Polyacrylate microsphere material, drop ball forming method and application thereof, and fluidized bed CO2 adsorbent

The preparation of polyacrylate microsphere materials through drip ball forming method solves the problems of uneven particle size distribution and low yield in the prior art, and achieves efficient and environmentally friendly microsphere preparation, which is suitable for CO2 adsorption in fluidized beds and improves the The feasibility of industrial production.

CN119081160AActive Publication Date: 2024-12-06PETROCHINA CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202310656860.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-06-05
Publication Date
2024-12-06
Estimated Expiration
2043-06-05

AI Technical Summary

Technical Problem

In the prior art, when preparing polyacrylate microsphere materials, the particle size distribution is uneven, the yield is low and the production efficiency is low, making it difficult to meet the needs of large-scale industrial production.

Method used

By using the drip ball forming method, by emulsifying components such as organic monomers, emulsifiers and initiators in the organic dispersed phase, and using the surface tension in water to form spherical microspheres, the polymerization of one-step balls is achieved, the process is simplified and the harvest is improved. Rate.

Benefits of technology

It achieves high yield, uniform particle size and high mechanical strength of polyacrylate microspheres, and is suitable for fluidized bed CO2 adsorption, reducing production costs and improving the industrialization level of the process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119081160A_ABST
    Figure CN119081160A_ABST
Patent Text Reader

Abstract

The invention provides a polyacrylate microsphere material, a drop ball forming method and application thereof, and a fluidized bed CO2 adsorbent, the drop ball forming method of the polyacrylate microsphere material comprises the following steps: firstly adding two or three organic monomers into an organic dispersion phase, and then sequentially adding an emulsifier, an initiator and a co-emulsifier to form a uniform organic phase; deionized water is dripped into the organic phase for sufficient emulsification, and then a reducing agent is added to obtain a formed emulsion; and carrying out ball-dropping molding and aging on the molding emulsion by using a ball-dropping molding device, and drying the aged balls to obtain the polyacrylate microsphere material. The drop ball forming method provided by the invention is simple in operation process, green and environment-friendly, easy to industrialize, high in yield and low in cost. The prepared polyacrylate microsphere material has the characteristics of low bulk density, small particle size, high sphericity, easy control of particle size, uniform particle size distribution, high mechanical strength and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a polyacrylate microsphere material, a drop ball forming method and application thereof, and a fluidized bed CO2 adsorbent, belonging to the technical field of CO2 adsorption and capture. Background Art

[0002] Greenhouse effect and climate warming are hot issues in the world today. CO2 is the anthropogenic gas that contributes most to the greenhouse effect. Large-scale CO2 capture is the main way to significantly reduce greenhouse gas emissions.

[0003] Regarding CO2 capture, the more mature technology at this stage is chemical absorption, which has the advantages of fast absorption, mature process, and large processing capacity, but it has many defects such as high regeneration energy consumption, limited space for further energy saving and consumption reduction, complex process, and easy corrosion of equipment. In comparison, chemical adsorption has many advantages such as low energy consumption, simple process, and no equipment corrosion. Solid adsorbents include calcium-based adsorbents, metal organic framework materials (MOFs), zeolites, hyper-cross-linked polymers, carbon materials, alkali metal carbonates, amine-functionalized adsorbents, etc. Among them, the polymer material prepared by the emulsion template method has a high porosity and a certain mechanical strength. The internal pores are a three-dimensional interconnected pore structure with a pore size of 0.1-300μm. The pore size can be adjusted to be appropriate and the pore size distribution is uniform. The above characteristics make the emulsion template polymer have outstanding advantages as a solid adsorbent carrier.

[0004] CN106589201A discloses a hydrophilic modification method for polystyrene materials and its products, which can reduce the specific adsorption of biomacromolecules by chloromethylating the surface of polystyrene microspheres and bonding PVA to the surface of polystyrene microspheres. PVA contains a large number of hydroxyl groups, which is convenient for coupling specific ligands to meet different separation mode requirements. However, the hydrophilic modification process is complicated, the steps are cumbersome, and it is difficult to control.

[0005] CN111825796A discloses a polyacrylate composite material for CO2 adsorption and a preparation method thereof. In the preparation process, a polymer emulsion is added to a dispersed phase, dispersed into spheres at a certain rotation speed, a reducing agent is added after stabilization, and the spherical porous polyacrylate spheres are prepared. The spheres are then subjected to amination grafting and epoxy resin surface end-capping treatment to obtain a polyacrylate composite material for CO2 adsorption.

[0006] CN114213581A discloses a method for preparing hydrophilic polyacrylate crosslinked microspheres, in which the hydrophilic substance is connected to the comonomer by chemical bonding, and then copolymerized with the crosslinking agent in an aqueous phase containing a stabilizer to form polymer microspheres.

[0007] The above methods all adopt emulsion suspension polymerization to prepare polyacrylate beads. Although suspension polymerization has been widely used in industry, the particle size of the microspheres obtained mainly depends on the stirring speed during polymerization, so the particle size distribution range is wide and can only be regulated within a narrow range, and there is a problem of low yield. In addition, polyacrylate beads can also be prepared by precipitation polymerization in the prior art, but the production efficiency of precipitation polymerization is very low and does not have the prospect of industrial large-scale production.

[0008] Therefore, providing a new type of polyacrylate microsphere material (polyacrylate cross-linked porous microsphere material) and its drop ball forming method and application, and fluidized bed CO2 adsorbent has become a technical problem that urgently needs to be solved in this field. Summary of the invention

[0009] In order to solve the above-mentioned shortcomings and deficiencies, an object of the present invention is to provide a drop ball forming method of polyacrylate microsphere material.

[0010] Another object of the present invention is to provide a polyacrylate microsphere material, which is prepared by the above-mentioned polyacrylate microsphere material drop ball molding method.

[0011] Another object of the present invention is to provide the use of the above-mentioned polyacrylate microsphere material as a solid adsorbent carrier for fluidized bed CO2 adsorption.

[0012] Another object of the present invention is to provide a fluidized bed CO2 solid adsorbent, wherein the solid adsorption carrier is the polyacrylate microsphere material described above.

[0013] In order to achieve the above objectives, on the one hand, the present invention provides a drop ball forming method of a polyacrylate microsphere material, wherein the drop ball forming method of the polyacrylate microsphere material comprises:

[0014] Step 1: First, two or three organic monomers are added to the organic dispersed phase, and then an emulsifier, an initiator and an emulsifier are added in sequence to form a uniform organic phase;

[0015] Step 2: adding deionized water dropwise into the organic phase for full emulsification and then adding a reducing agent to obtain a formed emulsion;

[0016] Step three: using a drop ball forming device to perform drop ball forming and aging on the formed latex, and then drying the aged small balls to obtain the polyacrylate microsphere material.

[0017] As a specific embodiment of the drop ball forming method described above in the present invention, the organic monomers include two or three organic monomers selected from the group consisting of glycidyl methacrylate, methyl methacrylate, ethyl methacrylate, methyl acrylate, ethyl acrylate, styrene, ethylene glycol dimethacrylate, tert-butyl acrylate, tert-butyl methacrylate and trimethylolpropane triacrylate.

[0018] As a specific embodiment of the drop ball forming method described above, the organic monomers include tert-butyl acrylate, tert-butyl methacrylate and trimethylolpropane triacrylate in a mass ratio of 2-3.5:0.5-1.5:2-3.5.

[0019] In the present invention, the amount of the organic dispersed phase affects the yield, dispersion and mechanical strength of the polyacrylate microsphere material finally obtained. As for the volume fraction of the organic dispersed phase, it is sufficient to ensure that each organic monomer can be fully dissolved and dispersed. As a specific embodiment of the drop ball forming method described above of the present invention, the volume fraction of the organic dispersed phase is 40-60% based on the total volume of the organic phase as 100%.

[0020] As a specific embodiment of the drop ball forming method described above in the present invention, the organic dispersed phase includes one or a combination of cyclohexane, toluene, carbon tetrachloride, dichloromethane, 1-2-dichloroethane, ethyl acetate, etc.; preferably, one or a combination of toluene, cyclohexane, ethyl acetate, etc.

[0021] As a specific embodiment of the drop ball forming method described above, based on the total weight of the two or three organic monomers as 100%, the amounts of the emulsifier, initiator and co-emulsifier are 5-20%, 1-10% and 1-5% respectively.

[0022] As a specific embodiment of the drop ball forming method described above in the present invention, the emulsifier includes one or a combination of span80 (Span 80), span60 (Span 60), span20 (Span 20), polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer, etc.; preferably, polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer (P123).

[0023] As a specific embodiment of the drop ball forming method described above in the present invention, the initiator includes one or a combination of ammonium persulfate, potassium persulfate, benzoyl peroxide, diisopropylbenzene peroxide, tert-butyl peroxide, azobisisobutyronitrile, azobisisovaleronitrile, etc.; preferably benzoyl peroxide.

[0024] As a specific embodiment of the drop ball forming method described above, in step 1, a uniform organic phase can be formed by ultrasound, and the present invention does not make specific requirements on the ultrasound time, etc., which can be reasonably adjusted according to the actual operation conditions on site. For example, in some embodiments of the present invention, the ultrasound time can be 5-10 minutes.

[0025] As a specific embodiment of the drop ball forming method described above, the co-emulsifier includes one or a combination of cetyl alcohol, hexanol, octanol, p-nonylphenol, etc.; preferably cetyl alcohol.

[0026] As a specific embodiment of the drop ball forming method described above, deionized water is dripped into the organic phase for full emulsification so that the deionized water accounts for 45-65% of the total volume of the emulsion obtained after full emulsification.

[0027] As a specific embodiment of the drop ball forming method described above, in step 2, the step of dropping deionized water into the organic phase for full emulsification and then adding the reducing agent specifically includes:

[0028] Under the condition of stirring at a speed of 1000-3000r / min in a high-speed stirrer, deionized water, i.e., the aqueous phase, is dropped into the organic phase. After the dropping is completed, the speed is increased to 5000-10000r / min and stirred for 5-10min to fully emulsify. Then, the reducing agent is added to the fully emulsified emulsion and stirring is continued for 1-2min.

[0029] As a specific embodiment of the drop ball forming method described above, the amount of the reducing agent is 5-20%, based on the total weight of the two or three organic monomers being 100%.

[0030] As a specific embodiment of the drop ball forming method described above in the present invention, the reducing agent includes one or a combination of N,N-dimethylaniline, N,N,N,N-tetramethylethylenediamine, ferrous sulfate, sodium sulfite, etc.; preferably N,N-dimethylaniline.

[0031] As a specific embodiment of the drop ball molding method described above in the present invention, in order to delay the occurrence of the polymerization reaction before molding, the preparation of the emulsion must be carried out under low temperature conditions, that is, step 2 is carried out in a low temperature environment throughout the process to reduce the temperature of the molded emulsion to below 5°C; preferably, step 1 and step 2 are carried out in a low temperature environment throughout the process to reduce the temperature of the molded emulsion to below 5°C.

[0032] As a specific embodiment of the drop ball forming method described above in the present invention, the drop ball forming device comprises a forming emulsion storage tank, a peristaltic pump and a forming column, the forming column is a jacketed glass tube with openings at both ends, a mechanical stirring device is mounted at the upper opening of the jacketed glass tube, a stirring paddle is arranged in the mechanical stirring device, and an embedded drip tray is sealed at the lower opening of the jacketed glass tube, and the embedded drip tray is provided with a plurality of drop ball forming needles that can extend into the forming column;

[0033] The outlet of the forming emulsion storage tank is connected to the inlet of the embedded drip tray through a pipeline via a peristaltic pump.

[0034] As a specific embodiment of the drop ball forming method described above, the lower end opening of the jacketed glass tube and the embedded drip tray are "clamped" together by a flange, and rubber gaskets are arranged between the jacketed glass tube and the embedded drip tray and the flange for isolation.

[0035] As a specific embodiment of the drop ball forming method described above in the present invention, the stirring paddle can be one of the stirring paddles in the form of three-blade paddle, tuning fork type, double crescent type, cross type, straight type, plate type, four-blade type, anchor type, etc.

[0036] As a specific embodiment of the drop ball forming method described above, the forming emulsion storage tank, peristaltic pump, jacketed glass tube, embedded drip tray, drop ball forming needle and mechanical stirring device are all conventional equipment and can be purchased from commercial sources or made by yourself.

[0037] As a specific embodiment of the drop ball forming method described above, in step 3, the drop ball forming and aging of the forming emulsion using a drop ball forming device includes:

[0038] Add an aqueous solution of a dispersant into the jacketed glass tube and heat it to 50-80°C by connecting a water bath to the jacket;

[0039] The molding emulsion is transported to the embedded drip tray by a peristaltic pump and dripped into the jacketed glass tube through a ball-drop molding needle. Since the density of the molding emulsion is lower than that of water, the molding emulsion droplets in the jacketed glass tube continuously float up. During the floating process, the molding emulsion droplets form a spherical shape under the action of the surface tension in the water and undergo polymerization reaction and preliminary solidification to quickly form small balls. When the small balls after preliminary solidification float to the upper part of the jacketed glass tube, they will continue to rotate and stay in the aqueous solution of the dispersant under the action of mechanical stirring and undergo sufficient polymerization reaction to ensure complete molding.

[0040] As a specific embodiment of the drop ball forming method described above, the mass concentration of the aqueous solution of the dispersant is 0.3-2.0%.

[0041] As a specific embodiment of the drop ball forming method described above, the dispersant includes one or a combination of organic dispersants such as polyvinyl alcohol (PVA) and / or polyethylene glycol.

[0042] As a specific embodiment of the drop ball forming method described above, the height of the jacketed glass tube is 1-2 m.

[0043] As a specific embodiment of the drop ball forming method described above, the inner diameter of the drop ball forming needle is 0.2-0.6 mm.

[0044] The present invention does not impose any specific requirements on the dripping rate, which can be reasonably adjusted according to the actual needs of on-site operations, as long as it is ensured that shaped emulsion droplets can be formed.

[0045] As a specific embodiment of the drop ball forming method described above in the present invention, the rotation speed of the mechanical stirring is 100-300 r / min.

[0046] As a specific embodiment of the drop ball forming method described above, the drying is performed at 40-80° C. for 4-8 hours. Drying is a conventional operation and can be performed in an oven.

[0047] On the other hand, the present invention further provides a polyacrylate microsphere material, wherein the polyacrylate microsphere material is prepared by the above-mentioned polyacrylate microsphere material drop ball forming method.

[0048] As a specific embodiment of the polyacrylate microsphere material described above in the present invention, the particle size of the polyacrylate microsphere material is 0.40-0.85 mm, and the bulk density is 0.10-0.20 g / mL.

[0049] In another aspect, the present invention also provides the use of the polyacrylate microsphere material described above as a solid adsorbent carrier for fluidized bed CO2 adsorption.

[0050] On the other hand, the present invention also provides a fluidized bed CO2 solid adsorbent, comprising a solid adsorption carrier and an adsorption active component loaded on the surface of the solid adsorption carrier, wherein the solid adsorption carrier is the polyacrylate microsphere material described above.

[0051] The present invention does not make specific requirements on the adsorption active components and their usage in the fluidized bed CO2 solid adsorbent, and can be reasonably adjusted according to the actual operation needs on site. For example, in some embodiments of the present invention, the adsorption active components can be organic amines such as pentaethylenehexamine.

[0052] Compared with the prior art, the beneficial technical effects that can be achieved by the present invention include:

[0053] The drop ball forming method of the polyacrylate microsphere material provided by the present invention first adds two or three organic monomers into an organic dispersed phase, then sequentially adds an emulsifier, an initiator and an emulsifier co-emulsifier to form a uniform organic phase, then drops an aqueous phase into the organic phase for full emulsification, and then adds a reducing agent to obtain an oil-in-water forming emulsion with a density less than that of water, and finally forms the formed emulsion by a bottom-up drop ball forming method, and obtains the polyacrylate microsphere material by utilizing the surface tension of the formed emulsion in water and the polymerization reaction occurring in the emulsion itself.

[0054] Compared with the traditional precipitation polymerization and suspension polymerization methods, the drop ball forming method of the polyacrylate microsphere material provided by the present invention has the following advantages:

[0055] (1) One-step ball forming, no need for secondary molding, simple operation process, green and environmentally friendly, easy to industrialize, high yield. Its yield can be increased by more than 30% compared with the emulsion suspension polymerization method, reducing production costs;

[0056] (2) The operating conditions are mild, and polymerization can be achieved at a relatively low temperature without the need for high-temperature calcination;

[0057] (3) The prepared polyacrylate microsphere material has the characteristics of low bulk ratio and small particle size, wherein the particle size is 0.40-0.85 mm and the bulk density is 0.10-0.20 g / mL, and is suitable as a solid adsorbent carrier for fluidized bed CO2 adsorption;

[0058] (4) The polyacrylate microsphere material prepared has high sphericity, easy to control particle size and uniform particle size distribution;

[0059] (5) The prepared polyacrylate microsphere material has high mechanical strength and is not easily worn during fluidized bed operation. BRIEF DESCRIPTION OF THE DRAWINGS

[0060] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0061] Figure 1 Schematic diagram of the structure of the drop ball forming device used in the embodiment of the present invention.

[0062] Figure 2 This is a physical picture of the polyacrylate microsphere material provided in Example 2 of the present invention.

[0063] Figure 3This is a physical picture of the polyacrylate microsphere material provided in Example 5 of the present invention.

[0064] Figure 4 This is a physical picture of the polyacrylate material provided in Comparative Example 1 of the present invention.

[0065] Figure 5 This is a physical picture of the polyacrylate material provided in Comparative Example 5A of the present invention.

[0066] Figure 6 This is a physical picture of the polyacrylate material provided in Comparative Example 5B of the present invention.

[0067] Figure 7 This is a scanning electron microscope image (500 μm) of the polyacrylate microsphere material provided in Example 1 of the present invention.

[0068] Figure 8 This is a scanning electron microscope image (3.00 μm) of the polyacrylate microsphere material provided in Example 1 of the present invention.

[0069] Description of main figures:

[0070] 1. Molding emulsion storage tank;

[0071] 2. Peristaltic pump;

[0072] 3. Embedded drip tray;

[0073] 31. Drop ball forming needle

[0074] 4. Molding column;

[0075] 5. Mechanical stirring device;

[0076] 51. Stirring paddle.

[0077] 6. Aqueous solution of dispersant. DETAILED DESCRIPTION

[0078] It should be noted that the term "comprises" and any variations thereof in the specification and claims of the present invention and the above-mentioned drawings are intended to cover non-exclusive inclusions. For example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.

[0079] "Scope" disclosed in the present invention is given in the form of lower limit and upper limit. It can be one or more lower limits, and one or more upper limits respectively. A given range is defined by selecting a lower limit and an upper limit. The selected lower limit and upper limit define the boundaries of a particular range. All ranges defined in this way are combinable, i.e. any lower limit can be combined with any upper limit to form a range. For example, for a specific parameter, a range of 60-120 and 80-110 is listed, and it is understood that a range of 60-110 and 80-120 is also expected. In addition, if the minimum range values ​​listed are 1 and 2, and the maximum range values ​​listed are 3, 4 and 5, then the following ranges can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5.

[0080] In the present invention, unless otherwise specified, the numerical range "ab" represents an abbreviation of any real number combination between a and b, where a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" have been listed in the present invention, and "0-5" is just an abbreviation of these numerical combinations.

[0081] In the present invention, unless otherwise specified, all embodiments and preferred embodiments mentioned in the present invention can be combined with each other to form a new technical solution.

[0082] In the present invention, unless otherwise specified, all technical features and preferred features mentioned in the present invention can be combined with each other to form a new technical solution.

[0083] In the present invention, if not specifically stated, the term "two" used in this specification means "at least two".

[0084] In the present invention, unless otherwise specified, all steps mentioned herein may be performed sequentially or randomly, but are preferably performed sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0085] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with the attached table, drawings and examples. The following described embodiments are some embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention, and should not be regarded as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present invention. If the specific conditions are not specified in the embodiments, they are carried out according to the normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified in the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0086] Example 1

[0087] This embodiment provides a polyacrylate microsphere material, which is prepared by a drop ball forming method comprising the following specific steps:

[0088] Step 1: Weigh 10g of tert-butyl acrylate, 2.5g of tert-butyl methacrylate and 10g of trimethylolpropane triacrylate and add them into toluene accounting for 40% of the total volume of the organic phase, then add 1.2g of P123, 0.3g of benzoyl peroxide (BPO) and 0.3g of hexadecanol in sequence, and then ultrasonicate in an ultrasonic cleaner for 5min to dissolve and mix evenly to obtain a uniform organic phase;

[0089] Step 2: Weigh a certain amount of deionized water (accounting for 45% of the total volume of the fully emulsified emulsion) as the water phase, put the dissolved oil phase, i.e., the uniform organic phase, in an ice bath, and slowly drop the water phase into the oil phase at a high-speed stirrer at a speed of 1000 r / min. After the drop is completed, increase the speed to 9000 r / min and stir for 5 minutes to fully emulsify, then add 1.2 g of reducing agent N, N-dimethylaniline and continue stirring for 2 minutes to obtain a formed emulsion;

[0090] Step 3: Using a drop ball forming device to perform drop ball forming and aging on the formed emulsion, wherein the structure diagram of the drop ball forming device is as follows: Figure 1 As shown, from Figure 1 It can be seen that the drop ball forming device includes: a forming emulsion storage tank 1, a peristaltic pump 2 and a forming column 4 with a height of 1.3m, the forming column 4 is a jacketed glass tube with openings at both ends, a mechanical stirring device 5 is set up at the upper end opening of the jacketed glass tube, a three-blade paddle 51 is arranged in the mechanical stirring device 5, and an embedded drip tray 3 is sealed at the lower end opening of the jacketed glass tube, and the embedded drip tray 3 is provided with a plurality of drop ball forming needles 31 that can extend into the forming column 4;

[0091] The outlet of the forming emulsion storage tank 1 is connected to the inlet of the embedded drip tray 3 through a pipeline via a peristaltic pump 2;

[0092] Therefore, the drop ball forming and aging of the formed emulsion using the drop ball forming device as shown above specifically includes:

[0093] Prepare an aqueous solution 6 of a dispersant, which in this embodiment is an aqueous solution of polyvinyl alcohol (PVA) with a mass concentration of 0.5%, and add it to a jacketed glass tube and a mechanical stirring device 5, while ensuring that a three-blade stirring paddle 51 is located below the liquid surface of the aqueous solution of polyvinyl alcohol (PVA), and then heat it to 60° C. by connecting a water bath device through the jacket;

[0094] The molding emulsion is transported to the embedded drip tray by a peristaltic pump and dripped into the jacketed glass tube by a drop ball molding needle (with an inner diameter of 0.21 mm). The molding emulsion droplets in the jacketed glass tube continuously float up. During the floating process, the molding emulsion droplets form a sphere under the action of the surface tension in the water and undergo polymerization reaction and preliminary solidification. When the preliminary solidified small ball floats to the upper part of the jacketed glass tube, close to the liquid surface position of the aqueous solution of polyvinyl alcohol (PVA), it will continue to rotate and stay in the aqueous solution of polyvinyl alcohol under the action of mechanical stirring of a three-blade paddle 51 (with a rotation speed of 150 r / min) and undergo sufficient polymerization reaction to ensure complete molding;

[0095] After the molding is completed, the small balls are taken out and placed in an oven at 50° C. to dry for 8 hours to prepare polymer small balls, namely the polyacrylate microsphere material.

[0096] Example 2

[0097] This embodiment provides a polyacrylate microsphere material, which is prepared by a drop ball forming method comprising the following specific steps:

[0098] Step 1: Weigh 10g of tert-butyl acrylate, 7.5g of tert-butyl methacrylate and 10g of trimethylolpropane triacrylate into toluene accounting for 45% of the total volume of the organic phase, then add 2.7g of span80, 0.5g of ammonium persulfate and 0.5g of hexanol in sequence, and then ultrasonicate in an ultrasonic cleaner for 8min to dissolve and mix evenly to obtain a uniform organic phase;

[0099] Step 2: Weigh a certain amount of deionized water (accounting for 50% of the total volume of the emulsion obtained after sufficient emulsification) as the water phase, put the dissolved oil phase, that is, the uniform organic phase, in an ice bath, and slowly add the water phase to the oil phase at a high-speed stirrer speed of 2000r / min. After the dripping is completed, increase the speed to 8000r / min and stir for 6min to fully emulsify, then add 2.7g of reducing agent N,N,N,N-tetramethylethylenediamine, and continue stirring for 2min to obtain a formed emulsion;

[0100] Step 3: Using a drop ball forming device to perform drop ball forming and aging on the formed emulsion, wherein the structure diagram of the drop ball forming device is as follows: Figure 1 As shown, from Figure 1 It can be seen that the drop ball forming device includes: a forming emulsion storage tank 1, a peristaltic pump 2 and a forming column 4 with a height of 1.3m, the forming column 4 is a jacketed glass tube with openings at both ends, a mechanical stirring device 5 is set up at the upper end opening of the jacketed glass tube, a tuning fork stirring paddle 51 is arranged in the mechanical stirring device 5, and an embedded drip tray 3 is sealed at the lower end opening of the jacketed glass tube, and the embedded drip tray 3 is provided with a plurality of drop ball forming needles 31 that can extend into the forming column 4;

[0101] The outlet of the forming emulsion storage tank 1 is connected to the inlet of the embedded drip tray 3 through a pipeline via a peristaltic pump 2;

[0102] Therefore, the drop ball forming and aging of the formed emulsion using the drop ball forming device as shown above specifically includes:

[0103] Prepare an aqueous solution 6 of a dispersant, which in this embodiment is an aqueous solution of polyethylene glycol with a mass concentration of 1.0%, and add it to a jacketed glass tube and a mechanical stirring device 5, while ensuring that a tuning fork stirring paddle 51 is below the liquid surface of the aqueous solution of polyethylene glycol, and then heat it to 65° C. by connecting a water bath device through the jacket;

[0104] The molding emulsion is transported to the embedded drip tray by a peristaltic pump and dripped into the jacketed glass tube by a drop ball molding needle (with an inner diameter of 0.31 mm). The molding emulsion droplets in the jacketed glass tube continuously float up. During the floating process, the molding emulsion droplets form a sphere under the action of the surface tension in the water and undergo polymerization reaction and preliminary solidification. When the preliminary solidified small ball floats to the upper part of the jacketed glass tube, close to the liquid surface position of the polyethylene glycol aqueous solution, it will continue to rotate and stay in the polyethylene glycol aqueous solution under the action of mechanical stirring (rotation speed of 250 r / min) of the tuning fork stirring paddle 51 and undergo sufficient polymerization reaction to ensure complete molding;

[0105] After the molding is completed, the small balls are taken out and placed in an oven at 60° C. to dry for 7 hours to prepare polymer small balls, namely the polyacrylate microsphere material.

[0106] Example 3

[0107] This embodiment provides a polyacrylate microsphere material, which is prepared by a drop ball forming method comprising the following specific steps:

[0108] Step 1: Weigh 10g of tert-butyl acrylate, 5g of tert-butyl methacrylate and 15g of trimethylolpropane triacrylate and add them into toluene accounting for 50% of the total volume of the organic phase, then add 3.6g of span60, 1.5g of diisopropylbenzene peroxide and 0.9g of octanol in sequence, and then ultrasonicate in an ultrasonic cleaner for 7min to dissolve and mix evenly to obtain a uniform organic phase;

[0109] Step 2: Weigh a certain amount of deionized water (accounting for 55% of the total volume of the emulsion obtained after full emulsification) as the water phase, put the dissolved oil phase, i.e., the organic phase, in an ice bath, and slowly drop the water phase into the oil phase at a high-speed stirrer at a speed of 2500 r / min. After the drop is complete, increase the speed to 7500 r / min and stir for 7 minutes to fully emulsify, then add 3.6 g of reducing agent ferrous sulfate, and continue stirring for 1 minute to obtain a formed emulsion;

[0110] Step 3: Using a drop ball forming device to perform drop ball forming and aging on the formed emulsion, wherein the structure diagram of the drop ball forming device is as follows: Figure 1 As shown, from Figure 1 It can be seen that the drop ball forming device includes: a forming emulsion storage tank 1, a peristaltic pump 2 and a forming column 4 with a height of 1.3m, the forming column 4 is a jacketed glass tube with openings at both ends, a mechanical stirring device 5 is set up at the upper end opening of the jacketed glass tube, a double crescent-shaped stirring paddle 51 is arranged in the mechanical stirring device 5, and an embedded drip tray 3 is sealed at the lower end opening of the jacketed glass tube, and the embedded drip tray 3 is provided with a plurality of drop ball forming needles 31 that can extend into the forming column 4;

[0111] The outlet of the forming emulsion storage tank 1 is connected to the inlet of the embedded drip tray 3 through a pipeline via a peristaltic pump 2;

[0112] Therefore, the drop ball forming and aging of the formed emulsion using the drop ball forming device as shown above specifically includes:

[0113] Prepare an aqueous solution 6 of a dispersant, which in this embodiment is a mixed aqueous solution of polyvinyl alcohol and polyethylene glycol with a mass concentration of 1.5%, and add it into a jacketed glass tube and a mechanical stirring device 5, while ensuring that the double crescent-shaped stirring paddle 51 is located below the liquid surface of the mixed aqueous solution of polyvinyl alcohol and polyethylene glycol, and then heat it to 70° C. by connecting a water bath device through the jacket;

[0114] The molding emulsion is transported to the embedded drip tray by a peristaltic pump and dripped into the jacketed glass tube by a drop ball molding needle (with an inner diameter of 0.41 mm). The molding emulsion droplets in the jacketed glass tube continuously float up. During the floating process, the molding emulsion droplets form a sphere under the action of the surface tension in the water and undergo polymerization reaction and preliminary solidification. When the preliminary solidified small ball floats to the upper part of the jacketed glass tube, close to the liquid surface position of the mixed aqueous solution of polyvinyl alcohol and polyethylene glycol, it will continue to rotate and stay in the aqueous solution of polyvinyl alcohol and polyethylene glycol under the action of mechanical stirring (rotation speed of 100 r / min) of the double crescent-shaped stirring paddle 51 and undergo sufficient polymerization reaction to ensure complete molding;

[0115] After the molding is completed, the small balls are taken out and placed in an oven at 70° C. to dry for 6 hours to prepare polymer small balls, namely the polyacrylate microsphere material.

[0116] Example 4

[0117] This embodiment provides a polyacrylate microsphere material, which is prepared by a drop ball forming method comprising the following specific steps:

[0118] Step 1: Weigh 9.8g of tert-butyl acrylate, 1.4g of tert-butyl methacrylate and 5.7g of trimethylolpropane triacrylate and add them to a mixture of cyclohexane and ethyl acetate accounting for 55% of the total volume of the organic phase, then add 2.6g of span20, 1.2g of BPO and 0.7g of p-nonylphenol in sequence, and then ultrasonicate in an ultrasonic cleaner for 7 minutes to dissolve and mix evenly to obtain a uniform organic phase;

[0119] Step 2: Weigh a certain amount of deionized water (accounting for 60% of the total volume of the fully emulsified emulsion) as the water phase, put the dissolved oil phase, i.e., the uniform organic phase, in an ice bath, and slowly drop the water phase into the oil phase at a high-speed stirrer at a speed of 3000 r / min. After the drop is completed, increase the speed to 6000 r / min and stir for 8 minutes to fully emulsify, then add 2.6 g of reducing agent N,N-dimethylaniline, and continue stirring for 1 minute to obtain a formed emulsion;

[0120] Step 3: Using a drop ball forming device to perform drop ball forming and aging on the formed emulsion, wherein the structure diagram of the drop ball forming device is as follows: Figure 1 As shown, from Figure 1It can be seen that the drop ball forming device includes: a forming emulsion storage tank 1, a peristaltic pump 2 and a forming column 4 with a height of 1.7m, the forming column 4 is a jacketed glass tube with openings at both ends, a mechanical stirring device 5 is set up at the upper end opening of the jacketed glass tube, a double crescent-shaped stirring paddle 51 is arranged in the mechanical stirring device 5, and an embedded drip tray 3 is sealed at the lower end opening of the jacketed glass tube, and the embedded drip tray 3 is provided with a plurality of drop ball forming needles 31 that can extend into the forming column 4;

[0121] The outlet of the forming emulsion storage tank 1 is connected to the inlet of the embedded drip tray 3 through a pipeline via a peristaltic pump 2;

[0122] Therefore, the drop ball forming and aging of the formed emulsion using the drop ball forming device as shown above specifically includes:

[0123] Prepare an aqueous solution 6 of a dispersant, which in this embodiment is an aqueous solution of polyvinyl alcohol (PVA) with a mass concentration of 1.5%, and add it to a jacketed glass tube and a mechanical stirring device 5, while ensuring that the double crescent-shaped stirring paddle 51 is located below the liquid surface of the aqueous solution of polyvinyl alcohol (PVA), and then heat it to 70° C. by connecting a water bath device through the jacket;

[0124] The molding emulsion is transported to the embedded drip tray by a peristaltic pump and dripped into the jacketed glass tube by a ball-drop molding needle (with an inner diameter of 0.51 mm). The molding emulsion droplets in the jacketed glass tube continuously float up. During the floating process, the molding emulsion droplets form a sphere under the action of the surface tension in the water and undergo polymerization reaction and preliminary solidification. When the preliminary solidified small ball floats to the upper part of the jacketed glass tube, close to the liquid surface position of the aqueous solution of polyvinyl alcohol (PVA), it will continue to rotate and stay in the aqueous solution of polyvinyl alcohol under the action of mechanical stirring (rotation speed of 200 r / min) of the double crescent-shaped stirring paddle 51 and undergo sufficient polymerization reaction to ensure complete molding;

[0125] After the molding is completed, the small balls are taken out and placed in an oven at 70° C. to dry for 6 hours to prepare polymer small balls, namely the polyacrylate microsphere material.

[0126] Example 5

[0127] This embodiment provides a polyacrylate microsphere material, which is prepared by a drop ball forming method comprising the following specific steps:

[0128] Step 1: Weigh 10g of tert-butyl acrylate, 4.3g of tert-butyl methacrylate and 10g of trimethylolpropane triacrylate and add them to a mixture of cyclohexane and ethyl acetate accounting for 60% of the total volume of the organic phase, then add a combined emulsifier formed by 2.8g of P123 and 2.0g of span80, 2.4g of BPO and a combined co-emulsifier formed by 0.7g of hexadecanol and 0.5g of hexanol, and then ultrasonicate in an ultrasonic cleaner for 10 minutes to dissolve and mix evenly to obtain a uniform organic phase;

[0129] Step 2: Weigh a certain amount of deionized water (accounting for 65% of the total volume of the fully emulsified emulsion) as the water phase, put the dissolved oil phase, i.e., the uniform organic phase, in an ice bath, and slowly drop the water phase into the oil phase at a high-speed stirrer at a speed of 3000 r / min. After the drop is completed, increase the speed to 5000 r / min and stir for 10 minutes to fully emulsify, then add 4.8 g of a combined reducing agent (i.e., 2.4 g of N,N,N,N-tetramethylethylenediamine and 2.4 g of sodium sulfite), and continue stirring for 1 minute to obtain a formed emulsion;

[0130] Step 3: Using a drop ball forming device to perform drop ball forming and aging on the formed emulsion, wherein the structure diagram of the drop ball forming device is as follows: Figure 1 As shown, from Figure 1 It can be seen that the drop ball forming device includes: a forming emulsion storage tank 1, a peristaltic pump 2 and a forming column 4 with a height of 1.7m, the forming column 4 is a jacketed glass tube with openings at both ends, a mechanical stirring device 5 is set up at the upper end opening of the jacketed glass tube, a cross-type stirring paddle 51 is arranged in the mechanical stirring device 5, and an embedded drip tray 3 is sealed at the lower end opening of the jacketed glass tube, and the embedded drip tray 3 is provided with a plurality of drop ball forming needles 31 that can extend into the forming column 4;

[0131] The outlet of the forming emulsion storage tank 1 is connected to the inlet of the embedded drip tray 3 through a pipeline via a peristaltic pump 2;

[0132] Therefore, the drop ball forming and aging of the formed emulsion using the drop ball forming device as shown above specifically includes:

[0133] Prepare an aqueous solution 6 of a dispersant, which in this embodiment is an aqueous solution of polyethylene glycol with a mass concentration of 2.0%, and add it into a jacketed glass tube and a mechanical stirring device 5, while ensuring that a cross-type stirring paddle 51 is below the liquid surface of the aqueous solution of polyethylene glycol, and then heat it to 80° C. by connecting a water bath device through the jacket;

[0134] The molding emulsion is transported to the embedded drip tray by a peristaltic pump and dripped into the jacketed glass tube by a ball-dropping molding needle (with an inner diameter of 0.6 mm). The molding emulsion droplets in the jacketed glass tube continuously float up. During the floating process, the molding emulsion droplets form a sphere under the action of the surface tension in the water and undergo polymerization reaction and preliminary solidification. When the preliminary solidified small ball floats to the upper part of the jacketed glass tube, close to the liquid surface position of the polyethylene glycol aqueous solution, it will continue to rotate and stay in the polyethylene glycol aqueous solution under the action of mechanical stirring (rotation speed of 300 r / min) by a cross-type stirring paddle 51 and undergo sufficient polymerization reaction to ensure complete molding;

[0135] After the molding is completed, the small balls are taken out and placed in an oven at 80° C. to dry for 4 hours to prepare polymer small balls, namely the polyacrylate microsphere material.

[0136] Comparative Example 1

[0137] This comparative example provides a polyacrylate material, which is also prepared by a drop ball forming method. The difference between this comparative example and Example 1 is only that:

[0138] Deionized water accounts for 30% of the total volume of the emulsion obtained by full emulsification.

[0139] Comparative Example 2

[0140] This comparative example provides a polyacrylate material, which is also prepared by a drop ball forming method. The difference between this comparative example and Example 2 is only that:

[0141] The forming emulsion is prepared in a room temperature environment instead of a low temperature environment, that is, the dissolved oil phase, i.e. the uniform organic phase, is not placed in an ice bath.

[0142] Comparative Example 3

[0143] This comparative example provides a polyacrylate material, which is also prepared by a drop ball forming method. The difference between this comparative example and Example 3 is only that:

[0144] There is no mechanical stirring device installed above the forming column.

[0145] Comparative Example 4

[0146] This comparative example provides a polyacrylate material, which is also prepared by a drop ball forming method. The difference between this comparative example and Example 4 is only that:

[0147] The molding liquid added to the molding column is pure water, not a PVA aqueous solution.

[0148] Comparative Example 5A

[0149] This comparative example provides a polyacrylate material, which is also prepared by a drop ball forming method. The difference between this comparative example and Example 5 is only that:

[0150] The jacket of the molding column is connected to a water bath and heated to 40°C.

[0151] Comparative Example 5B

[0152] This comparative example provides a polyacrylate material, which is also prepared by a drop ball forming method. The difference between this comparative example and Example 5 is only that:

[0153] The jacket of the molding column is connected to a water bath and heated to 90°C.

[0154] Comparative Example 6

[0155] This comparative example provides a polyacrylic acid sphere material, which is prepared by an emulsion suspension polymerization method comprising the following specific steps, specifically comprising:

[0156] Step 1: Weigh 10g of tert-butyl acrylate, 2.5g of tert-butyl methacrylate and 10g of trimethylolpropane triacrylate, add toluene accounting for 40% of the total volume of the organic phase, then add 1.2g of P123, 0.3g of benzoyl peroxide (BPO) and 0.3g of hexadecanol in sequence, and then ultrasonicate in an ultrasonic cleaner for 5min to dissolve and mix evenly to obtain a uniform organic phase;

[0157] Step 2: Weigh a certain amount of deionized water (accounting for 45% of the total volume of the fully emulsified emulsion) as the water phase, put the dissolved oil phase, i.e., the uniform organic phase, in an ice bath, and slowly drop the water phase into the oil phase at a high-speed stirrer at a speed of 1000 r / min. After the drop is completed, increase the speed to 9000 r / min and stir for 5 minutes to fully emulsify, then add 1.2 g of reducing agent N, N-dimethylaniline and continue stirring for 2 minutes to obtain a formed emulsion;

[0158] Step 3: Measure 150 mL of water and add it to a 250 mL three-necked flask and add 0.15 g of ammonium persulfate and 1.5 mL of polyvinyl alcohol dispersant. Stir with an electric stirrer at a speed of 300 rpm and heat in a constant temperature water bath at 45°C; after the temperature is kept constant for 10 minutes, add the prepared molding emulsion to the above three-necked flask. Under the action of its own interfacial tension, the molding emulsion will be dispersed into spheres. After continuing to stir for 10 minutes, take out the small balls and put them in an oven at 60°C to dry for 6 hours to prepare macroporous polymer balls, i.e., polyacrylate materials.

[0159] The appearance of the polyacrylate microsphere materials prepared in Examples 1 to 5 of the present invention is basically the same, and they are all regular spherical particles. Here, only the appearance pictures of the polyacrylate microsphere materials prepared in Examples 2 and 5 are provided, as shown respectively. Figure 2 and Figure 3 shown.

[0160] The physical pictures of the polyacrylate microsphere materials provided in Comparative Example 1, Comparative Example 5A and Comparative Example 5B are as follows: Figure 4-Figure 6 As shown. Figure 4-Figure 6 It can be seen that the appearances of the polyacrylate microsphere materials provided in Comparative Example 1, Comparative Example 5A and Comparative Example 5B are quite different, and most of them are ellipsoidal or irregularly shaped particles with poor sphericity.

[0161] In addition, the scanning electron microscope image of the polyacrylate microsphere material prepared in Example 1 of the present invention is as follows: Figure 7 and Figure 8 As shown. Figure 7 and Figure 8 It can be seen from the internal details of the polyacrylate microsphere material that there are a large number of macroporous structures inside.

[0162] In addition, the molding effects of Examples 1 to 5 and Comparative Examples 1 to 6 of the present invention, the bulk density and mechanical strength of the prepared polyacrylate microsphere materials or polyacrylate material samples are shown in Table 1 below.

[0163] Table 1

[0164]

[0165] From the molding effect data shown in Table 1 above, it can be seen that the yields of Examples 1 to 5 of the present invention are all above 60%, the molding effect is good, and the particle size is uniform (the higher the yield, the more uniform the particle size), and a polyacrylate microsphere material with a lower bulk density that is suitable for the fluidized bed process can be obtained.

[0166] Among them, in Comparative Example 1, due to the reduced proportion of deionized water, the viscosity of the formed emulsion is large, the formed emulsion droplets are prone to stringing and tailing, and are difficult to form balls, and the yield is reduced to 20%, indicating that in order to ensure a good molding effect, the water phase should not be too small in the total volume of the emulsion.

[0167] In Comparative Example 2, the molding emulsion was not prepared in a low-temperature environment, resulting in the molding emulsion quickly polymerizing into a solid before molding, which made further molding impossible. This indicates that the molding emulsion should be prepared in a low-temperature environment to prolong its polymerization time.

[0168] In comparative example 3, no mechanical stirring device is installed above the molding column, resulting in the molding emulsion droplets being unable to stay in the molding liquid, i.e., the aqueous solution of polyvinyl alcohol, for a sufficiently long time. They float to the surface of the molding liquid and rupture before being solidified. This indicates that a mechanical stirring device must be installed above the molding column during the molding emulsion droplet molding process to ensure that the molding emulsion droplets are completely solidified in the molding liquid.

[0169] In Comparative Example 4, the molding liquid added to the molding column is pure water. Since no polyvinyl alcohol dispersant is added, the molding emulsion droplets are prone to adhesion during the polymerization process, which greatly reduces the yield. This shows that a certain concentration of dispersant must be added to the molding liquid to ensure that the molding emulsion droplets are smoothly formed and maintain good dispersion.

[0170] Comparative Example 5A and Comparative Example 5B respectively investigated the appropriate molding temperature range. From the results shown in Table 1 above, it can be seen that when the molding temperature is too low, the polymerization and solidification speed of the molded emulsion droplets slows down, and they are still in a droplet state without hardness when rising to the mechanical stirring device, and are easily broken by the stirring paddle, and the particle size is reduced; when the molding temperature is too high, part of the organic phase in the molded emulsion droplets reaches the boiling point and escapes in the form of gas, resulting in the deterioration of the sphericity of the final small balls, such as Figure 5-Figure 6 As shown, therefore, the molding temperature should be controlled at 50-80℃.

[0171] Comparative Example 6 adopts the traditional emulsion suspension polymerization method to prepare the polyacrylate microsphere material sample. The results show that its yield is only 38%. Compared with Comparative Example 6, the yield in Example 4 is increased by as much as 42%, indicating that the drop ball forming method provided by the present invention can effectively improve the yield of the small ball carrier and ensure good sphericity.

[0172] It can also be seen from Table 1 above that the polyacrylate microsphere materials prepared in Examples 1 to 5 of the present invention all have higher mechanical strength. Compared with the currently used emulsion suspension polymerization method, the mechanical strength of the polyacrylate microsphere materials can be increased by more than 15%, and they are not easily worn during fluidized bed operation.

[0173] Application Examples

[0174] In order to further evaluate the performance of the polyacrylate microsphere material samples prepared in the embodiments and comparative examples of the present invention as solid adsorbent carriers for fluidized bed CO2 adsorption, this application example adopts a physical impregnation method to load a certain amount of organic amine on the polyacrylate microsphere material samples prepared in Examples 1-5 and Comparative Examples 1-6 of the present invention and evaluate their adsorption performance. The specific loading steps are: weigh 2g of the polyacrylate microsphere material samples prepared in Examples 1-5 and Comparative Examples 1-6, respectively, and place them in a round-bottom flask, add 15g of pentaethylenehexamine, and use a rotary evaporator to rotate and impregnate for 6h at a temperature of 60°C. After the impregnation, wash with a small amount of alcohol, and then dry at a temperature of 40°C for 10h. Finally, the CO2 adsorption capacity of the polyacrylate microsphere material samples loaded with pentaethylenehexamine at a temperature of 25°C and a pressure of 1 bar was tested using a physical adsorption instrument, and the specific results are shown in Table 2 below.

[0175] Table 2

[0176] project Adsorption capacity (mmol / g) project Adsorption capacity (mmol / g) Example 1 3.8 Comparative Example 1 1.9 Example 2 3.5 Comparative Example 2 Unformed Example 3 3.6 Comparative Example 3 Unformed Example 4 3.3 Comparative Example 4 1.1 Example 5 3.2 Comparative Example 5A 2.1 Comparative Example 5B 2.6 Comparative Example 6 3.1

[0177] It can be seen from Table 2 above that under the same conditions, the CO2 adsorption capacity of the polyacrylate microsphere material sample prepared in the embodiment of the present invention as a solid adsorbent carrier for fluidized bed CO2 adsorption is significantly higher than that of the polyacrylate microsphere material sample prepared in the comparative example, indicating that the polyacrylate microsphere material sample prepared by the drop ball molding method provided by the present invention has more excellent CO2 adsorption performance.

[0178] The above is only a specific embodiment of the present invention, and cannot be used to limit the scope of the invention. Therefore, the replacement of equivalent components, or equivalent changes and modifications made according to the protection scope of the patent of the present invention, should still fall within the scope of this patent. In addition, the technical features of the present invention can be freely combined with each other, with each other and with each other, and with each other.

Claims

1. A drop ball forming method of polyacrylate microsphere material, characterized in that: The drop ball forming method of the polyacrylate microsphere material comprises: Step 1: First, two or three organic monomers are added to the organic dispersed phase, and then an emulsifier, an initiator and an emulsifier are added in sequence to form a uniform organic phase; Step 2: adding deionized water dropwise into the organic phase for full emulsification and then adding a reducing agent to obtain a formed emulsion; Step three: using a drop ball forming device to perform drop ball forming and aging on the formed latex, and then drying the aged small balls to obtain the polyacrylate microsphere material.

2. The drop ball forming method according to claim 1, characterized in that: The organic monomers include two or three organic monomers selected from the group consisting of glycidyl methacrylate, methyl methacrylate, ethyl methacrylate, methyl acrylate, ethyl acrylate, styrene, ethylene glycol dimethacrylate, tert-butyl acrylate, tert-butyl methacrylate and trimethylolpropane triacrylate.

3. The drop ball forming method according to claim 2, characterized in that: The organic monomers include tert-butyl acrylate, tert-butyl methacrylate and trimethylolpropane triacrylate in a mass ratio of 2-3.5:0.5-1.5:2-3.

5.

4. The drop ball forming method according to claim 1, characterized in that: Taking the total volume of the organic phase as 100%, the volume fraction of the organic dispersed phase is 40-60%.

5. The drop ball forming method according to claim 1 or 4, characterized in that: The organic dispersed phase includes one or a combination of cyclohexane, toluene, carbon tetrachloride, dichloromethane, 1-2-dichloroethane, and ethyl acetate; preferably, one or a combination of toluene, cyclohexane, and ethyl acetate.

6. The drop ball forming method according to any one of claims 1 to 3, characterized in that: Based on the total weight of the two or three organic monomers being 100%, the amounts of the emulsifier, the initiator and the co-emulsifier are 5-20%, 1-10% and 1-5% respectively.

7. The drop ball forming method according to claim 6, characterized in that: The emulsifier includes one or a combination of span80, span60, span20, and a polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer.

8. The drop ball forming method according to claim 6, characterized in that: The initiator includes one or a combination of ammonium persulfate, potassium persulfate, benzoyl peroxide, dicumyl peroxide, tert-butyl peroxide, azobisisobutyronitrile, and azobisisovaleronitrile.

9. The drop ball forming method according to claim 6, characterized in that: The auxiliary emulsifier includes one or a combination of hexadecanol, hexanol, octanol, and p-nonylphenol.

10. The drop ball forming method according to claim 1, characterized in that: Deionized water is dripped into the organic phase to fully emulsify the phase so that the deionized water accounts for 45-65% of the total volume of the emulsion obtained after full emulsification.

11. The drop ball forming method according to claim 1, characterized in that: Based on the total weight of the two or three organic monomers being 100%, the amount of the reducing agent used is 5-20%.

12. The drop ball forming method according to claim 1 or 11, characterized in that: The reducing agent includes one or a combination of N,N-dimethylaniline, N,N,N,N-tetramethylethylenediamine, ferrous sulfate, and sodium sulfite.

13. The drop ball forming method according to claim 1, characterized in that: The entire step 2 is carried out in a low temperature environment to reduce the temperature of the formed emulsion to below 5°C.

14. The drop ball forming method according to claim 1, characterized in that: The drop ball forming device comprises a forming emulsion storage tank, a peristaltic pump and a forming column, wherein the forming column is a jacketed glass tube with openings at both ends, a mechanical stirring device is mounted at the upper opening of the jacketed glass tube, a stirring paddle is arranged in the mechanical stirring device, and an embedded drip tray is sealed at the lower opening of the jacketed glass tube, wherein the embedded drip tray is provided with a plurality of drop ball forming needles that can extend into the forming column; The outlet of the forming emulsion storage tank is connected to the inlet of the embedded drip tray through a pipeline via a peristaltic pump.

15. The drop ball forming method according to claim 1 or 14, characterized in that: In step 3, using a drop ball forming device to perform drop ball forming and aging on the formed emulsion comprises: Add an aqueous solution of a dispersant into the jacketed glass tube and heat it to 50-80°C by connecting a water bath to the jacket; The molding emulsion is transported to the embedded drip tray by a peristaltic pump and dripped into the jacketed glass tube through a ball-drop molding needle. The molding emulsion droplets in the jacketed glass tube continuously float up. During the floating process, the molding emulsion droplets form a sphere under the action of the surface tension in the water and undergo polymerization reaction and initial solidification. When the initially solidified small balls float to the upper part of the jacketed glass tube, they will continue to rotate and stay in the aqueous solution of the dispersant under the action of mechanical stirring and undergo sufficient polymerization reaction to ensure complete molding.

16. The drop ball forming method according to claim 15, characterized in that: The mass concentration of the aqueous solution of the dispersant is 0.3-2.0%; Preferably, the dispersant comprises polyvinyl alcohol and / or polyethylene glycol.

17. The drop ball forming method according to claim 15, characterized in that: The height of the jacketed glass tube is 1-2 m; preferably, the inner diameter of the drop ball forming needle is 0.2-0.6 mm; also preferably, the rotation speed of the mechanical stirring is 100-300 r / min.

18. A polyacrylate microsphere material, characterized in that: The polyacrylate microsphere material is prepared by the drop ball forming method of the polyacrylate microsphere material according to any one of claims 1 to 17; Preferably, the particle size of the polyacrylate microsphere material is 0.40-0.85 mm, and the bulk density is 0.10-0.20 g / mL.

19. Use of the polyacrylate microsphere material according to claim 18 as a solid adsorbent carrier for fluidized bed CO2 adsorption.

20. A fluidized bed CO2 solid adsorbent, comprising a solid adsorption carrier and an adsorption active component loaded on the surface of the solid adsorption carrier, characterized in that: The solid adsorption carrier is the polyacrylate microsphere material as described in claim 18.

Citation Information

Patent Citations

  • Hydrophilic modification method of polystyrene material and product thereof

    CN106589201A

  • Polyacrylate composite material for CO2 adsorption and preparation method of polyacrylate composite material

    CN111825796A

  • Preparation method of hydrophilic polyacrylate crosslinked microspheres

    CN114213581A

  • ALF composite material for CO2 capture and preparation method thereof

    CN115814769A

  • Dropping ball forming experimental device used for preparing spherical carriers

    CN204247160U