Point array patterned super-hydrophobic gas electrode and preparation method and application thereof
By designing dot arrays on the electrodes to pattern supergasperspex electrodes, and using infrared laser etching to form dot arrays on the catalyst coating, the problems of easy peeling of the electrolytic catalyst and low mass transfer efficiency are solved, and the electrode performance is improved .
Patent Information
- Application Number
- CN202411267471.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-11
- Publication Date
- 2024-12-06
AI Technical Summary
The existing electrolytic catalysts are prone to peel off on the electrode surface, resulting in a decrease in electrode stability and the binder hinders the gas mass transfer efficiency.
A dot array patterned supergass electrode is designed to form a dot array on the catalyst coating by distributing a dot array on the substrate, thereby promoting gas release by infrared laser etching.
It improves the electrode performance, promotes the rapid release of gas inside the catalyst layer, and enhances the application prospects of the electrode, especially in electrochemical gas analysis reactions.
Smart Images

Figure CN119082760A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of catalytic materials, and in particular relates to a dot array patterned super-aerophobic electrode and a preparation method and application thereof. Background Art
[0002] Water electrolysis technology is an important way to prepare green hydrogen. The hydrogen evolution electrode is one of its core components, which is mainly composed of a catalyst and a conductive substrate. The catalyst is one of the important factors affecting its performance. Currently, the commercial catalyst is mainly a powdered platinum-carbon catalyst, which is widely used and has extremely high commercial value. However, in continuous electrochemical reactions, the catalyst often peels off from the collector surface, which greatly reduces the stability of the electrode.
[0003] In order to solve the problem of easy peeling of the above-mentioned catalyst, a binder (such as Nafion, carboxymethyl cellulose, PTFE, etc.) needs to be added during the production of the electrode to fix the electrode material before the electrode test (see: Materials). The reactants and catalyst materials are in full contact, which affects the catalytic effect of the catalyst (reference: Accounts of Chemical Research, 2018, 51(4): 881-9).
[0004] Therefore, based on the existing commercial platinum-carbon catalyst preparation and loading technology, optimizing the catalyst coating structure, designing new electrodes, and promoting product gas mass transfer are the key to improving electrode performance. Summary of the invention
[0005] In view of the problems in the prior art that the water electrolysis catalyst is easily peeled off from the electrode surface and the use of binders hinders the gas mass transfer efficiency, the present invention provides a dot array patterned super-gas-repellent electrode and a preparation method and application, which effectively improve the electrode performance.
[0006] The present invention is achieved through the following technical solutions: A dot array patterned super-gas-repellent electrode, characterized in that it comprises a substrate and a super-gas-repellent catalyst layer disposed on the substrate, and a dot array is distributed on the surface of the super-gas-repellent catalyst layer; The super-aerophobic catalyst layer comprises a catalyst and an adhesive.
[0007] Furthermore, the substrate is one of a titanium sheet, a nickel sheet, a platinum sheet, a copper sheet, carbon paper and ITO conductive glass.
[0008] Furthermore, the catalyst is one or more of platinum-carbon powder, palladium-carbon powder and iridium dioxide powder; and the adhesive is Nafion adhesive.
[0009] Furthermore, the point array (3) is a square or hexagonal array.
[0010] Furthermore, a single dot in the dot array (3) is in the shape of a circular hole, a single dot diameter is 100-1000 μm, and a dot spacing is 100-5000 μm.
[0011] Furthermore, the ratio of the catalyst to the adhesive is 4 mg:50 μL.
[0012] In the present invention, the method for preparing the super-aerophobic electrode with dot array patterning comprises the following steps: 1) Substrate pretreatment: polish and clean the substrate and remove the surface oxide layer; 2) Preparation of catalyst slurry: mixing the catalyst, the binder and the organic solvent, and dispersing the catalyst evenly to obtain the catalyst slurry; 3) dripping the catalyst slurry onto the substrate surface, allowing the solvent to evaporate and the catalyst to form a film on the substrate surface as a catalyst coating; 4) Laser marking: Use an infrared laser to etch a dot array on the surface of the catalyst coating to form a super-aerophobic catalyst layer with a patterned dot array distributed on the surface.
[0013] Furthermore, the organic solvent in step 2) is one of methanol, isopropanol, ethanol, N,N-dimethylformamide and dimethyl sulfoxide.
[0014] In the present invention, the dot array patterned super-aerophobic electrode is used in an electrochemical gas evolution reaction.
[0015] Furthermore, the electrochemical gas evolution reaction is electrochemical hydrogen evolution reaction, electrochemical chlorine evolution, and electrochemical oxygen evolution.
[0016] The dot array patterned super-aerophobic electrode catalyst layer surface dot array of the present invention is obtained by infrared laser etching, the etched area is aerophobic underwater, and the dot array provides an outlet for releasing gas inside the coating, which is conducive to the rapid release of bubbles from the dot array.
[0017] Beneficial Effects (1) The method for preparing the dot array patterned super-gas-repellent electrode of the present invention is simple. The dot array can be introduced on the electrode surface by a one-step treatment of the electrode surface prepared by the conventional drop coating method through laser etching technology, thereby realizing the preparation of the dot array patterned super-gas-repellent electrode; (2) The present invention improves electrode performance by promoting gas mass transfer. The introduction of the dot array can promote the rapid release of gas inside the catalyst layer, thereby achieving improved electrode performance without increasing the catalyst loading. It has good application prospects in electrochemical gas evolution reactions. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 11. Schematic diagram of the main view of the dot array patterned super-aerophobic electrode, 2. Super-aerophobic catalyst layer, 3. Dot array; Figure 2 Schematic side view of a dot array patterned super-aerophobic electrode, 1. substrate, 2. super-aerophobic catalyst layer, 3. dot array; Figure 3 The dot array patterned super-aerophobic electrode image is prepared for Example 1; Figure 4 This is a SEM image of the dot array patterned super-aerophobic electrode prepared in Example 1; Figure 5 Schematic diagram of the bubble contact angle at the dot array of the dot array patterned super aerophobic electrode prepared in Example 1; Figure 6 The behavior of bubbles on the surface of the super-aerophobic dot array electrode of Example 1 during the catalytic hydrogen evolution reaction; Figure 7 The graphs of the current density of the electrodes prepared in Example 2 and Comparative Example 2 versus the applied potential are shown; Figure 8 The bubble behavior on the surface of the catalyst electrode in Comparative Example 1 during catalytic hydrogen evolution reaction. DETAILED DESCRIPTION
[0019] The present invention is described in detail below in conjunction with specific implementations and drawings, but the protection scope of the present invention is not limited by the embodiments. All technologies implemented based on the above content of the present invention are included in the scope of protection intended by the present invention.
[0020] Unless otherwise defined, all professional and scientific terms used in the present invention have the same meanings as those understood by technicians in the technical field of the present invention. Unless otherwise specified, the drugs or reagents used in the present invention are used in accordance with the product instructions or the conventional methods of use in the field. The technical solution of the present invention is further described according to the drawings and specific embodiments of the specification.
[0021] The main schematic diagram of the dot array patterned super-aerophobic electrode in the present invention is as follows Figure 1 As shown, the side view diagram is as follows Figure 2 As shown, 1 is the substrate, 2 is the super-aerophobic catalyst layer, and 3 is the dot array. Figure 1 and Figure 2It can be seen that the super-aerophobic electrode with a dot array pattern includes a substrate 1 and a super-aerophobic catalyst layer 2 arranged on the substrate 1, and a dot array pattern 3 (square or hexagonal array) is distributed on the surface of the super-aerophobic catalyst layer 2; the super-aerophobic catalyst layer 2 includes a catalyst and an adhesive, and the super-aerophobic catalyst layer 2 is used to generate a hydrogen evolution reaction by electrolysis of water and to transfer the bubble nucleation growth to the dot array 3 when bubbles are generated; the dot array 3 on the surface of the super-aerophobic catalyst layer 2 is used to provide an outlet for the release of bubbles, so that they can quickly detach from the electrode from the dot array; a single dot in the dot array 3 is in the shape of a circular hole, a single dot diameter is 100-1000 μm, and a dot spacing is 100-5000 μm.
[0022] The preparation method and application of the dot array patterned super-aerophobic electrode are now described in conjunction with the accompanying drawings and specific embodiments.
[0023] Example 1 1) Substrate pretreatment: The surface of a 1.0 cm × 1.0 cm × 0.5 cm titanium sheet was polished with 600# sandpaper. After polishing, the titanium sheet was ultrasonically cleaned in an ethanol solution and deionized water respectively. After drying at room temperature, the titanium sheet was immersed in a 10wt% oxalic acid solution, heated at 90°C for 1 h, taken out, ultrasonically cleaned with deionized water and ethanol in sequence for multiple times, and dried naturally to obtain substrate 1, which was then left to stand for use. 2) Preparation of catalyst slurry: Take 4 mg of platinum-carbon powder in a clean reagent bottle, add 50 μL of Nafion and 950 μL of isopropanol, shake, and perform ultrasonic treatment at room temperature for 2 h to evenly disperse the components in the catalyst slurry to obtain a catalyst slurry; 3) Use a pipette to take 40 μL of the catalyst slurry prepared in step (2) and drip it onto the surface of substrate 1. Slowly drip it onto the surface of the titanium sheet. The liquid will be completely spread over a 1.0 cm × 1.0 cm area on the surface of the titanium sheet. Cover it with a glass slide to prevent dust from falling in. Let it stand at room temperature for 45 min as a catalyst coating. 4) Laser marking: An infrared laser is used to etch a dot array on the surface of the catalyst coating to form a super-aerophobic catalyst layer 2 with a surface distributed dot array 3, thereby obtaining a super-aerophobic electrode with a dot array; wherein a single dot is a circular hole, a single dot diameter is 0.2 mm, a dot spacing is 0.5 mm, and the number of dot array holes is 20 × 20. Figure 3 Patterning super-aerophobic electrodes for dot arrays, Figure 4 This is a scanning electron microscope (SEM) image of the micro-nanostructure on the surface of the dot array electrode. The bubble contact angle at the dot array of the dot array patterned super-aerophobic electrode is 154° ( Figure 5 ).
[0024] Electrochemical performance test of the super-aerophobic electrode with dot array pattern prepared in Example 1: The dot array pattern super-aerophobic electrode was fixed with a polytetrafluoroethylene electrode clamp, and the entire electrode was placed in 0.5 M sulfuric acid for electrochemical hydrogen evolution reaction. The surface of the electrode during electrochemical reaction and hydrogen evolution was observed by high-speed video. During the electrocatalytic hydrogen evolution reaction, the bubble behavior on the surface of the super-aerophobic dot array electrode is as follows: Figure 6 As shown, the bubbles first nucleate and grow at the point array and are continuously desorbed and renewed. After the inside of the coating contacts the electrolyte, the small bubbles generated on the contact surface are mostly generated from the point array, forming several columns of bubble clusters. The bubble sites are continuously renewed, exposing the reaction active sites of the catalyst so that the electrochemical reaction continues.
[0025] Example 2 1) Substrate pretreatment: The surface of a 1.0 cm × 1.0 cm × 0.5 cm titanium sheet was polished with 600# sandpaper. After polishing, the titanium sheet was ultrasonically cleaned in an ethanol solution and deionized water respectively. After drying at room temperature, the titanium sheet was immersed in a 10wt% oxalic acid solution, heated at 90°C for 1 h, taken out, ultrasonically cleaned with deionized water and ethanol in sequence for multiple times, and dried naturally to obtain substrate 1, which was then left to stand for use. 2) Preparation of catalyst slurry: Take 4 mg of platinum-carbon powder in a clean reagent bottle, add 50 μL of Nafion and 950 μL of isopropanol, shake, and perform ultrasonic treatment at room temperature for 2 h to evenly disperse the components in the catalyst slurry to obtain a catalyst slurry; 3) Use a pipette to take 40 μL of the catalyst slurry prepared in step (2) and drip it onto the surface of substrate 1. Slowly drip it onto the surface of the titanium sheet. The liquid will be completely spread over a 1.0 cm × 1.0 cm area on the surface of the titanium sheet. Cover it with a glass slide to prevent dust from falling in. Let it stand at room temperature for 45 min as a catalyst coating. 4) Laser marking: An infrared laser is used to etch a dot array on the surface of the catalyst coating to form a super-aerophobic catalyst layer 2 with a surface distributed dot array 3, thereby obtaining a dot array patterned super-aerophobic electrode; wherein a single dot is in the shape of a circular hole, a single dot diameter is 0.2 mm, a dot spacing is 0.125 mm, and the number of dot array holes is 80 × 80.
[0026] The electrochemical performance of the dot array patterned super-gas-repellent electrode prepared in Example 2 was tested. The dot array patterned super-gas-repellent electrode was fixed with a polytetrafluoroethylene electrode clamp, and the entire electrode was placed in 0.5 M sulfuric acid for electrochemical hydrogen evolution reaction. The curve of the change of current with the applied potential is shown in FIG. Figure 7 shown.
[0027] Comparative Example 1 1) Substrate pretreatment: The surface of a 1.0 cm × 1.0 cm × 0.5 cm titanium sheet was polished with 600# sandpaper. After polishing, the titanium sheet was ultrasonically cleaned in an ethanol solution and deionized water respectively. After drying at room temperature, the titanium sheet was immersed in a 10wt% oxalic acid solution, heated at 90°C for 1 h, taken out, ultrasonically cleaned with deionized water and ethanol in sequence for multiple times, and dried naturally to obtain substrate 1, which was then left to stand for use. 2) Preparation of catalyst slurry: Take 4 mg of platinum-carbon powder in a clean reagent bottle, add 50 μL of Nafion and 950 μL of isopropanol, shake, and perform ultrasonic treatment at room temperature for 2 h to evenly disperse the components in the catalyst slurry to obtain a catalyst slurry; 3) Use a pipette to take 40 μL of the catalyst slurry prepared in step (2) and drip it onto the surface of substrate 1, then slowly drip it onto the surface of the titanium sheet. The liquid will completely spread over a 1.0 cm × 1.0 cm area on the surface of the titanium sheet. Cover with a glass slide to prevent dust from falling in. Leave at room temperature for 45 min to allow the organic solvent to evaporate and form a film as catalyst coating 2. Catalyst coating 2 and substrate 1 constitute a catalyst-containing electrode. The electrochemical performance was tested according to the method of Example 1. The behavior of bubbles in the catalyst electrode during the electrochemical hydrogen evolution process was as follows: Figure 8 As shown, the bubble nucleation and release positions are irregular, and the size of the released bubbles is larger than that of Example 1.
[0028] Comparative Example 2 1) Substrate pretreatment: The surface of a 1.0 cm × 1.0 cm × 0.5 cm titanium sheet was polished with 600# sandpaper. After polishing, the titanium sheet was ultrasonically cleaned in an ethanol solution and deionized water respectively. After drying at room temperature, the titanium sheet was immersed in a 10wt% oxalic acid solution, heated at 90°C for 1 h, taken out, ultrasonically cleaned with deionized water and ethanol in sequence for multiple times, and dried naturally to obtain substrate 1, which was then left to stand for use. 2) Preparation of catalyst slurry: Take 4 mg of platinum-carbon powder in a clean reagent bottle, add 50 μL of Nafion and 950 μL of isopropanol, shake, and perform ultrasonic treatment at room temperature for 2 h to evenly disperse the components in the catalyst slurry to obtain a catalyst slurry; 3) Use a pipette to take 40 μL of the catalyst slurry prepared in step (2) and drip it onto the surface of substrate 1, then slowly drip it onto the surface of the titanium sheet. The liquid will completely spread over a 1.0 cm × 1.0 cm area on the surface of the titanium sheet. Cover with a glass slide to prevent dust from falling in. Leave at room temperature for 45 min to allow the organic solvent to evaporate and form a film as catalyst coating 2. Catalyst coating 2 and substrate 1 constitute a catalyst-containing electrode. The electrochemical performance was tested according to the method of Example 2. The curve of the change of the catalyst electrode current with the applied potential is as follows: Figure 7As shown, the current density at each applied voltage is lower than that of Example 2.
Claims
1. A dot array patterned super-aerophobic electrode, It is characterized in that It comprises a substrate (1), a super-aerophobic catalyst layer (2) arranged on the substrate (1), and a surface distribution point array (3) of the super-aerophobic catalyst layer (2); The super-aerophobic catalyst layer (2) comprises a catalyst and an adhesive.
2. The dot array patterned super-aerophobic electrode according to claim 1, It is characterized in that The substrate (1) is one of a titanium sheet, a nickel sheet, a platinum sheet, a copper sheet, carbon paper and ITO conductive glass.
3. The dot array patterned super-aerophobic electrode according to claim 1, It is characterized in that The catalyst is one or more of platinum carbon powder, palladium carbon powder and iridium dioxide powder; and the adhesive is Nafion adhesive.
4. The dot array patterned super-aerophobic electrode according to claim 1, It is characterized in that The point array (3) is a square or hexagonal array.
5. The dot array patterned super-aerophobic electrode according to claim 4, It is characterized in that A single dot in the dot array (3) is in the shape of a circular hole, a single dot diameter is 100-1000 μm, and a dot spacing is 100-5000 μm.
6. The dot array patterned super-aerophobic electrode according to claim 1, It is characterized in that The ratio of the catalyst to the adhesive is 4 mg:50 μL.
7. A method for preparing a super-aerophobic electrode having a dot array pattern according to any one of claims 1 to 6, It is characterized in that The following steps are involved: 1) Substrate pretreatment: grinding and cleaning the substrate (1) and removing the surface oxide layer; 2) Preparation of catalyst slurry: mixing the catalyst, the binder and the organic solvent, and dispersing the catalyst evenly to obtain the catalyst slurry; 3) dripping the catalyst slurry onto the surface of the substrate (1), allowing the solvent to evaporate, and the catalyst to form a film on the surface of the substrate (1) as a catalyst coating; 4) Laser marking: using an infrared laser to etch a dot array on the surface of the catalyst coating to form a super-aerophobic catalyst layer (2) having a patterned dot array (3) distributed on the surface.
8. The method for preparing the dot array patterned super-aerophobic electrode according to claim 7, It is characterized in that The organic solvent in step 2) is one of methanol, isopropanol, ethanol, N,N-dimethylformamide and dimethyl sulfoxide.
9. Use of the dot array patterned super-gas-repellent electrode according to any one of claims 1 to 6 in an electrochemical gas evolution reaction.
10. The use according to claim 9, It is characterized in that The electrochemical gas evolution reaction is electrochemical hydrogen evolution reaction, electrochemical chlorine evolution, and electrochemical oxygen evolution.
Citation Information
Patent Citations
Micron array electrode structure, preparation method and application thereof
CN114134528A
Gas evolution electrode for promoting bubble transfer and gas diffusion as well as preparation method and application of gas evolution electrode
CN115354355A
Super-aerophobic powder catalyst layer as well as preparation method and application thereof
CN118299592A