Zirconium alloy coating manufacturing method, zirconium alloy coating and anti-corrosion method

By forming a supersaturated solid solution zirconium alloy coating on the surface of the zirconium alloy matrix, the PVD process and reinforcement elements are used to solve the phase transition problem of zirconium oxide layer of zirconium alloy, and its corrosion resistance and wear resistance are significantly improved.

CN119082686APending Publication Date: 2024-12-06SHANGHAI NUCLEAR ENGINEERING RESEARCH & DESIGN INSTITUTE CO LTD +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411226840.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Under high temperature conditions, the zirconium oxide layer of zirconium alloy is prone to phase change and cause rupture, which affects its wear resistance and corrosion resistance. The addition of existing alloy elements has low solubility or precipitation problems, making it difficult to effectively stabilize the zirconium oxide layer.

Method used

The PVD process is used to deposit the surface of the zirconium alloy matrix to form a supersaturated solid solution zirconium alloy coating with Zr as the matrix, and the content of reinforced elements such as Nb, V, Cu, Fe, Cr, Y, Si, Mo is between 1% and 50%. , a stable zirconia layer is formed by magnetron sputtering or multi-arc ion plating process to inhibit the zirconia phase transition.

Benefits of technology

It effectively improves the stability and service life of the zirconia layer, avoids the decline in mechanical properties caused by the precipitation of reinforced elements, and significantly improves the corrosion and wear resistance of zirconium alloys.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119082686A_ABST
    Figure CN119082686A_ABST
Patent Text Reader

Abstract

A zirconium alloy coating manufacturing method comprises the following steps that a coating-containing target material is provided, and the coating-containing target material comprises one or more of Nb, V, Cu, Fe, Cr, Y, Si and Mo and a Zr element; a zirconium alloy coating is deposited on the surface of a matrix part through the PVD technology, the supersaturated solid solution zirconium alloy coating with Zr as the matrix is obtained, the weight ratio of strengthening elements in the zirconium alloy coating is 1%-50%, and at least one strengthening element is not less than 1%. According to the method, the zirconium alloy supersaturated solid solution coating is formed through the PVD technology, mechanical property and corrosion resistance loss caused by precipitation of alloy elements in the zirconium alloy is effectively avoided, zirconium oxide phase change under the high-temperature condition is inhibited through the alloy elements, and therefore the corrosion resistance and wear resistance of a workpiece are improved. The invention further provides a zirconium alloy coating and an anti-corrosion method.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of corrosion protection, and in particular relates to a zirconium alloy coating manufacturing method, a zirconium alloy coating and an corrosion protection method. Background Art

[0002] Zirconium alloy has the advantages of high strength and corrosion resistance, as well as good neutron permeability. Therefore, it is widely used in the manufacture of important equipment such as fuel assemblies in the nuclear industry. Under high temperature conditions, a dense zirconium oxide layer is easily formed on the surface of zirconium alloy to prevent further oxidation, thereby improving the wear resistance and corrosion resistance of zirconium alloy. However, zirconium oxide undergoes phase change at around 1100°C and is accompanied by a relatively significant volume strain. In this process, the zirconium oxide layer is easily broken, resulting in the loss of zirconium alloy performance. In order to improve the performance of the zirconium oxide layer and reduce or avoid cracking caused by phase change, in some technical solutions, the alloy is modified by adding elements such as Sn, Nb, Fe, and Cr to the zirconium alloy to stabilize the zirconium oxide structure and improve the strength of zirconium oxide. However, since these alloy elements usually have very low solubility in zirconium alloys, they are easy to form intermetallic compounds and precipitate from the zirconium alloy matrix, which has an adverse effect on the mechanical properties and corrosion resistance of the zirconium alloy. Therefore, a method for manufacturing a zirconium alloy coating is provided through a surface modification process to improve the wear resistance and corrosion resistance of the zirconium alloy, which has a positive significance for improving the comprehensive performance of the zirconium alloy. Summary of the invention

[0003] The purpose of the present invention is to provide a method for manufacturing a zirconium alloy coating to improve the corrosion resistance and wear resistance of the zirconium alloy. The present invention also provides a zirconium alloy coating and an anti-corrosion method.

[0004] According to an embodiment of one aspect of the present invention, a method for manufacturing a zirconium alloy coating is provided, the method comprising the following steps:

[0005] Step a): providing a substrate member and a coating target, wherein the coating target comprises Zr and a strengthening element, wherein the strengthening element comprises one or more of Nb, V, Cu, Fe, Cr, Y, Si, and Mo;

[0006] Step b): adopting a PVD process to deposit the coating target on the surface of the substrate to form a zirconium alloy coating, wherein the mass percentage of the strengthening elements in the zirconium alloy coating is 1%-50%, and at least one of the strengthening elements is not less than 1%; the structure of the zirconium alloy coating is a supersaturated solid solution with Zr as the matrix.

[0007] This method deposits a supersaturated solid solution of Zr on the surface of the substrate through the PVD process. After the zirconium alloy coating is oxidized, the strengthening elements in the coating can effectively improve the stability of zirconium oxide and inhibit the phase change of zirconium oxide, thereby achieving the effect of improving the stability and service life of the dense zirconium oxide layer. At the same time, since the supersaturated solid solution is formed through the PVD process, the strengthening elements in the coating are not easy to precipitate in the form of intermetallic compounds, thereby improving the strength and durability of the coating.

[0008] Furthermore, in some embodiments, in the step a), the target material includes a plurality of single-component targets, and the element purity of each of the single-component targets is not less than 99.5%.

[0009] Furthermore, in some embodiments, in the step a), the target material is an alloy target material, the alloy target material includes Zr and the strengthening element, and the composition ratio of the alloy target material is the same as that of the zirconium alloy coating.

[0010] Furthermore, in some embodiments, in the step b), the PVD process includes magnetron sputtering or multi-arc ion plating.

[0011] Further, in some embodiments, in step b), the PVD process is configured as magnetron sputtering, and includes the following steps: providing an equipment chamber, placing the substrate component into the equipment chamber and evacuating the chamber to a vacuum of no more than 8×10 -3 Pa, filling with argon to 0.1Pa-1Pa; applying a bias voltage of -30V to -300V to the substrate component, and energizing the coating target to deposit the coating; after the zirconium alloy coating is deposited to a given thickness, cooling it, and taking the substrate component out of the equipment cavity.

[0012] Furthermore, in some embodiments, before coating deposition, the step of ion cleaning the substrate component is also included. In the ion cleaning step, a bias voltage of -400V to -800V is first applied to the substrate component to ionize the argon gas and bombard the substrate component, and the ion cleaning is completed for 5 minutes to 60 minutes.

[0013] Furthermore, in some embodiments, when the coating is deposited, the electric power supplied to the coating target is 1w / cm 2 -5w / cm 2 .

[0014] According to an embodiment of another aspect of the present invention, there is provided a zirconium alloy coating, which comprises a Zr matrix and strengthening elements, wherein the strengthening elements comprise one or more of Nb, V, Cu, Fe, Cr, Y, Si, and Mo, and the strengthening elements account for 1%-50% by weight; the structure of the zirconium alloy coating is a supersaturated solid solution with Zr as the matrix; the zirconium alloy coating is manufactured by the zirconium alloy coating manufacturing method provided in any of the aforementioned embodiments.

[0015] According to another embodiment of the present invention, an anti-corrosion method is provided, wherein a zirconium alloy coating is applied to the surface of a substrate member that needs to be treated for anti-corrosion to improve the corrosion resistance. The zirconium alloy coating is manufactured using the zirconium alloy coating manufacturing method provided in any of the above embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 A comparison diagram of weight gain curves of an embodiment and a comparative water corrosion test;

[0017] Figure 2 FIG. 1 is a schematic diagram of X-ray diffraction analysis results in one embodiment.

[0018] The purpose of the above drawings is to explain the present invention in detail so that those skilled in the art can understand the technical concept of the present invention, but it is not intended to limit the present invention. DETAILED DESCRIPTION

[0019] The present invention is further described in detail below through specific embodiments in conjunction with the accompanying drawings.

[0020] Reference to "embodiment" herein means that a particular feature, structure or characteristic described in conjunction with the embodiment may be included in at least one embodiment of the present invention. The phrase appearing in various locations in the specification does not necessarily refer to the same embodiment, nor is it limited to mutually exclusive independent or alternative embodiments. It should be understood by those skilled in the art that the embodiments herein may be combined with other embodiments without structural conflicts. In the description herein, "multiple" means at least two.

[0021] Zirconium alloys have the advantages of high strength and corrosion resistance, as well as good neutron permeability. Therefore, they are widely used in the nuclear industry and have become the preferred material for the manufacture of important structural parts such as pressurized water reactor fuel assemblies. In a high-temperature oxidizing environment, such as a high-temperature water environment, a water vapor environment, or an oxygen-containing atmosphere, a dense zirconium oxide layer will form on the surface of the zirconium alloy. The dense zirconium oxide layer can effectively prevent the further development of the oxidation reaction, thereby achieving a good anti-corrosion effect. At the same time, the high hardness of zirconium oxide also improves the wear resistance of zirconium alloy parts, which helps to increase the service life of zirconium alloy parts in application scenarios with friction, such as being used to manufacture fuel rod fixtures with flow-induced vibrations.

[0022] The crystal form of zirconium oxide has different lattice structures such as monoclinic, tetragonal and cubic. The stability of these different zirconium oxide phases at different temperatures is also different. The primary zirconium oxide on the surface of zirconium alloy is a tetragonal structure, which appears as a black and shiny film. Below 1100°C, tetragonal zirconium oxide is a metastable phase. Therefore, when the temperature rises and the oxidation process further develops, tetragonal zirconium oxide tends to transform into a more stable monoclinic zirconium oxide, which is grayish white or white in macroscopic appearance. During this phase change process, zirconium oxide has significant volume strain, which can easily cause the originally dense zirconium oxide layer to crack due to stress-strain incoordination, resulting in loss of wear resistance and corrosion resistance.

[0023] In order to inhibit the phase transformation of zirconium oxide, some existing technical solutions modify zirconium alloys by adding alloying elements such as Sn, Nb, Fe, and Cr during the smelting process of zirconium alloys. When the modified zirconium alloy is oxidized, the alloying elements will enter the lattice of zirconium oxide, which will stabilize the tetragonal zirconium oxide and regulate the defect concentration of zirconium oxide, thereby further improving the strength of zirconium oxide and improving the corrosion resistance and wear resistance of zirconium alloys. However, the solubility of the above alloying elements in the zirconium alloy matrix is ​​very low. For example, the solubility of Nb in α-Zr is less than 0.6%, the solubility of Cr and Cu in α-Zr is less than 0.15%, and the solubility of Fe and Si in α-Zr is less than 0.02%. When the amount of alloying elements added is low, it cannot stabilize and strengthen zirconium oxide; and when the amount of alloying elements added is high, the alloying elements exceeding the upper limit of solid solubility are easy to form precipitation phases in the zirconium alloy matrix in the form of intermetallic compounds, which have an adverse effect on the mechanical properties and corrosion resistance of the zirconium alloy matrix. Therefore, there are insurmountable technical difficulties in further optimizing and improving the corrosion resistance of zirconium alloys only by alloying.

[0024] In order to solve the above problems, an embodiment of one aspect of the present invention provides a method for manufacturing a zirconium alloy coating, which forms a supersaturated solid solution of zirconium alloy on the surface of a substrate to be strengthened by deposition, so as to overcome the problem that alloy components in the zirconium alloy substrate are prone to precipitation under conventional metallurgical processes. The method specifically comprises the following steps:

[0025] First, a substrate component and a coating target to be strengthened are provided. The substrate component may be a zirconium alloy component, or other metal material component with good compatibility with zirconium alloy, or a ceramic material component or a polymer material component. The coating target includes Zr and strengthening elements, wherein the strengthening elements include one or a combination of Nb, V, Cu, Fe, Cr, Y, Si, and Mo. In different embodiments, the coating target may be a single component target with a purity of not less than 99.5%, or Zr and strengthening elements may be prepared into an alloy target in advance by smelting or powder metallurgy according to the composition ratio of the zirconium alloy coating.

[0026] Next, a PVD process is used to deposit a zirconium alloy coating on the surface of the substrate using a coating target. The weight percentage of strengthening elements in the zirconium alloy coating is 1%-50%, and the weight percentage of at least one strengthening element is not less than 1%, forming a supersaturated solid solution with Zr as the matrix. The coating thickness can be from a few nanometers to hundreds of microns according to specific needs. According to the research experience of the present invention, when the content of strengthening elements is too low, the phase transformation of zirconium oxide cannot be effectively suppressed.

[0027] In different embodiments, the PVD process may be a magnetron sputtering process or a multi-arc ion plating process.

[0028] In a preferred embodiment, the zirconium alloy coating is prepared by magnetron sputtering. First, the surface of the substrate is cleaned to remove oil, dust, loose oxide layer, etc., and the substrate is dried. The substrate is hung or clamped on the rotating frame of the magnetron sputtering equipment to keep the substrate installed stably, and the area of ​​the substrate that needs to be coated can be fully exposed to the front of the target during the rotation process. The equipment chamber is evacuated to less than 8×10 -3Pa, in order to avoid air interference with the coating composition. In a further preferred embodiment, the substrate is first ion cleaned before deposition: argon gas is introduced to stabilize the vacuum degree at 0.1Pa-1Pa, and a bias voltage of -400V to -800V is applied to the equipment turret to ionize the argon gas. The argon ions continuously bombard the surface of the substrate, and the ion cleaning is completed for 5min-60min to further improve the cleanliness of the surface of the substrate. After the ion cleaning is completed, the vacuum degree of 0.1Pa-1Pa is maintained, and a bias voltage of -30V to -300V is applied to the substrate through the equipment turret. At the same time, the target material is energized to deposit the coating. In different embodiments, the target material can be a plurality of target materials including a pure Zr target and a pure strengthening element target, or it can be an alloy target material containing Zr and strengthening elements pre-manufactured according to the target zirconium alloy coating composition; the target material power supply can be set at 1w / cm 2 -5w / cm 2 After the zirconium alloy target material is deposited to a given thickness, the power is turned off, and the substrate is cooled to below 60°C and then taken out of the equipment cavity to complete the manufacture of the zirconium alloy coating.

[0029] The zirconium alloy coating manufactured by this method has a supersaturated solid solution with Zr as the matrix. Since the various element components are rapidly cooled on the surface of the matrix component during the deposition process, the migration distance of the strengthening elements in the Zr matrix is ​​limited, and the intermetallic compound precipitation phase commonly present in the molten alloy will not appear, so the supersaturated solid solution zirconium alloy coating can maintain good mechanical properties and corrosion resistance. During the oxidation process, the strengthening elements in the coating can effectively stabilize the tetragonal zirconium oxide, inhibit the phase change of zirconium oxide, and prevent the zirconium oxide layer from being damaged due to phase change.

[0030] Through this method, zirconium alloy parts or other metal or non-metal parts can be treated for corrosion resistance, effectively improving the corrosion resistance and wear resistance of the base parts and increasing the service life of the base parts.

[0031] In a comparative example, a pure zirconium sheet was melted as a target material.

[0032] The coating preparation process is as follows: using chrome-gold as the base workpiece, the chrome alloy sheet is suspended on the rotating frame of the magnetron sputtering equipment and the contact is ensured to be stable. The equipment chamber is evacuated to a vacuum of less than 8×10 -3 Pa, ensure that the air is fully exhausted; fill with argon, adjust the vacuum degree to 0.5Pa, and then apply a -400V bias voltage to the turntable where the substrate is located, and perform ion cleaning for 30 minutes; then adjust the vacuum degree to 0.1Pa, apply a -30V bias voltage to the chromium alloy sheet, and energize the pure zirconium sheet target to deposit the coating. The deposition time is controlled to 30h to obtain a pure Zr coating with a thickness of 10μm. Wait for the chromium alloy sheet to cool to below 60℃ and take it out.

[0033] X-ray diffraction analysis shows that the coating structure is α-Zr.

[0034] In one embodiment, a Zr-Nb alloy with a Nb content of 2% is smelted as a target material, and the Nb element in the target material mainly exists in the form of β-Nb intergranular precipitation phase.

[0035] The coating preparation process is as follows: Using chromium alloy as the base workpiece, the chromium alloy sheet is suspended on the rotating frame of the magnetron sputtering equipment and the contact is ensured to be stable. The equipment cavity is evacuated to less than 8×10 -3 Pa, ensure that the air is fully exhausted; fill with argon, adjust the vacuum degree to 0.5Pa, and then apply a -400V bias voltage to the turntable where the substrate is located, and perform ion cleaning for 30 minutes; then adjust the vacuum degree to 0.1Pa, apply a -30V bias voltage to the chromium alloy sheet, and energize the Zr-Nb target to deposit the coating. The deposition time is controlled to 30h to obtain a zirconium alloy coating with a thickness of 10μm. Wait for the chromium alloy sheet to cool to below 60℃ and take it out.

[0036] The X-ray diffraction analysis results of the zirconium alloy coating are as follows: Figure 2 As shown, the coating structure is α-Zr and there is no β-Nb phase inclusion in the coating.

[0037] The chromium alloy sheets in the embodiment and the comparative example were respectively put into water and subjected to a 14-day high-temperature and high-pressure water corrosion test. The weighing results are as follows: Figure 1 As shown, it can be seen that the corrosion weight gain of the zirconium alloy coating in the embodiment is significantly lower than that of the pure Zr coating in the comparative example, and the embodiment shows good corrosion resistance.

[0038] In another embodiment, a Zr-Nb-Cu alloy with a Nb content of 2% and a Cu content of 2% is smelted as a target material, wherein the Nb element in the target material mainly exists in the form of β-Nb intergranular precipitation phase, and the Cu element exists in the form of Zr 2 The Cu intermetallic compound precipitate phase is the main existing form, and the average size of the precipitate phase is greater than 300nm.

[0039] The coating preparation process is as follows: Using chromium alloy as the base workpiece, the chromium alloy sheet is suspended on the rotating frame of the magnetron sputtering equipment and the contact is ensured to be stable. The equipment cavity is evacuated to less than 8×10 -3 Pa, ensure that the air is fully exhausted; fill with argon, adjust the vacuum degree to 0.5Pa, and then apply a -400V bias voltage to the turntable where the substrate is located, and perform ion cleaning for 30 minutes; then adjust the vacuum degree to 0.1Pa, apply a -30V bias voltage to the chromium alloy sheet, and energize the Zr-Nb-Cu target to deposit the coating. The deposition time is controlled to 30h to obtain a zirconium alloy coating with a thickness of 10μm. Wait for the chromium alloy sheet to cool to below 60℃ and take it out.

[0040] X-ray diffraction analysis of the zirconium alloy coating shows that the coating structure is α-Zr, without β-Nb or Zr 2 Cu precipitation phase; no Cu or Nb inclusions larger than 10 nm were observed under an electron microscope. The zirconium alloy coating exhibited good structural uniformity.

[0041] In some other embodiments, the magnetron sputtering process may also be replaced by other PVD processes such as a multi-arc ion plating process.

[0042] In some other embodiments, the base member may also be replaced by a zirconium alloy member, a heat-resistant steel member or other metal material member compatible with the zirconium alloy, or may be replaced by a ceramic or heat-resistant polymer material member.

[0043] In some embodiments, the zirconium alloy coating may be further strengthened by surface shot peening, surface nano-crystallization, laser shock and other processes.

[0044] In different embodiments, the matrix may be a component of a pressurized water reactor fuel assembly, such as a fuel rod cladding, a fuel rod bracket or other fixed structure, or may be a component in other fields such as a chemical reaction vessel, a medical implant, etc. that requires corrosion and wear resistance treatment.

[0045] The zirconium alloy coating manufacturing method provided in the above embodiment forms a supersaturated solid solution zirconium alloy, thereby increasing the content of strengthening elements in the coating while avoiding the adverse effects of the precipitation of strengthening elements on the mechanical properties and corrosion resistance. It can effectively inhibit the phase change of the surface zirconium oxide layer in a high-temperature oxidizing environment, and the oxidation transition time is longer. It can effectively improve the corrosion resistance and wear resistance of the base component, and reduce the hydrogen absorption phenomenon under specific working conditions, thereby effectively improving the durability of the component.

[0046] The purpose of the above embodiments is to further explain the present invention in detail in conjunction with the accompanying drawings so that those skilled in the art can understand the technical concept of the present invention. Within the scope of the present invention, the optimization or equivalent replacement of the method steps involved, and the combination of the implementation methods in different embodiments without conflict of structure and principle, all fall within the protection scope of the present invention.

Claims

1. A method for manufacturing a zirconium alloy coating, characterized in that: The following steps are involved: Step a): providing a substrate member and a coating target, wherein the coating target comprises Zr and a strengthening element, wherein the strengthening element comprises one or more of Nb, V, Cu, Fe, Cr, Y, Si, and Mo; Step b): adopting a PVD process to deposit the coating target on the surface of the substrate to form a zirconium alloy coating, wherein the mass percentage of the strengthening elements in the zirconium alloy coating is 1%-50%, and at least one of the strengthening elements is not less than 1%; the structure of the zirconium alloy coating is a supersaturated solid solution with Zr as the matrix.

2. The method for manufacturing a zirconium alloy coating according to claim 1, characterized in that: In the step a), the target material comprises a plurality of single-component targets, and the purity of a single element in each of the single-component targets is not less than 99.5%.

3. The method for manufacturing a zirconium alloy coating according to claim 1, characterized in that: In the step a), the target material is an alloy target material, the alloy target material includes Zr and the strengthening element, and the composition ratio of the alloy target material is the same as that of the zirconium alloy coating.

4. The method for manufacturing a zirconium alloy coating according to claim 1, 2 or 3, characterized in that: In the step b), the PVD process includes magnetron sputtering or multi-arc ion plating.

5. The method for manufacturing a zirconium alloy coating according to claim 4, characterized in that: In the step b), the PVD process is configured as magnetron sputtering and includes the following steps: Provide an equipment chamber, place the substrate into the equipment chamber and evacuate the chamber to a vacuum level not higher than 8×10 -3 Pa, fill with argon to 0.1Pa-1Pa; Applying a bias voltage of -30V to -300V to the substrate, and electrifying the coating target to perform coating deposition; After the zirconium alloy coating is deposited to a given thickness and then cooled, the substrate is taken out of the equipment chamber.

6. The method for manufacturing a zirconium alloy coating according to claim 5, characterized in that: Before coating deposition, the method further includes performing ion cleaning on the substrate. In the ion cleaning step, a bias voltage of -400V to -800V is first applied to the substrate to ionize the argon gas and bombard the substrate. The ion cleaning is completed by maintaining the voltage for 5 minutes to 60 minutes.

7. The method for manufacturing a zirconium alloy coating according to claim 5, characterized in that: When the coating is deposited, the electric power supplied to the coating target is 1w / cm 2 -5w / cm 2 .

8. A zirconium alloy coating, characterized in that: The zirconium alloy coating comprises a Zr matrix and strengthening elements, wherein the strengthening elements comprise one or more of Nb, V, Cu, Fe, Cr, Y, Si, and Mo, and the strengthening elements account for 1% to 50% by weight; the structure of the zirconium alloy coating is a supersaturated solid solution with Zr as the matrix; The zirconium alloy coating is manufactured by the zirconium alloy coating manufacturing method according to any one of claims 1 to 7.

9. A method for preventing corrosion, characterized in that: The anti-corrosion method comprises coating a zirconium alloy coating on the surface of a substrate component that needs to be treated for anti-corrosion to improve corrosion resistance, wherein the zirconium alloy coating is deposited on the surface of the substrate component by the zirconium alloy coating manufacturing method according to any one of claims 1 to 7.