Multi-element alloyed copper-zinc-tin-sulfur-selenium absorption layer, preparation thereof and solar cell
By introducing non-intrinsic cations into copper-zinc-tin-sulfur-selenium solar cells, the mesophase stability and metal-selenium bond strength during selenization are reduced, and the formation of deep defects is suppressed, and the problem of low efficiency of copper-zinc-tin-selenium solar cells is solved. , achieving high efficiency and low defect density battery performance.
Patent Information
- Application Number
- CN202310656343.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-05
- Publication Date
- 2024-12-06
AI Technical Summary
The efficiency of copper-zinc-tin-sulfur-selenium solar cells is lower than their theoretical limits and industrialization levels, mainly due to charge loss caused by deep defects in the lattice. Existing thermodynamic methods have failed to effectively suppress these defects.
Using a multi-alloyed copper-zinc-tin sulfide-selenium absorbing layer, the stability of the Cu2SnSe3 mesophase during selenization is reduced or the Zn-Se bond is weakened by introducing at least two non-intrinsic cations, such as silver ions, cadmium ions and germanium ions. The strength of the SnZn deep defect dynamically inhibits the formation of SnZn deep defects.
It significantly improves the photoelectric conversion efficiency, reduces charge loss, and has a simple process, which is suitable for large-scale applications.
Smart Images

Figure CN119092567A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of thin-film solar cells, and in particular to a multi-element alloyed copper-zinc-tin-sulfur-selenium absorption layer and a preparation method thereof, and a copper-zinc-tin-sulfur-selenium solar cell comprising the multi-element alloyed copper-zinc-tin-sulfur-selenium absorption layer. Background Art
[0002] Thin-film solar cells such as CIGS (copper indium gallium selenide) and CdTe have the disadvantages of scarce raw materials (In, Te) and toxic cations (Cd), which limit their large-scale commercial production. Compared with the above material systems, the emerging copper zinc tin sulfur selenide (Cu2ZnSn(S x Se 1-x )4) The battery has the advantages of high abundance of constituent cations, non-toxicity, excellent material stability and outstanding industrial compatibility, and is considered to be a battery that can promote large-scale and low-cost applications of thin-film photovoltaics. After nearly two decades of development, the highest certified power conversion efficiency (PCE) of copper-zinc-tin-sulfur-selenide cells has reached 13.8%. However, the efficiency of copper-zinc-tin-sulfur-selenide solar cells is still far below its Shockley-Quiesser theoretical limit efficiency and the level of industrialized photovoltaic devices (PCE>20%). Extensive studies have shown that deep defects in the copper-zinc-tin-sulfur-selenide lattice and the charge loss they cause are the most critical factors affecting the progress of battery PCE.
[0003] In order to suppress these defects, the prior art has tried to use a variety of thermodynamic methods such as fine optimization of cation content, Ag / Cu substitution alloys, and Fermi level modification to increase the defect formation energy. However, these efforts have not helped copper-zinc-tin-sulfur-selenium solar cells break the deadlock of stagnant efficiency. Therefore, there is an urgent need for a new technical solution that can effectively suppress the formation of deep defects in copper-zinc-tin-sulfur-selenium, thereby improving the performance of photovoltaic devices. Summary of the invention
[0004] In view of the above problems, the present invention proposes a multi-element alloyed copper-zinc-tin-sulfur-selenium absorption layer and a preparation method thereof, as well as a copper-zinc-tin-sulfur-selenium solar cell including the multi-element alloyed copper-zinc-tin-sulfur-selenium absorption layer that overcomes the above problems or at least partially solves the above problems.
[0005] One object of the present invention is to provide a multi-element alloyed copper-zinc-tin-sulfur-selenium absorption layer that can kinetically inhibit the formation of deep defects in copper-zinc-tin-sulfur-selenium and thus significantly improve the photoelectric conversion efficiency of the battery.
[0006] Another object of the present invention is to provide a method for preparing a multi-element alloyed copper-zinc-tin-sulfur-selenium absorption layer with a simple process.
[0007] Another object of the present invention is to provide a copper-zinc-tin-sulfur-selenium solar cell comprising the multi-element alloyed copper-zinc-tin-sulfur-selenium absorption layer with significantly improved photoelectric conversion efficiency.
[0008] According to one aspect of the present invention, a multi-element alloyed copper, zinc, tin, sulfur and selenium absorption layer is provided, wherein the absorption layer contains at least two non-intrinsic cations participating in the alloying.
[0009] Optionally, the at least two extrinsic cations include at least two of silver ions, cadmium ions, germanium ions, barium ions, and silicon ions.
[0010] Optionally, the at least two non-intrinsic cations are silver ions and germanium ions, cadmium ions and germanium ions, or silver ions, cadmium ions and germanium ions.
[0011] Optionally, in the absorber layer, Ge / Sn≤0.01 on a molar basis; and
[0012] When silver ions are present, 0.05≤Ag / (Ag+Cu)≤0.15;
[0013] When cadmium ions are present, 0.03≤Cd / (Cd+Zn)≤0.12.
[0014] According to another aspect of the present invention, there is also provided a method for preparing the aforementioned multi-element alloyed copper, zinc, tin, sulfur and selenium absorption layer, comprising:
[0015] preparing a prefabricated precursor film containing intrinsic cations of copper, zinc and tin, at least two extrinsic cations, and sulfur or selenium;
[0016] The prefabricated precursor film is subjected to selenization annealing or sulfurization annealing to form a multi-element alloyed copper-zinc-tin-sulfur-selenium thin film.
[0017] Optionally, the prefabricated precursor film is prepared by a solution method, a vacuum method, an electrochemical deposition method or a nanocrystal method.
[0018] Optionally, the non-intrinsic cations are introduced into the prefabricated precursor film by sputtering, evaporation, ion implantation or solution method.
[0019] According to another aspect of the present invention, a copper-zinc-tin-sulfur-selenium solar cell is provided, comprising the aforementioned multi-element alloyed copper-zinc-tin-sulfur-selenium absorption layer.
[0020] Optionally, the copper-zinc-tin-sulfur-selenium solar cell further includes: a substrate, a back electrode, a buffer layer, a window layer and a top gate electrode, wherein the substrate, the back electrode, the multi-element alloyed copper-zinc-tin-sulfur-selenium absorption layer, the buffer layer, the window layer and the top gate electrode are stacked sequentially from bottom to top.
[0021] Optionally, the back electrode is a molybdenum electrode; and / or
[0022] The material of the buffer layer is one or more of CdS, (Zn, Cd)S and (Zn, Mg)O; and / or
[0023] The window layer is a ZnO / ITO double-layer structure or an AZO single-layer structure; and / or
[0024] The top gate electrode is a Ni / Al double-layer electrode, an Al single-layer electrode or an Ag single-layer electrode.
[0025] The multi-element alloyed copper-zinc-tin-sulfur-selenium absorption layer provided by the present invention reduces the stability of the Cu2SnS(e)3 intermediate phase or weakens the strength of the Zn-S(e) bond during the selenization (sulfurization) process by introducing a variety of non-intrinsic cations to participate in the alloying, so that the two phases are more quickly and better fused into the copper-zinc-tin-sulfur-selenium phase, and the Sn is kinetically inhibited. Zn The formation of deep defects can achieve low defect density and significantly improve the photoelectric conversion efficiency of the battery.
[0026] The preparation method of the multi-element alloyed copper, zinc, tin, sulfur and selenium absorption layer provided by the invention adopts a precursor film-post-selenization (sulfurization) method, and has a simple process and good repeatability.
[0027] The copper-zinc-tin-sulfur-selenium solar cell provided by the invention comprises a multi-element alloyed copper-zinc-tin-sulfur-selenium absorption layer, has low charge loss, high photoelectric conversion efficiency, is easy to prepare, and is suitable for large-scale application.
[0028] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention, it can be implemented according to the contents of the specification. In order to make the above and other purposes, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are listed below.
[0029] Based on the following detailed description of specific embodiments of the present invention in conjunction with the accompanying drawings, those skilled in the art will become more aware of the above and other objects, advantages and features of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Various other advantages and benefits will become apparent to those of ordinary skill in the art by reading the detailed description of the preferred embodiments below. The accompanying drawings are only for the purpose of illustrating the preferred embodiments and are not to be considered as limiting the present invention. Moreover, the same reference symbols are used throughout the accompanying drawings to represent the same components. In the accompanying drawings:
[0031] Figure 1 A schematic diagram of the structure of a copper-zinc-tin-sulfur-selenium solar cell according to an embodiment of the present invention is shown;
[0032] Figure 2A schematic diagram showing a process of preparing a copper-zinc-tin-sulfur-selenium solar cell according to an embodiment of the present invention is shown;
[0033] Figure 3 is the extraction efficiency η of the solar cells of Example 2 of the present invention and Comparative Example 1 E and collection efficiency η C Graph of
[0034] Figure 4 The fluorescence spectra of the copper-zinc-tin-sulfur-selenium absorption layers of Example 2 of the present invention and Comparative Example 1 at a temperature of 12K. DETAILED DESCRIPTION
[0035] The exemplary embodiments of the present disclosure will be described in more detail below with reference to the accompanying drawings. Although the exemplary embodiments of the present disclosure are shown in the accompanying drawings, it should be understood that the present disclosure can be implemented in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided to enable a more thorough understanding of the present disclosure and to fully convey the scope of the present disclosure to those skilled in the art.
[0036] In order to suppress deep defects in the CuZnSnS lattice, a variety of thermodynamic methods have been developed in the prior art to increase the defect formation energy, such as fine optimization of cation content, Ag / Cu substitution alloys, Fermi level modification, etc., but these methods have failed to break the deadlock of stagnant efficiency of CuZnSnS solar cells.
[0037] The inventors of the present application have found through research that the current methods cannot promote the development of battery efficiency, possibly due to the following reasons: (1) the currently proposed thermodynamic mechanism cannot fully reflect the copper-zinc-tin-sulfur-selenide defect formation process far from thermodynamic equilibrium at high temperature; (2) the thermodynamic regulation method is difficult to achieve a balance between the defect formation energy, the copper-zinc-tin-sulfur-selenide phase structure and the necessary high-vacancy alloy.
[0038] Based on the above understanding, an embodiment of the present invention proposes a multi-element alloyed copper-zinc-tin-sulfur-selenium absorption layer. The multi-element alloyed copper-zinc-tin-sulfur-selenium absorption layer contains at least two non-intrinsic cations participating in the alloying. The non-intrinsic cations mentioned in this article refer to other cations in the copper-zinc-tin-sulfur-selenium absorption layer except copper ions, zinc ions and tin ions. These non-intrinsic cations can reduce the stability of the selenium (sulfur) reaction intermediate phase or the strength of the metal-selenium (sulfur) bond.
[0039] The embodiment of the present invention introduces a variety of non-intrinsic cations into the copper-zinc-tin-sulfur-selenium absorption layer to participate in alloying, thereby reducing the stability of the Cu2SnS(e)3 intermediate phase or weakening the strength of the Zn-S(e) bond during the selenization (sulfurization) process, so that the two phases are faster and better fused into the copper-zinc-tin-sulfur-selenium phase, and kinetically suppressing the Sn ZnThe formation of deep defects can achieve low defect density and significantly improve the photoelectric conversion efficiency of the battery.
[0040] In some preferred embodiments, the at least two non-intrinsic cations may include at least two of silver ions, cadmium ions, germanium ions, barium ions, and silicon ions. These cation alloys can better reduce the stability of the selenium (sulfur) reaction intermediate phase or the strength of the metal-selenium (sulfur) bond, thereby inhibiting Sn Zn Deep defect formation.
[0041] In some further embodiments, the at least two extrinsic cations are silver ions and germanium ions.
[0042] In some further embodiments, the at least two extrinsic cations are cadmium ions and germanium ions.
[0043] In yet further embodiments, the at least two extrinsic cations are silver ions, cadmium ions, and germanium ions.
[0044] Furthermore, in the copper-zinc-tin-sulfur-selenium absorption layer, Ge / Sn≤0.01 by mole. For example, the value of Ge / Sn can be 0.009, 0.008, 0.007, 0.006, 0.005, 0.004, 0.003, 0.002, 0.001, etc. And, by mole, when silver ions are present, 0.05≤Ag / (Ag+Cu)≤0.15. For example, the value of Ag / (Ag+Cu) can be 0.06, 0.07, 0.08, 0.09, 0.10, 0.11, 0.12, 0.13, 0.14, etc. By mole, when cadmium ions are present, 0.03≤Cd / (Cd+Zn)≤0.12. For example, the value of Cd / (Cd+Zn) can be 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, 0.10, 0.11, etc.
[0045] Accordingly, an embodiment of the present invention further provides a method for preparing a multi-element alloyed copper, zinc, tin, sulfur and selenium absorption layer, comprising:
[0046] preparing a prefabricated precursor film containing intrinsic cations of copper, zinc and tin, at least two extrinsic cations, and sulfur or selenium;
[0047] The prefabricated precursor film is subjected to selenization annealing or sulfurization annealing to form a multi-element alloyed copper-zinc-tin-sulfur-selenium thin film.
[0048] Those skilled in the art should understand that when the prefabricated precursor film contains sulfur, the prefabricated precursor film is subjected to selenization annealing; when the prefabricated precursor film contains selenium, the prefabricated precursor film is subjected to sulfurization annealing. The selenization annealing and sulfurization annealing can adopt conventional selenization annealing and sulfurization annealing operating conditions.
[0049] The method for preparing the multi-element alloyed copper-zinc-tin-sulfur-selenium absorption layer of the embodiment of the present invention adopts a precursor film-post-selenization (sulfurization) method, which has a simple process and good repeatability.
[0050] In some specific embodiments, the prefabricated precursor film can be prepared by a solution method, a vacuum method, an electrochemical deposition method, or a nanocrystalline method.
[0051] In some further embodiments, the extrinsic cations may be introduced into the prefabricated precursor film by sputtering, evaporation, ion implantation or solution method.
[0052] The types and molar ratios of the non-intrinsic cations are as described above and will not be repeated here.
[0053] Based on the same technical concept, an embodiment of the present invention also provides a copper-zinc-tin-sulfur-selenium solar cell, which includes the aforementioned multi-element alloyed copper-zinc-tin-sulfur-selenium absorption layer. In the multi-element alloyed copper-zinc-tin-sulfur-selenium absorption layer, the formation of deep defects in the absorption layer is effectively suppressed by introducing a variety of cations to regulate the selenization (sulfurization) kinetics. The introduced cations can reduce the stability of the Cu2SnS(e)3 phase of the selenization (sulfurization) reaction intermediate product or the strength of the Zn-S(e) bond, thereby accelerating the fusion of the two phases, thereby avoiding the Sn caused by insufficient phase fusion. Zn The formation of deep defects. The reduction of deep defects leads to a reduction in charge loss caused by them, thus obtaining a copper-zinc-tin-sulfur-selenium solar cell with significantly improved performance.
[0054] Figure 1 FIG. 2 shows a schematic structural diagram of a copper-zinc-tin-sulfur-selenium solar cell 10 according to an embodiment of the present invention. Figure 1 As shown, in some embodiments, in addition to the multi-element alloyed copper-zinc-tin-sulfur-selenium absorption layer 13, the copper-zinc-tin-sulfur-selenium solar cell 10 further includes a substrate 11, a back electrode 12, a buffer layer 14, a window layer 15, and a top gate electrode 16. The substrate 11, the back electrode 12, the multi-element alloyed copper-zinc-tin-sulfur-selenium absorption layer 13, the buffer layer 14, the window layer 15, and the top gate electrode 16 are stacked sequentially from bottom to top.
[0055] Generally, the material of the back electrode 12 can be molybdenum, that is, the back electrode 12 is a molybdenum electrode. Of course, other appropriate back electrode materials can also be used, and the present invention does not specifically limit the material of the back electrode 12.
[0056] Similarly, the buffer layer 14, the window layer 15 and the top gate electrode 16 may also be made of common materials of copper-zinc-tin-sulfur-selenium solar cells, and the present invention does not impose any specific limitation on this.
[0057] In some further embodiments, the material of the buffer layer 14 may be one or more of CdS, (Zn, Cd)S and (Zn, Mg)O.
[0058] In some further embodiments, the window layer 15 may be a ZnO / ITO double-layer structure or an AZO single-layer structure.
[0059] In some further embodiments, the top gate electrode 16 may be a double-layer electrode, for example Figure 1 The double-layer top gate electrode shown. Specifically, the double-layer top gate electrode can be a Ni / Al double-layer electrode.
[0060] In some further embodiments, the top gate electrode 16 may also be a single-layer electrode. Specifically, the top gate electrode 16 may be, for example, an Al single-layer electrode or an Ag single-layer electrode.
[0061] The substrate 11 is used to support the other layers mentioned above. In some optional embodiments, the substrate 11 may be an insulating substrate, such as a soda-lime glass substrate. In other alternative embodiments, the substrate 11 may also be a conductive substrate, such as a flexible / rigid molybdenum foil. In this case, the back electrode layer becomes an optional option, that is, the back electrode layer may not be additionally provided, and the conductive substrate may serve as the back electrode.
[0062] Figure 2 FIG. 1 is a schematic diagram showing a process of manufacturing a copper-zinc-tin-sulfur-selenium solar cell 10 according to an embodiment of the present invention. Figure 2 As shown, the preparation method comprises the following steps:
[0063] Step S1, sputtering a Mo back electrode on a soda-lime glass substrate.
[0064] In step S1, the soda-lime glass substrate is cleaned with detergent, deionized water, and ethanol in sequence and blown dry with nitrogen. A 1.2 μm thick Mo film is sputtered on the clean soda-lime glass substrate by DC magnetron sputtering as a back electrode. During the sputtering process, the chamber background vacuum is 4×10 -4 Pa, the working gas pressure is 0.2 Pa, the working atmosphere is argon, the substrate heating temperature is 400°C, and the sputtering time is 1 hour.
[0065] Step S2, preparing a prefabricated layer film containing multiple alloy elements.
[0066] It should be noted that, in this embodiment, three alloy elements of silver, cadmium and germanium are used as an example to provide an optional preparation method. However, the alloy elements used in the present invention are not limited to Ag, Cd and Ge.
[0067] In step S2, a GeO2 thin film is prepared by spin coating. Specifically, GeO2 powder is added to a container containing 20 ml of ethylene glycol and 10 ml of ammonia water mixed solvent, and stirred until the solution is clear, to prepare a GeO2 solution with a concentration of 0.04-0.13 g / ml. The GeO2 solution is spin coated on a clean Mo back electrode in air and annealed on a hot stage, with a spin coating speed of 4200 r / min, a spin coating time of 40 s, and an annealing temperature of 300°C, to prepare a Mo back electrode coated with a GeO2 thin film.
[0068] In step S2, a copper-zinc-tin-sulfur-selenium precursor film containing silver-cadmium is prepared on the GeO2 film. Specifically, cuprous chloride, silver chloride, zinc acetate, cadmium chloride, tin tetrachloride and thiourea are dissolved in ethylene glycol methyl ether to prepare a precursor solution with a cation molar ratio of (Cu+Ag) / (Zn+Cd+Sn)=1.12, (Zn+Cd) / Sn=0.75, Tu / (Cu+Ag+Zn+Cd+Sn)=1.7, 0.05≤Ag / (Ag+Cu)≤0.15, 0.03≤Cd / (Cd+Zn)≤0.12. The precursor solution is spin-coated on the GeO2 film in a glove box filled with nitrogen, the spin-coating speed is 2000r / min, the spin-coating time is 40s, and annealed on a hot stage at 300°C for 2min. The spin coating-annealing operation was repeated 7-8 times to obtain a 1 μm thick precursor film containing silver, cadmium, copper, zinc, tin, sulfur and selenium. At this point, the preparation of the prefabricated layer film containing the three alloy elements of silver, cadmium and germanium was completed.
[0069] Step S3, selenization to form a multi-element alloyed copper-zinc-tin-sulfur-selenium film.
[0070] In step S3, the prepared prefabricated layer film containing multiple alloy elements and 0.8g of selenium particles are placed in a rapid heating furnace, annealed at 540°C for 20 minutes under a nitrogen flow, and naturally cooled to obtain a multi-element alloyed copper, zinc, tin, sulfur and selenium absorption layer with a thickness of 1.2μm.
[0071] Step S4, preparing a CdS buffer layer.
[0072] In step S4, a 30 nm thick CdS film is prepared as a buffer layer by chemical water bath deposition.
[0073] Step S5, preparing a ZnO / ITO window layer.
[0074] In step S5, a 40 nm thick intrinsic ZnO (i-ZnO) film and a 200 nm thick ITO film are sequentially prepared as window layers by magnetron sputtering.
[0075] Step S6, preparing a Ni / Al top gate electrode.
[0076] In step S6, a 20 nm thick Ni and a 2 μm thick Al are sequentially prepared as top gate electrodes by using a vacuum thermal evaporation method in combination with a mask.
[0077] A specific embodiment of the method for preparing a copper-zinc-tin-sulfur-selenium solar cell (hereinafter referred to as a multi-element alloyed copper-zinc-tin-sulfur-selenium solar cell) including a multi-element alloyed copper-zinc-tin-sulfur-selenium absorption layer of the present invention is described in detail above, but the present invention is not limited thereto. The specific implementation of each step may be different depending on the situation. For example, in some embodiments, the substrate may be a flexible / rigid molybdenum foil, and the back electrode layer may not be prepared. In some embodiments, the absorption layer precursor film may be prepared by sputtering Cu, Zn, and Sn metal stacking layers. In some embodiments, the alloying elements may not be Ag, Cd, or Ge. In some embodiments, the precursor film may be sulfurized. In some embodiments, the buffer layer may be a thin film such as (Zn, Cd)S, (Zn, Mg)O, etc. In some embodiments, the preparation of ZnO may be omitted. In some embodiments, the window layer may be made of aluminum-doped zinc oxide (AZO).
[0078] The above describes various embodiments of the multi-element alloyed copper-zinc-tin-sulfur-selenium solar cell of the present invention, which will be described in detail below in conjunction with some more specific embodiments. Those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.
[0079] Example 1 to Example 12
[0080] In these embodiments, a copper-zinc-tin-sulfur-selenium solar cell including a multi-element alloy is prepared by the following steps:
[0081] (1) A Mo back electrode is prepared on a soda-lime glass substrate according to the method and process parameters described in step S1 above.
[0082] (2) According to the aforementioned step S2, a GeO2 film is prepared, and the thickness of the GeO2 film is regulated by controlling the concentration of the GeO2 solution, thereby regulating the Ge content (expressed as the Ge / Sn ratio) doped into the copper-zinc-tin-sulfur-selenium absorption layer. The specific process parameters are shown in Table 1. According to the aforementioned step S2, a copper-zinc-tin-sulfur-selenium precursor film containing silver and cadmium is prepared, and the Ag and Cd contents doped into the copper-zinc-tin-sulfur-selenium absorption layer are regulated by controlling the concentrations of AgCl and CdCl2 in the precursor solution. The specific process parameters are shown in Table 1.
[0083] (3) preparing a multi-element alloyed copper-zinc-tin-sulfur-selenium absorption layer by selenization reaction according to the method and process parameters described in the aforementioned step S3.
[0084] (4) According to the aforementioned steps S4 to S6, a buffer layer, a window layer and a top gate electrode are sequentially prepared on the multi-element alloyed copper-zinc-tin-sulfur-selenium absorption layer to prepare a complete battery.
[0085] Table 1
[0086] Ag / (Ag+Cu) Cd / (Cd+Zn) <![CDATA[GeO2 concentration (g / ml)]]> Example 1 0.05 0.06 0.07 Example 2 0.10 0.06 0.07 Example 3 0.15 0.06 0.07 Example 4 0.10 0.03 0.07 Example 5 0.10 0.09 0.07 Example 6 0.10 0.12 0.07 Example 7 0.10 0.06 0.04 Example 8 0.10 0.06 0.10 Example 9 0.10 0.06 0.13 Example 10 0.10 0 0.07 Embodiment 11 0.10 0 0.07 Example 12 0 0.06 0.07
[0087] Comparative Examples 1 to 4
[0088] The difference between Comparative Examples 1 to 4 and the aforementioned Examples 1 to 12 is that the Comparative Examples contain no or only one type of cation to participate in alloying. The specific process parameters are shown in Table 2.
[0089] Table 2
[0090]
[0091]
[0092] Table 3 below lists the performance test data of the copper-zinc-tin-sulfur-selenium solar cells obtained in the aforementioned Examples 1-12 and Comparative Examples 1-4.
[0093] Table 3
[0094]
[0095]
[0096] Figure 3 The extraction efficiency η of the solar cells of Example 2 and Comparative Example 1 is shown. E and collection efficiency η C Graph of the curve. Figure 4 The fluorescence spectra of the copper-zinc-tin-sulfur-selenium absorption layers of Example 2 and Comparative Example 1 at 12K are shown.
[0097] It can be seen from Tables 1 to 3 that the introduction of three cations of silver, cadmium and germanium into the copper-zinc-tin-sulfur-selenium absorption layer in the present invention can effectively improve the device performance of the copper-zinc-tin-sulfur-selenium solar cell. It can be seen from the data in the table that the best configuration is Ag / (Ag+Cu)=0.10, Cd / (Cd+Zn)=0.06 and the GeO2 solution concentration is 0.07g / ml.
[0098] The main reason for the improved performance of the copper-zinc-tin-sulfur-selenide solar cells in each experimental example is that the incorporation of silver, cadmium, and germanium cations changes the selenization kinetics of the copper-zinc-tin-sulfur-selenide thin film. These three cations promote the fusion of the Cu2SnSe3 phase and the ZnSe phase during the selenization process, thereby suppressing the formation of deep defect Sn Zn The formation of Figure 3 It can be seen that the extraction efficiency (η E ) is significantly enhanced at high voltage, even higher than the collection efficiency (η C ), which indicates that the non-radiative recombination loss of charge in this CuZnSSe solar cell is reduced. By fitting η E The defect density is obtained. The defect density of the copper-zinc-tin-sulfur-selenium solar cell prepared in Example 2 is about one order of magnitude lower than that of the copper-zinc-tin-sulfur-selenium solar cell prepared in Comparative Example 1. Figure 4 It can be seen that compared with the copper-zinc-tin-sulfur-selenium absorption layer prepared in comparative example 1, the red shift of the fluorescence peak (relative to the band gap) of the absorption layer prepared in Example 2 is reduced by about 20 meV, which indicates that the potential fluctuation caused by deep defects is reduced, proving the reduction of deep defects in Example 2. Thanks to the reduction in charge loss, the performance of the multi-element alloyed copper-zinc-tin-sulfur-selenium solar cell is significantly improved.
[0099] In the embodiments 1-12 of the present invention, three cation alloys of silver, cadmium and germanium are introduced. The introduction of these three cations reduces the strength of the Zn-Se bond and reduces the stability of the Cu2SnSe3 intermediate phase, so that the ZnSe phase merges with the Cu2SnSe3 phase faster and better during the selenization process, thereby inhibiting the Sn Zn The formation of deep defects. The reduction of deep defects leads to a reduction in charge loss caused by them, thus obtaining a copper-zinc-tin-sulfur-selenium solar cell with significantly improved performance.
[0100] In the description provided herein, a large number of specific details are described. However, it is understood that embodiments of the present invention can be practiced without these specific details. In some instances, well-known methods, structures and techniques are not shown in detail so as not to obscure the understanding of this description.
[0101] At this point, those skilled in the art should recognize that, although multiple exemplary embodiments of the present invention have been shown and described in detail herein, many other variations or modifications that conform to the principles of the present invention can still be directly determined or derived based on the content disclosed in the present invention without departing from the spirit and scope of the present invention. Therefore, the scope of the present invention should be understood and recognized as covering all these other variations or modifications.
Claims
1. A multi-element alloyed copper, zinc, tin, sulfur and selenium absorption layer, characterized in that: The absorption layer contains at least two non-intrinsic cations participating in alloying.
2. The multi-element alloyed copper-zinc-tin-sulfur-selenium absorption layer according to claim 1, characterized in that: The at least two extrinsic cations include at least two of silver ions, cadmium ions, germanium ions, barium ions, and silicon ions.
3. The multi-element alloyed copper-zinc-tin-sulfur-selenium absorption layer according to claim 2, characterized in that: The at least two non-intrinsic cations are silver ions and germanium ions, cadmium ions and germanium ions, or silver ions, cadmium ions and germanium ions.
4. The multi-element alloyed copper-zinc-tin-sulfur-selenium absorption layer according to claim 3, characterized in that: In the absorber layer, Ge / Sn≤0.01 on a molar basis; and When silver ions are present, 0.05≤Ag / (Ag+Cu)≤0.15; When cadmium ions are present, 0.03≤Cd / (Cd+Zn)≤0.
12.
5. The method for preparing the multi-element alloyed copper, zinc, tin, sulfur and selenium absorption layer according to any one of claims 1 to 4, comprising: preparing a prefabricated precursor film containing intrinsic cations of copper, zinc and tin, at least two extrinsic cations, and sulfur or selenium; The prefabricated precursor film is subjected to selenization annealing or sulfurization annealing to form a multi-element alloyed copper-zinc-tin-sulfur-selenium thin film.
6. The preparation method according to claim 5, characterized in that: The prefabricated precursor film is prepared by a solution method, a vacuum method, an electrochemical deposition method or a nanocrystal method.
7. The preparation method according to claim 5, characterized in that: The non-intrinsic cations are introduced into the prefabricated precursor film by sputtering, evaporation, ion implantation or solution method.
8. A copper-zinc-tin-sulfur-selenium solar cell, characterized in that: It comprises a multi-element alloyed copper, zinc, tin, sulfur and selenium absorption layer according to any one of claims 1 to 4.
9. The copper-zinc-tin-sulfur-selenium solar cell according to claim 8, characterized in that: Also includes: A substrate, a back electrode, a buffer layer, a window layer and a top gate electrode, wherein the substrate, the back electrode, the multi-element alloyed copper-zinc-tin-sulfur-selenium absorption layer, the buffer layer, the window layer and the top gate electrode are stacked sequentially from bottom to top.
10. The copper-zinc-tin-sulfur-selenium solar cell according to claim 9, characterized in that: The back electrode is a molybdenum electrode; and / or The material of the buffer layer is one or more of CdS, (Zn, Cd)S and (Zn, Mg)O; and / or The window layer is a ZnO / ITO double-layer structure or an AZO single-layer structure; and / or The top gate electrode is a Ni / Al double-layer electrode, an Al single-layer electrode or an Ag single-layer electrode.