Passivation solution for improving oxidation resistance of copper material and application of passivation solution

By using passivation solution of methylbenzotriazole, sodium polyaspartate, oxidant and compound surfactant, a dense oxide film is formed, which solves the problem of corrosion and discoloration of copper materials in humid and hot environments, and achieves no Improved toxic and environmentally friendly high-efficiency antioxidant performance.

CN119082718APending Publication Date: 2024-12-06JIANGSU SILICON INTEGRITY SEMICON TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411226071.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Copper materials are prone to corrosion and discoloration in humid and hot environments. The existing passivation process has the problem of using harmful substances and pollution, which makes it difficult to effectively improve its antioxidant performance.

Method used

A passivation solution composed of methylbenzotriazole, sodium polyaspartate, oxidant and compound surfactant is used to form a dense oxide film through specific preparation and application steps to inhibit corrosion and oxidation of the copper surface.

Benefits of technology

Effectively improve the antioxidant and anti-discoloration properties of copper materials, reduce the use of metal anti-rust agents, avoid pollution and environmental hazards, and the generated oxide film is uniform and dense, suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119082718A_ABST
    Figure CN119082718A_ABST
Patent Text Reader

Abstract

The invention provides a passivation solution for improving oxidation resistance of a copper material. The passivation solution comprises the following components: 1-5g / L of methylbenzotriazole, 0.1-0.5 g / L of sodium polyaspartate, 5-10g / L of an oxidizing agent, 0.2-1.0 g / L of a compound surfactant and the balance of deionized water. The passivation solution is also applied to the copper material. According to the copper material passivated through the passivation solution, corrosion and oxidation of the surface of the copper material can be effectively inhibited, and the oxidation resistance and discoloration prevention performance of the surface of the copper material are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of semiconductor material processing, and more specifically to a passivation solution for improving the anti-oxidation performance of copper materials and application thereof. Background Art

[0002] Copper and its alloys have excellent electrical and thermal conductivity and are widely used in automobile manufacturing, surface treatment technology, electronic equipment manufacturing and other fields. However, metal materials such as copper and copper alloys are prone to lose electrons due to oxidation under certain conditions, resulting in corrosion and discoloration. In particular, there are potential differences between various elements in copper alloys, which are more prone to corrosion and discoloration in hot and humid environments. Therefore, preventing discoloration after copper passivation has become an important surface treatment process. In order to solve this problem, people have studied a variety of methods to protect copper materials, among which significant progress has been made in the research and development of various corrosion inhibitors.

[0003] The specific implementation of the copper passivation process includes a series of steps, such as degreasing, degreasing, pickling, machine washing, strong pickling, water washing, surface conditioning, water washing again, passivation, final water washing and drying, etc. This series of steps is aimed at forming a corrosion-resistant oxide film on the surface of the copper material to effectively prevent further electrochemical corrosion or rust, while increasing the surface finish. This process not only improves the protective effect of the copper material, but also increases the aesthetics of the copper material.

[0004] In addition, copper passivation is an important anti-corrosion method that forms a dense and stable oxide film on the copper surface to prevent the intrusion of oxygen, moisture and other harmful substances. Common copper surface passivation methods include acid passivation, alkaline passivation and electrochemical passivation, each with its own advantages and disadvantages. The appropriate method should be selected according to the actual application requirements. Copper passivator is a chemical agent that can protect copper products from corrosion and oxidation. Summary of the invention

[0005] In order to solve the above problems, the present invention provides a passivation solution for improving the anti-oxidation performance of copper materials and its application. The copper material passivated by the passivation solution of the present invention can effectively inhibit the corrosion and oxidation of the copper material surface, and improve the anti-oxidation performance and anti-discoloration performance of the copper material surface.

[0006] In a first aspect, the present invention provides a passivation solution for improving the anti-oxidation performance of copper materials, wherein the components of the passivation solution are: 1-5 g / L of methylbenzotriazole, 0.1-0.5 g / L of sodium polyaspartate, 5-10 g / L of an oxidant, 0.2-1.0 g / L of a compound surfactant, and the balance is deionized water;

[0007] The preparation method of the above passivation solution is:

[0008] S1. Add oxidant to deionized water and stir until completely dissolved;

[0009] S2, add methylbenzotriazole and sodium polyaspartate respectively, and stir until completely dissolved;

[0010] S3, adding the compound surfactant, stirring thoroughly until completely dissolved, to obtain the passivation solution.

[0011] Preferably, the oxidant is one or more of hydrogen peroxide, peracetic acid, nitric acid, salicylic acid, sodium persulfate, and ammonium persulfate.

[0012] Preferably, the compound surfactant is two or more of nonylphenol polyoxyethylene ether, fatty amine polyoxyethylene ether, trans-block polyether, sodium dodecyl sulfate, sodium dodecylbenzene sulfonate, fatty acid methyl ester polyoxyethylene ether sodium sulfate, and long-chain alcohol polyoxyethylene ether.

[0013] In a second aspect, the present invention further discloses a method for passivating the surface of a copper material using the above passivation solution, the method comprising the following steps:

[0014] S1. Rinse the copper material after removing the surface oil with deionized water and blow dry;

[0015] S2, placing the copper material in a pickling agent to remove the oxide layer on the surface of the copper material, and rinsing the pickled copper material with deionized water and drying it;

[0016] S3, adjusting the pH value of the passivation solution to 3-6, placing the treated copper material into the passivation solution at room temperature or under heating conditions, and performing passivation treatment according to the corresponding passivation process;

[0017] S4. The passivated copper material is neutralized, washed with deionized water, and then blown dry.

[0018] Preferably, in step S1, the copper material is brass or red copper.

[0019] Preferably, in step S4, the solution for neutralization treatment is a 5 wt.% sodium carbonate or sodium hydroxide solution.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] On the one hand, only a small amount of metal rust inhibitor is used in the passivation solution disclosed in the present invention, and a protective film is formed on the metal surface to isolate external corrosive substances and slow down the oxidation of the metal surface; the corrosion inhibitor is adsorbed on the metal surface to form a protective layer to prevent the contact between the corrosive medium and the metal, thereby playing a role in corrosion resistance; it then plays a synergistic role with the oxidant and the compound surfactant to form a dense and uniform oxide film on the metal surface, inhibiting the corrosion and oxidation of the copper surface, and improving the anti-oxidation and anti-discoloration properties of the copper surface;

[0022] On the other hand, compared with the traditional passivation method, the method of passivating copper materials using the passivation solution of the present invention has simple materials and is non-toxic; traditional passivation mostly uses chromate, and although hexavalent chromium is low in cost, it is toxic and causes harm to the human body during the production process, and the waste liquid produced will pollute the environment. Therefore, with the improvement of sustainable development and environmental awareness, various industries are actively seeking greener and more environmentally friendly treatment solutions such as chromium-free passivation. The preparation method of the passivation solution in the present invention is simple, and the environmentally friendly passivation formula does not contain harmful substances, there is no burden on waste liquid treatment, and it is pollution-free to the environment; the metal surface after passivation still retains a metallic luster, significantly improves corrosion resistance, and is expected to be manufactured on a large scale. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 3 is a comparison diagram before and after the comparative example experiment in Example 3 of the present invention;

[0024] Figure 2 is a comparison diagram before and after the experiment of Experimental Example 1 in Example 3 of the present invention;

[0025] Figure 3 is a comparison diagram before and after the experiment of Experimental Example 2 in Example 3 of the present invention;

[0026] Figure 4 It is a comparison diagram before and after the experiment of Experimental Example 3 in Example 3 of the present invention. DETAILED DESCRIPTION

[0027] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Generally, the components of the embodiments of the present invention described and shown in the drawings here can be arranged and designed in various different configurations.

[0028] Therefore, the following detailed description of the embodiments of the present invention provided in the accompanying drawings is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0029] Example 1

[0030] The present embodiment provides a passivation solution for improving the anti-oxidation performance of copper materials. The components of the passivation solution are: 1-5 g / L of methylbenzotriazole, 0.1-0.5 g / L of sodium polyaspartate, 5-10 g / L of oxidant, 0.2-1.0 g / L of compound surfactant, and the balance is deionized water.

[0031] The preparation method of the above passivation solution is:

[0032] S1. Add oxidant to deionized water and stir until completely dissolved;

[0033] S2, add methylbenzotriazole and sodium polyaspartate respectively, and stir until completely dissolved;

[0034] S3, adding the compound surfactant, stirring thoroughly until completely dissolved, to obtain the passivation solution.

[0035] The oxidant is one or more of hydrogen peroxide, peracetic acid, nitric acid, salicylic acid, sodium persulfate, and ammonium persulfate.

[0036] The compound surfactant is two or more than three of nonylphenol polyoxyethylene ether, fatty amine polyoxyethylene ether, trans-block polyether, sodium dodecyl sulfate, sodium dodecylbenzene sulfonate, fatty acid methyl ester polyoxyethylene ether sodium sulfate, and long-chain alcohol polyoxyethylene ether.

[0037] In the passivation solution components disclosed in the present embodiment, methyl benzotriazole is used as a corrosion inhibitor, sodium polyaspartate is a metal rust and scale inhibitor, an oxidant peels off the oxide on the surface of the substrate, and a surfactant reduces the interfacial tension. There is no strong acid in the passivation solution components, and the methyl benzotriazole (TTA for short) can play the corrosion inhibition effect in the range of 1-5g / L. The passivation solution preparation method in the present embodiment is simple, the preparation process is safe and non-toxic, reduces material consumption, and reduces production costs.

[0038] Example 2

[0039] This embodiment discloses a method for passivating the surface of a copper material using the passivation solution in Embodiment 1, the method comprising the following steps:

[0040] S1. Rinse the copper material with deionized water after removing the surface oil stains and blow dry; the copper material is brass or red copper.

[0041] S2. Put the copper material into a pickling agent to remove the oxide layer on the surface of the copper material. Rinse the pickled copper material with deionized water and blow dry. The pickling agent is a copper chemical polishing pickling agent. The pickling agent model SYT8671 produced by Shanghai Xinyang Semiconductor Materials Co., Ltd. can be used.

[0042] S3. Adjust the pH value of the passivation solution to 3-6. Place the treated copper material in the passivation solution at room temperature or under heating conditions and passivate for 10-30 minutes. The passivation process can be carried out at room temperature, but heating conditions will increase the reaction rate of the chemical and shorten the process time. It can be carried out at a temperature of 50°C.

[0043] S4. The copper material after passivation is neutralized, washed with deionized water, and then dried. The neutralization solution is 5wt.% sodium carbonate or sodium hydroxide solution.

[0044] Example 3

[0045] According to the passivation time in Example 2, copper materials were formed in Experimental Example 1 (passivation for 10 minutes), Experimental Example 2 (passivation for 20 minutes), and Experimental Example 3 (passivation for 30 minutes).

[0046] An unpassivated copper material is prepared as a comparative example, and its preparation method is as follows: first, the copper material is placed in a degreasing agent for cleaning to remove oil stains on the surface, and then the degreased substrate is rinsed with deionized water and blown dry; the degreased substrate is placed in a pickling agent to remove the oxide layer on the surface, and then rinsed with deionized water and blown dry.

[0047] The neutral salt spray test conditions and evaluation criteria for the passivation film are:

[0048]

[0049] The unpassivated copper material of the comparative example and the passivated copper material of the experimental examples 1-3 were subjected to the neutral salt spray test of the passivation film according to the above test conditions. Figure 1-4 shown. Figure 1 This is a comparison chart before and after the comparative experiment. Figure 2 This is a comparison chart before and after the experiment in Experiment 1. Figure 3 This is a comparison chart before and after the experiment in Experiment 2. Figure 4 This is a comparison diagram before and after the experiment of Experiment 3. It can be seen from the figure that the unpassivated copper material of the comparative example showed obvious corrosion within 2 hours, while the passivated copper material of Experimental Examples 1-3 showed no obvious rust within 120 hours.

[0050] In summary, the passivation film prepared by the formula of the present invention can withstand neutral salt spray for up to 120 hours, the passivation time is short (10min-30min), the generated passivation film is uniform and dense, does not affect the appearance, color, gloss and size of the copper material, and can effectively prevent the risk of oxidation and discoloration of the copper material, and does not affect the conductivity of the copper material.

[0051] The above are only some embodiments of the present invention. It should be pointed out that for ordinary technicians in this field, other modifications and improvements can be made without departing from the creative concept of the present invention, which all belong to the protection scope of the present invention.

Claims

1. A passivation solution for improving the anti-oxidation performance of copper materials, characterized in that: The components of the passivation solution are: 1-5 g / L methylbenzotriazole, 0.1-0.5 g / L sodium polyaspartate, 5-10 g / L oxidant, 0.2-1.0 g / L compound surfactant, and the balance is deionized water; The preparation method of the passivation solution is: S1. Add oxidant to deionized water and stir until completely dissolved; S2, add methylbenzotriazole and sodium polyaspartate respectively, and stir until completely dissolved; S3, adding the compound surfactant, stirring thoroughly until completely dissolved, to obtain the passivation solution.

2. A passivation solution for improving the anti-oxidation performance of copper materials according to claim 1, characterized in that: The oxidant is one or more of hydrogen peroxide, peracetic acid, nitric acid, salicylic acid, sodium persulfate, and ammonium persulfate.

3. A passivation solution for improving the anti-oxidation performance of copper materials according to claim 2, characterized in that: The compound surfactant is two or more than three of nonylphenol polyoxyethylene ether, fatty amine polyoxyethylene ether, trans-block polyether, sodium dodecyl sulfate, sodium dodecylbenzene sulfonate, fatty acid methyl ester polyoxyethylene ether sodium sulfate, and long-chain alcohol polyoxyethylene ether.

4. A method for passivating a copper material surface using the passivating solution of any one of claims 1 to 3, characterized in that: The following steps are involved: S1. Rinse the copper material after removing the surface oil with deionized water and blow dry; S2, placing the copper material in a pickling agent to remove the oxide layer on the surface of the copper material, and rinsing the pickled copper material with deionized water and drying it; S3, adjusting the pH value of the passivation solution to 3-6, placing the treated copper material into the passivation solution at room temperature or under heating conditions, and performing passivation treatment according to the corresponding passivation process; S4. The passivated copper material is neutralized, washed with deionized water, and then blown dry.

5. The method according to claim 4, characterized in that In step S1, the copper material is brass or copper.

6. The method according to claim 5, characterized in that In step S4, the solution for neutralization treatment is a 5 wt.% sodium carbonate or sodium hydroxide solution.