermal treatment to ammonium exchange and roasting treatment; the conditions of the roasting treatment include: temperature of 400-800° C., time of 0.5-8 hours, and atmosphere of air or water vapor.
6. The method according to claim 1, wherein: The silicon source includes one or more of silica gel, silicon dioxide, white carbon black and silicate; The aluminum source includes one or more of sodium metaaluminate, SB powder, aluminum alcoholate, aluminum oxide, aluminum hydroxide and aluminum sulfate; The alkali source includes sodium hydroxide and / or potassium hydroxide; The seed crystals include one or more ZSM-5 molecular sieves with a silicon-aluminum ratio of 20-50, and the average particle size of the ZSM-5 molecular sieve is 0.5-2 μm; The iron source is selected from one or more of ferric nitrate, ferric oxalate, ferric sulfate and ferric hydroxide; The template agent includes an organic nitrogen-containing template agent, preferably one or more of n-butylamine, tetrapropylammonium hydroxide and tetrapropylammonium bromide.
7. The ZSM-5 molecular sieve containing small iron crystals prepared by the method according to any one of claims 1 to 6.
8. The iron-containing small-grain ZSM-5 molecular sieve according to claim 7, wherein: The ZSM-5 molecular sieve containing small iron crystals has a structure in which the ZSM-5 molecular sieve has an iron active component encapsulated inside; The iron active component is distributed on the framework of the ZSM-5 molecular sieve, and the grain size of the iron-containing small-grain ZSM-5 molecular sieve is 0.5-0.8 μm.
9. The iron-containing ZSM-5 molecular sieve according to claim 7, wherein: The specific surface area of the ZSM-5 molecular sieve containing small iron crystals is 240-550 m 2 / g, with a total pore volume of 0.150-0.28 cm 3 ·g -1 , the micropore volume is 0.140-0.20cm 3 ·g -1 , the mesopore volume is 0.010-0.120cm 3 ·g -1 , relative crystallinity is 82-100%; In the ZSM-5 molecular sieve containing small iron crystals, the molar ratio of SiO2 to Al2O3 is 20-300; Relative to the total weight of the ZSM-5 molecular sieve containing small iron crystals, the content of the iron active component calculated as Fe2O3 is 0.8-1.5 wt%.
10. Use of the iron-containing small-grain ZSM-5 molecular sieve according to any one of claims 7 to 9 in the catalytic cracking reaction of n-tetradecane.
11. The use according to claim 10, wherein: The conditions of the catalytic cracking reaction include: a temperature of 500-680°C, a reaction mass space velocity of 20-40h -1 , the reaction pressure is 0.8-1.2MPa, and the agent-oil weight ratio is 1-2.
Citation Information
Patent Citations
High-iron content Fe-ZSM-5 molecular sieve preparation method
CN108217681A
Method for synthesizing hierarchical porous Fe-ZSM-5 zeolite molecular sieve by crystal seed process
CN109721076A
Fe-ZSM-5 molecular sieve, preparation method and application thereof
CN112694100A
Hierarchical porous Fe / ZSM-5 molecular sieve and preparation method and application thereof
CN114405538A