Lithium ion multilayer pole piece and preparation method and application thereof

By adopting a multi-layer structure design and micro-channel structure on the lithium-ion battery electrode, combining conductive carbon nanofiber film and optimized particle size distribution of active substances, the problem of insufficient liquid absorption capacity of thick-coated electrode sheets is solved, and the battery is improved Energy density and cycle life improve battery performance and safety.

CN119092644APending Publication Date: 2024-12-06XIAOGAN CORNEX NEW ENERGY INNOVATION TECHNOLOGY CO LTD

Patent Information

Application Number
CN202411291179.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-14
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing thick-coated lithium-ion battery poles have poor liquid absorption and liquid retention capabilities, resulting in poor rate performance and circulation performance, and increased active lithium loss and internal resistance during charging and discharging at high and low temperatures.

Method used

Using a multi-layer electrode sheet structure design, including loading the first film layer and the second film layer sequentially on the current collector surface, etching the microchannels on the second film layer and covering the conductive carbon nanofiber film, optimizing the particle size distribution and conduction of the active substance Agent types to improve the energy density and cycle life of the battery.

Benefits of technology

Through the multi-layer structure design and micro-channel structure, the embedded and release rate of lithium ions is improved, the charging and discharge speed and cycle life of the battery are enhanced, the cohesion and wettability of the electrode sheet are improved, and the energy density and safety performance are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119092644A_ABST
    Figure CN119092644A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of lithium battery preparation, and particularly relates to a lithium ion multi-layer pole piece and a preparation method and application thereof, and the lithium ion multi-layer pole piece comprises a current collector; the first film layer and the second film layer are sequentially loaded on at least one surface of the current collector; a micro-channel is etched on the upper surface of the second film layer; a conductive carbon nanofiber film which is implanted into the microchannel and covers the surface of the second film layer is arranged on the upper surface of the second film layer. The micro-channel is etched on the upper surface of the second film layer, and the conductive carbon nanofiber film which is implanted into the micro-channel and covers the surface of the second film layer is further arranged on the upper surface of the second film layer, so that the ion transmission speed is increased, and the liquid absorption and retention capability of the thick coating pole piece is improved; therefore, the wettability of the pole piece can be greatly improved, and the cycle performance and the safety performance of an energy density system can be effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of lithium battery preparation, and specifically relates to a lithium ion multilayer pole piece and a preparation method and application thereof. Background Art

[0002] Lithium-ion battery is a common secondary battery widely used in mobile devices, electric vehicles, energy storage systems and other fields. It realizes the charging and discharging process by the insertion and deintercalation of lithium ions between the positive and negative electrodes. Compared with traditional disposable batteries, lithium-ion batteries have the advantages of high energy density, long cycle life and no memory effect.

[0003] Lithium-ion batteries are mainly composed of positive electrode sheets, negative electrode sheets, electrolytes, separators and battery shells. Among them, the positive electrode sheet of lithium-ion batteries is an important component in lithium-ion batteries that stores and releases lithium ions. It is usually composed of active materials, conductive agents and binders. The active material can be lithium manganese oxide, lithium cobalt oxide, ternary materials, etc. The conductive agent is used to improve the conductivity of the electrode, and the binder is used to bond the active material and the conductive agent together.

[0004] At present, high energy density lithium iron phosphate batteries are developing towards high compaction of pole pieces, accompanied by thick coating of pole pieces. Therefore, the liquid absorption and liquid retention capabilities of pole pieces are required to be high. By improving the liquid absorption and liquid retention capabilities of high compaction and thick coating lithium iron phosphate pole pieces, the development of lithium iron phosphate batteries in the direction of high energy and long life can be promoted, and its application in other fields can be promoted.

[0005] However, existing thick-coated pole pieces are conventionally coated directly, resulting in poor adhesion of the pole pieces, long electrolyte wettability and infiltration time, and thus poor rate performance and later cycle performance of lithium-ion batteries.

[0006] In some existing patented technologies, double-layer coating or pore-making technology is usually used to coat thick electrodes and increase the wettability of the electrolyte, but this will reduce the cohesion of the electrode and destroy the adhesion between the electrode materials, thereby leading to a sharp drop in high and low temperature charging and discharging or cycle performance, loss of active lithium and increase in internal resistance. Summary of the invention

[0007] The present invention aims to overcome the defects of poor liquid absorption and liquid retention capabilities of thick-coated pole pieces in the prior art, and thus provides a lithium-ion multilayer pole piece and a preparation method and application thereof to overcome the above defects.

[0008] In a first aspect, the present invention first provides a lithium ion multilayer electrode sheet. including a current collector; and, A first film layer and a second film layer sequentially loaded on at least one surface of a current collector; A microchannel is etched on the upper surface of the second film layer; A conductive carbon nanofiber film is disposed on the upper surface of the second membrane layer, which is embedded in the microchannel and covers the surface of the second membrane layer.

[0009] The lithium-ion pole piece in the present application adopts a multi-layer structure design, and the energy density and power density of the battery can be increased by sequentially loading the first film layer and the second film layer on the surface of the current collector. The multi-layer structure can provide a larger surface area, increase the insertion and release rate of lithium ions, and thus improve the charge and discharge speed of the battery. Moreover, through the design of this type of multi-layer film structure, the pole piece can effectively meet the requirements of high coating amount and high compaction in a high energy density system.

[0010] Moreover, on this basis, the microchannels etched on the upper surface of the second film layer increase the contact area between the positive electrode of the battery and the electrolyte, and create a porous passage, thereby increasing the ion transmission speed and increasing the liquid absorption and retention capacity of the thick coating electrode. In addition, the microchannel can promote the diffusion and conduction of ions, reduce the internal resistance of the battery, and improve the performance and cycle life of the battery.

[0011] Finally, the present application also provides a conductive carbon nanofiber film on the upper surface of the second film layer, which is embedded in the microchannel and covers the surface of the second film layer. This film has good conductivity, can improve the conductivity of the battery, reduce the internal resistance of the battery, and improve the energy conversion efficiency of the battery.

[0012] At the same time, the electrolyte can also be transported to the microchannel using the carbon nanotubes in the conductive carbon nanofiber film as a carrier to supply sufficient electrolyte to the electrode. The carbon nanotubes have a large specific surface area and strong liquid absorption and retention capabilities, which can greatly improve the wettability of the electrode and effectively improve the cycle performance and safety performance of the energy density system.

[0013] Preferably, the first film layer contains a first positive electrode active material; The second film layer contains a second active substance; wherein, The particle size of the first positive electrode active material is larger than that of the second active material.

[0014] In this application, the particle size of the positive electrode active material in the first film layer and the second film layer is specifically designed. Specifically, in this application, the particle size of the first positive electrode active material in the first film layer is larger than the particle size of the second active material in the second film layer. The reason is that the first positive electrode active material with a larger particle size forms larger particles on the surface of the current collector, and the contact area between these particles is smaller, thereby reducing the bonding area. However, since the particles with larger particle sizes are relatively heavy, they are more likely to form a good physical connection on the surface of the current collector, thereby improving the cohesion of the pole piece. This first positive electrode active material with a larger particle size can effectively prevent the bonding failure between the electrode materials and improve the stability and reliability of the pole piece.

[0015] At the same time, there are larger gaps between the particles of the first positive electrode active material with a larger particle size, which are conducive to the transmission of lithium ions in the electrolyte. Lithium ions can diffuse into the electrolyte faster through these gaps, thereby increasing the ion transmission rate of the battery. This rapid ion transmission helps to reduce the resistance within the pole piece and improve the performance of the battery.

[0016] The second active material in the second film layer has a smaller particle size and a larger surface area than the first positive electrode active material in the first film layer, so it is easier to embed and release lithium ions. By placing active materials with smaller particle sizes in the second film layer, the cycle life of the battery can be improved. Active materials with smaller particle sizes are beneficial to reducing stress and loss during the embedding and release of lithium ions, slowing down the capacity decay rate of the battery.

[0017] In addition, the distribution of active materials with different particle sizes in the first film layer and the second film layer helps to optimize the performance and stability of the battery. The large particle size active material in the first film layer can provide higher energy density, while the small particle size active material in the second film layer provides better cycle life and stability. By rationally designing the particle size distribution of the active material, the purpose of balancing battery performance and cycle life can be achieved.

[0018] Preferably, the particle size D50 of the first positive electrode active material is greater than 1 μm; The particle size D50 of the second active material is ≤1 μm.

[0019] Preferably, the first film layer comprises, by weight percentage, 96-97% of the first positive electrode active material, 1-2% of the conductive agent, and 1-2% of the binder; The second film layer contains 97-98% of the second active material, 0.3-1.5% of the conductive agent and 1.2-1.7% of the binder in terms of weight percentage.

[0020] Preferably, the first positive electrode active material in the first film layer is any one of lithium iron phosphate and lithium manganese iron phosphate, or a mixture of the two; The conductive agent in the first film layer is a mixture of any one or more of SP, KS-6, and acetylene black; The second active material in the second film layer is any one of lithium iron phosphate and lithium manganese iron phosphate or a mixture of the two; The conductive agent in the second film layer has a diameter of less than 8 nm, a length of less than 30 μm, and a specific surface area of ​​more than 100 m 2 / g of carbon nanotubes.

[0021] The types of conductive agents used in the first film layer and the second film layer in this application are different because the conductive agents (SP, KS-6, acetylene black) in the first film layer are relatively common and easy to obtain, and have lower costs than carbon nanotubes. This can reduce manufacturing costs and improve the economy of batteries for large-scale production and commercial applications. At the same time, conductive agents such as SP, KS-6 and acetylene black can form good interface contact with active materials and binders, which helps to improve the structural stability and electronic conductivity of electrode materials. This helps to reduce electrode polarization and improve charge and discharge efficiency and power performance.

[0022] The carbon nanotubes in the second film layer, as a conductive agent, have a high specific surface area and conductivity, which can promote electron transfer and ion diffusion, and improve the cycle stability and capacity retention rate of the battery. In addition, carbon nanotubes can also increase the stability of the electrode structure and reduce the loss and peeling of electrode materials. And carbon nanotubes have good liquid absorption and liquid retention capabilities, so they can introduce external electrolyte into the interior of the electrode, thereby greatly improving the wettability of the electrode.

[0023] Preferably, the width of the microchannel is 8 μm to 15 μm; The depth of the microchannel is 5 μm-15 μm; The spacing between the microchannels is 10 cm-20 cm.

[0024] Preferably, the single-sided surface density of the first film layer is 15-20 mg / cm 2 ; The single surface density of the second film layer is 15-20 mg / cm 2 ; The implanted thickness of the conductive carbon nanofiber film is 30-50 μm.

[0025] In a second aspect, the present invention also provides a method for preparing the lithium ion multilayer electrode sheet as described above. The following steps are involved: (S.1) respectively mixing raw material components for preparing the first membrane layer and the second membrane layer with a solvent to obtain a first membrane layer slurry and a second membrane layer slurry; (S.2) coating the first film layer slurry on at least one surface of the positive electrode current collector, and obtaining the first film layer after drying; (S.3) coating the second film layer slurry on the surface of the first film layer, and obtaining the second film layer after drying; (S.4) Flattening and positioning the positive electrode sheet, aligning the front and back surfaces of the electrode sheet with a laser, and longitudinally etching the electrode sheet to construct a microchannel for electrolyte transmission on the surface of the electrode sheet; (S.5) preparing a conductive adhesive by mixing carbon nanotubes, a binder and a solvent, implanting the conductive adhesive into the microchannel and the surface of the second membrane layer by electrospinning technology, and obtaining a conductive carbon nanofiber film after drying; (S.6) Roll-pressing the above-mentioned electrode sheet to obtain the lithium-ion multilayer electrode sheet.

[0026] Preferably, in the step (S.1), the solid content of the first membrane layer slurry and the second membrane layer slurry is 55%-65%, and the discharge viscosity is 4000-7000 mPa.s.

[0027] Preferably, the specific surface area of ​​the carbon nanotubes in step (S.5) is 1000-2000 m 2 / g, pore volume 0.4ml / g -2.0ml / g.

[0028] Preferably, the compaction density in step (S.6) is 2.5-2.7 g / cm 3 .

[0029] In a third aspect, the present invention further provides a lithium-ion battery comprising a lithium-ion multilayer electrode sheet as described in any one of the above.

[0030] Therefore, the present invention has the following beneficial effects: The lithium ion multilayer pole piece in the present invention is composed of a conductive carbon nanofiber film (electrospinning layer), a second film layer, a first film layer and a current collector from top to bottom. The composite film has a high surface density and can effectively meet the requirements of high coating amount and high compaction under a high energy density system; by including carbon microtubes in at least one layer of the second film layer and the third film layer, the purpose of improving the charging performance of the battery is achieved. At the same time, the electrolyte is transmitted to the microchannel with carbon nanotubes as carriers to supply the pole piece with sufficient electrolyte. The carbon nanotubes have a large specific surface area and strong liquid absorption and liquid retention capabilities, which greatly improves the wettability of the pole piece and can effectively improve the cycle performance and safety performance of the energy density system. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 This is a raw material diagram of each layer of the lithium-ion multilayer electrode of the present invention.

[0032] Figure 2 It is a schematic diagram of the structure of the lithium-ion multilayer electrode of the present invention.

[0033] Figure 3 1C charge-discharge cycle life curve of the battery prepared by the lithium-ion multilayer electrode sheets in Example 1 and Comparative Example 1.

[0034] Among them: 1 is the current collector; 2 is the first membrane layer; 3 is the second membrane layer; 4 is the microchannel; 5 is the conductive carbon nanofiber film. DETAILED DESCRIPTION

[0035] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments of the specification. Those of ordinary skill in the art will be able to implement the present invention based on these descriptions. In addition, the embodiments of the present invention involved in the following description are generally only embodiments of a part of the present invention, rather than all embodiments. Therefore, based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work should fall within the scope of protection of the present invention.

[0036] Example 1 A method for preparing a lithium-ion multilayer electrode sheet, the specific method is as follows: Step 1: Figure 1 As shown, the raw material components for preparing the first film layer, such as the first positive electrode active material (LFP with large particles D50>1μm), the conductive agent (SP) and the binder (PVDF), are added to the solvent (NMP) in a ratio of 96:2:2, and the solid content is ensured to be 60%, and the discharge viscosity is 5000mPa.s. After being stirred evenly, a slurry of the first film layer is formed, which is also called the first film layer slurry; Step 2: Figure 1 As shown, the raw material components for preparing the second film layer, such as the second active material (D50≤1μm small particle LFP), carbon nanotubes (diameter <8nm, length <30μmm, specific surface area >100m 2 / g) and binder (PVDF) are added to the solvent (NMP) in a certain ratio of 98:0.5:1.5, and mixed evenly to form the slurry of the second membrane layer, ensuring that the solid content is 60% and the discharge viscosity is 5000mPa.s, also known as the second membrane layer slurry; Step 3: Apply the first film layer slurry prepared in step 1 above to at least one surface of the positive electrode current collector to ensure that the single-surface surface density is 18 mg / cm 2 Then the second film layer slurry prepared in step 2 is coated on the surface of the first film layer to ensure that the single-sided surface density is 12 mg / cm 2After drying, the second film layer (middle layer) is obtained.

[0037] Step 4: After the second film layer is applied, the positive electrode is flattened and positioned, and the front and back surfaces of the electrode are aligned with a laser and etched longitudinally at the same time. During the laser etching process, the etched part of the electrode is vacuumed and dusted to ensure that the dust on the surface of the electrode is qualified, thereby constructing an electrolyte transmission microchannel on the surface of the electrode, controlling the microchannel width to 10μm, the microchannel depth to 12μm, and the microchannel spacing on the surface of the electrode to 15cm.

[0038] Step 5: Prepare a conductive glue solution with carbon nanotubes, a binder and a solvent. The carbon nanotube content in the conductive glue solution is 30%. The carbon nanotubes are implanted into the microchannel and the surface of the second membrane layer by electrospinning technology to form a conductive carbon nanofiber film (upper layer). The implanted carbon nanotubes have a thickness of 40 μm and a specific surface area of ​​1500 m 2 / g, pore volume 1.0 ml / g, the electrolyte is transported to the microchannel with carbon nanotubes as carrier to supply enough electrolyte to the electrode. Carbon nanotubes have strong liquid absorption and liquid retention capabilities, which greatly improves the wettability of the electrode.

[0039] The structure of the prepared lithium ion multilayer electrode is as follows: Figure 2 As shown, it includes a current collector 1, the upper surface of the current collector 1 is a first film layer 2, the upper surface of the first film layer 2 is a second film layer 3, the upper surface of the second film layer 3 is provided with a microchannel 4, and the upper surface of the second film layer 3 is also provided with a layer of conductive carbon nanofiber film 5 implanted in the microchannel 4 and covering the surface of the second film layer 3.

[0040] Step 6: Compact the above-mentioned electrode according to the compaction density of 2.6g / cm 3 After roller pressing, the positive electrode sheet is manufactured.

[0041] Example 2 A method for preparing a lithium-ion multilayer electrode sheet, the specific method is as follows: Step 1: Add the raw material components for preparing the first film layer, such as the first positive electrode active material (D50>1μm large particle LMFP), the conductive agent (acetylene black) and the binder (PVDF), into the solvent (NMP) in a ratio of 97:2:1, and mix them to ensure that the solid content is 60% and the discharge viscosity is 5000mPa.s. After stirring evenly, a slurry of the first film layer is formed, which is also called the first film layer slurry; Step 2: Prepare the raw material components of the second film layer, such as the second active material (D50≤1μm small particle LFP), carbon nanotubes (diameter <8nm, length <30μmm, specific surface area >100m 2 / g) and binder (PVDF) are added to the solvent (NMP) in a certain ratio of 98:0.5:1.5, and mixed evenly to form the slurry of the second membrane layer, ensuring that the solid content is 55% and the discharge viscosity is 4000mPa.s, also known as the second membrane layer slurry; Step 3: Apply the first film layer slurry prepared in step 1 above to at least one surface of the positive electrode current collector to ensure that the single-surface surface density is 15 mg / cm 2 Then the second film layer slurry prepared in step 2 is coated on the surface of the first film layer to ensure that the single-sided surface density is 15 mg / cm 2 After drying, the second film layer (middle layer) is obtained.

[0042] Step 4: After the second film layer is applied, the positive electrode is flattened and positioned, and the front and back surfaces of the electrode are aligned with a laser and etched longitudinally at the same time. During the laser etching process, the etched part of the electrode is vacuumed and dusted to ensure that the dust on the surface of the electrode is qualified, thereby constructing an electrolyte transmission microchannel on the surface of the electrode, controlling the microchannel width to 8μm, the microchannel depth to 15μm, and the microchannel spacing on the surface of the electrode to 10cm.

[0043] Step 5: Prepare a conductive glue solution with carbon nanotubes, a binder and a solvent. The carbon nanotube content in the conductive glue solution is 30%. The carbon nanotubes are implanted into the microchannel and the surface of the second membrane layer by electrospinning technology to form a conductive carbon nanofiber film (upper layer). The implanted carbon nanotubes have a thickness of 50 μm and a specific surface area of ​​2000 m 2 / g, pore volume 2.0 ml / g, the electrolyte is transported to the microchannel with carbon nanotubes as carrier to supply enough electrolyte to the electrode. Carbon nanotubes have strong liquid absorption and liquid retention capabilities, which greatly improves the wettability of the electrode.

[0044] Step 6: Compact the above-mentioned pole piece at a density of 2.5g / cm 3 After roller pressing, the positive electrode sheet is manufactured.

[0045] Example 3 A method for preparing a lithium-ion multilayer electrode sheet, the specific method is as follows: Step 1: Add the raw material components for preparing the first film layer, such as the first positive electrode active material (D50>1μm large particle LMFP), the conductive agent (acetylene black) and the binder (PVDF), to the solvent (NMP) in a ratio of 97:1:2, and mix them to ensure that the solid content is 65% and the discharge viscosity is 7000mPa.s. After stirring evenly, a slurry of the first film layer is formed, which is also called the first film layer slurry; Step 2: Prepare the raw material components of the second film layer, such as the second active material (small particles LMFP with a D50 of ≤ 1 μm), carbon nanotubes (diameter < 8 nm, length < 30 μ mm, specific surface area > 100 m 2 / g) and binder (PVDF) are added to the solvent (NMP) in a certain ratio of 98:0.5:1.5, and mixed evenly to form the slurry of the second membrane layer, ensuring that the solid content is 65% and the discharge viscosity is 7000mPa.s, also known as the second membrane layer slurry; Step 3: Apply the first film layer slurry prepared in step 1 above to at least one surface of the positive electrode current collector to ensure that the single-surface surface density is 20 mg / cm 2 Then the second film layer slurry prepared in step 2 is coated on the surface of the first film layer to ensure that the single-sided surface density is 12 mg / cm 2 After drying, the second film layer (middle layer) is obtained.

[0046] Step 4: After the second film layer is applied, the positive electrode is flattened and positioned, and the front and back surfaces of the electrode are aligned with a laser and etched longitudinally at the same time. During the laser etching process, the etched part of the electrode is vacuumed and dusted to ensure that the dust on the surface of the electrode is qualified, thereby constructing an electrolyte transmission microchannel on the surface of the electrode, controlling the microchannel width to 15μm, the microchannel depth to 5μm, and the microchannel spacing on the surface of the electrode to 20cm.

[0047] Step 5: Prepare a conductive glue solution with carbon nanotubes, a binder and a solvent. The carbon nanotube content in the conductive glue solution is 30%. The carbon nanotubes are implanted into the microchannel and the surface of the second membrane layer by electrospinning technology to form a conductive carbon nanofiber film (upper layer). The implanted carbon nanotubes have a thickness of 30 μm and a specific surface area of ​​1000 m 2 / g, pore volume 0.4 ml / g, the electrolyte is transported to the microchannel with carbon nanotubes as carrier to supply enough electrolyte to the electrode. Carbon nanotubes have strong liquid absorption and liquid retention capabilities, which greatly improves the wettability of the electrode.

[0048] Step 6: Compact the above-mentioned electrode according to the compaction density of 2.7g / cm 3 After roller pressing, the positive electrode sheet is manufactured.

[0049] Example 4 A method for preparing a lithium-ion multilayer electrode sheet, the specific method is as follows: Step 1: Add the raw material components for preparing the first film layer, such as the first positive electrode active material (D50>1μm large particle LMFP), the conductive agent (KS-6) and the binder (PVDF), to the solvent (NMP) in a ratio of 97:1.5:1.5, and mix them to ensure that the solid content is 60% and the discharge viscosity is 5000mPa.s. After stirring evenly, a slurry of the first film layer is formed, which is also called the first film layer slurry; Step 2: Prepare the raw material components of the second film layer, such as the second active material (small particles LMFP with a D50 of ≤ 1 μm), carbon nanotubes (diameter < 8 nm, length < 30 μ mm, specific surface area > 100 m 2 / g) and binder (PVDF) are added to the solvent (NMP) in a certain ratio of 97:1.3:1.7, and mixed evenly to form the slurry of the second membrane layer, ensuring that the solid content is 65% and the discharge viscosity is 7000mPa.s, also known as the second membrane layer slurry; Step 3: Apply the first film layer slurry prepared in step 1 above to at least one surface of the positive electrode current collector to ensure that the single-surface surface density is 20 mg / cm 2 Then the second film layer slurry prepared in step 2 is coated on the surface of the first film layer to ensure that the single-sided surface density is 12 mg / cm 2 After drying, the second film layer (middle layer) is obtained.

[0050] Step 4: After the second film layer is applied, the positive electrode is flattened and positioned, and the front and back surfaces of the electrode are aligned with a laser and etched longitudinally at the same time. During the laser etching process, the etched part of the electrode is vacuumed and dusted to ensure that the dust on the surface of the electrode is qualified, thereby constructing an electrolyte transmission microchannel on the surface of the electrode, controlling the microchannel width to 10μm, the microchannel depth to 10μm, and the microchannel spacing on the surface of the electrode to 10cm.

[0051] Step 5: Prepare a conductive glue solution with carbon nanotubes, a binder and a solvent. The carbon nanotube content in the conductive glue solution is 30%. The carbon nanotubes are implanted into the microchannel and the surface of the second membrane layer by electrospinning technology to form a conductive carbon nanofiber film (upper layer). The implanted carbon nanotubes have a thickness of 30 μm and a specific surface area of ​​1000 m 2 / g, pore volume 0.4 ml / g, the electrolyte is transported to the microchannel with carbon nanotubes as carrier to supply enough electrolyte to the electrode. Carbon nanotubes have strong liquid absorption and liquid retention capabilities, which greatly improves the wettability of the electrode.

[0052] Step 6: Compact the above-mentioned electrode according to the compaction density of 2.7g / cm 3 After roller pressing, the positive electrode sheet is manufactured.

[0053] Example 5 A method for preparing a lithium-ion multilayer electrode sheet, the specific method is as follows: Step 1: Add the raw material components for preparing the first film layer, such as the first positive electrode active material (D50>1μm large particle LMFP), the conductive agent (KS-6) and the binder (PVDF), to the solvent (NMP) in a ratio of 97:1.5:1.5, and mix them to ensure that the solid content is 60% and the discharge viscosity is 5000mPa.s. After stirring evenly, a slurry of the first film layer is formed, which is also called the first film layer slurry; Step 2: Prepare the raw material components of the second film layer, such as the second active material (small particles LMFP with a D50 of ≤ 1 μm), carbon nanotubes (diameter < 8 nm, length < 30 μ mm, specific surface area > 100 m 2 / g) and binder (PVDF) are added to the solvent (NMP) in a certain ratio of 98:0.8:1.2, and mixed evenly to form the slurry of the second membrane layer, ensuring that the solid content is 60% and the discharge viscosity is 5000mPa.s, also known as the second membrane layer slurry; Step 3: Apply the first film layer slurry prepared in step 1 above to at least one surface of the positive electrode current collector to ensure that the single-surface surface density is 18 mg / cm 2 Then the second film layer slurry prepared in step 2 is coated on the surface of the first film layer to ensure that the single-sided surface density is 15 mg / cm 2 After drying, the second film layer (middle layer) is obtained.

[0054] Step 4: After the second film layer is applied, the positive electrode is flattened and positioned, and the front and back surfaces of the electrode are aligned with a laser and etched longitudinally at the same time. During the laser etching process, the etched part of the electrode is vacuumed and dusted to ensure that the dust on the surface of the electrode is qualified, thereby constructing an electrolyte transmission microchannel on the surface of the electrode, controlling the microchannel width to 10μm, the microchannel depth to 10μm, and the microchannel spacing on the surface of the electrode to 10cm.

[0055] Step 5: Prepare a conductive glue solution with carbon nanotubes, a binder and a solvent. The carbon nanotube content in the conductive glue solution is 30%. The carbon nanotubes are implanted into the microchannel and the surface of the second membrane layer by electrospinning technology to form a conductive carbon nanofiber film (upper layer). The implanted carbon nanotubes have a thickness of 50 μm and a specific surface area of ​​1000 m 2 / g, pore volume 0.4 ml / g, the electrolyte is transported to the microchannel with carbon nanotubes as carrier to supply enough electrolyte to the electrode. Carbon nanotubes have strong liquid absorption and liquid retention capabilities, which greatly improves the wettability of the electrode.

[0056] Step 6: Compact the above-mentioned electrode according to the compaction density of 2.7g / cm 3 After roller pressing, the positive electrode sheet is manufactured.

[0057] Comparative Example 1 The basic steps of Comparative Example 1 are the same as those of Example 1, except that Step 4 and Step 5 are eliminated, that is, the obtained electrode only includes the first film layer and the second film layer.

[0058] Comparative Example 2 The basic steps of Comparative Example 2 are the same as those of Example 1, except that step five is eliminated, that is, the obtained electrode only includes the first film layer and the second film layer, and the surface of the second film layer includes microchannels for electrolyte transmission.

[0059] Comparative Example 3 The basic steps of Comparative Example 3 are the same as those of Example 1, except that step 4 is eliminated, i.e., the obtained electrode only includes the first membrane layer, the second membrane layer and the conductive carbon nanofiber film, and there is no microchannel for electrolyte transmission on the surface of the second membrane layer.

[0060] Comparative Example 4 Comparative Example 4 has the same basic steps as Example 1, except that the first active material (Large particle LMFP with D50>1 μm) is used in both the first film layer and the second film layer.

[0061] Comparative Example 5 The basic steps of Comparative Example 5 are the same as those of Example 1, except that the second active material (small particles LMFP with D50≤1 μm) is used in both the first film layer and the second film layer.

[0062]

Performance test

[0063] Pole cohesion test: The test process is the same as the peeling force, but the double-sided adhesive tape is replaced with green adhesive with lower viscosity.

[0064] Charge and discharge cycle life test: 1) 25℃±2℃ rest 120min; 2) 1 C CC to 3.65V, CV to 0.05C; 3) rest for 5 minutes, 4) 0.2C DC to 2.5V, denoted as C0; 5) 25℃±2℃ rest 120min; 6) rest for 5 minutes, 7) 1C0 CC to 3.65V, CV to 0.05C0; 8) rest for 5 minutes; 9) 1C0 DC to 2.5V; 10) rest for 5 minutes; 11) Repeat steps 7-10 2000 times.

[0065] The performance test results are shown in Table 1 below.

[0066] Table 1 .

[0067]

Performance Analysis

[0068] The above-described embodiments are only preferred embodiments for fully illustrating the present invention, and the protection scope of the present invention is not limited thereto. Equivalent substitutions or changes made by those skilled in the art based on the present invention are all within the protection scope of the present invention. The protection scope of the present invention shall be subject to the claims.

Claims

1. A lithium-ion multilayer electrode, It is characterized in that including a current collector; as well as, A first film layer and a second film layer sequentially loaded on at least one surface of a current collector; A microchannel is etched on the upper surface of the second film layer; A conductive carbon nanofiber film is disposed on the upper surface of the second membrane layer, which is embedded in the microchannel and covers the surface of the second membrane layer.

2. A lithium ion multilayer electrode according to claim 1, It is characterized in that The first film layer contains a first positive electrode active material; The second film layer contains a second active substance; wherein, The particle size of the first positive electrode active material is larger than that of the second active material.

3. A lithium ion multilayer electrode according to claim 2, It is characterized in that The particle size D50 of the first positive electrode active material is greater than 1 μm; The particle size D50 of the second active material is ≤1 μm.

4. A lithium ion multilayer electrode according to claim 2 or 3, It is characterized in that The first film layer comprises, by weight percentage, 96-97% of a first positive electrode active material, 1-2% of a conductive agent, and 1-2% of a binder; The second film layer contains 97-98% of the second active material, 0.3-1.5% of the conductive agent and 1.2-1.7% of the binder in terms of weight percentage.

5. A lithium ion multilayer electrode according to claim 4, It is characterized in that The first positive electrode active material in the first film layer is any one of lithium iron phosphate and lithium manganese iron phosphate or a mixture of the two; The conductive agent in the first film layer is a mixture of any one or more of SP, KS-6, and acetylene black; The second active material in the second film layer is any one of lithium iron phosphate and lithium manganese iron phosphate or a mixture of the two; The conductive agent in the second film layer has a diameter of less than 8 nm, a length of less than 30 μm, and a specific surface area of ​​more than 100 m 2 / g of carbon nanotubes.

6. A lithium ion multilayer electrode according to claim 1, It is characterized in that The width of the microchannel is 8 μm to 15 μm; The depth of the microchannel is 5 μm-15 μm; The spacing between the microchannels is 10 cm-20 cm.

7. A lithium ion multilayer electrode according to claim 1 or 2 or 3 or 6, It is characterized in that The single-sided surface density of the first film layer is 15-20 mg / cm 2 ; The single surface density of the second film layer is 12-15 mg / cm 2 ; The implanted thickness of the conductive carbon nanofiber film is 30-50 μm.

8. A method for preparing a lithium ion multilayer electrode as claimed in any one of claims 1 to 7 , It is characterized in that The following steps are involved: (S.1) respectively mixing raw material components for preparing the first membrane layer and the second membrane layer with a solvent to obtain a first membrane layer slurry and a second membrane layer slurry; (S.2) coating the first film layer slurry on at least one surface of the positive electrode current collector, and obtaining the first film layer after drying; (S.3) coating the second film layer slurry on the surface of the first film layer, and obtaining the second film layer after drying; (S.4) Flattening and positioning the positive electrode sheet, aligning the front and back surfaces of the electrode sheet with a laser, and longitudinally etching the electrode sheet to construct a microchannel for electrolyte transmission on the surface of the electrode sheet; (S.5) preparing a conductive adhesive by mixing carbon nanotubes, a binder and a solvent, implanting the conductive adhesive into the microchannel and the surface of the second membrane layer by electrospinning technology, and obtaining a conductive carbon nanofiber film after drying; (S.6) Roll-pressing the above-mentioned electrode sheet to obtain the lithium-ion multilayer electrode sheet.

9. The method according to claim 8, It is characterized in that In the step (S.1), the solid content of the first membrane layer slurry and the second membrane layer slurry is 55%-65%, and the discharge viscosity is 4000-7000 mPa.s; In the step (S.5), the specific surface area of ​​the carbon nanotubes is 1000-2000 m 2 / g, pore volume 0.4ml / g-2.0ml / g; The compacted density in step (S.6) is 2.5-2.7 g / cm 3 .

10. A lithium ion battery, It is characterized in that Comprising a lithium-ion multilayer electrode as described in any one of claims 1 to 7.

Citation Information

Patent Citations

  • Lithium ion battery pole piece and preparation method thereof

    CN105336916A

  • Carbon-coated aluminum foil and preparation method thereof

    CN109411762A

  • Method for improving wettability of lithium ion battery

    CN115632111A

  • Preparation method of high-porosity battery pole piece and solid-state battery

    CN115663108A

  • Positive pole piece and preparation method thereof, secondary battery, battery module, battery pack and power utilization device

    CN115832183A

Cited By

  • Stripped carbon nanotube, positive electrode slurry, positive electrode plate, secondary battery and electric equipment