Rechargeable lithium battery
By using polyalkylene glycol copolymers as electrolyte additives in rechargeable lithium batteries, the problem of wettability reduction caused by the increase in current density of the positive electrode plate is solved, and the uniform interface formation of lithium cations is achieved, and lithium is suppressed Dendritic crystals precipitate, improving the battery's cycle life and fast charging performance.
Patent Information
- Application Number
- CN202410719692.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-06-05
- Filing Date
- 2024-06-05
- Publication Date
- 2024-12-06
AI Technical Summary
When improving the high capacity and cycle life characteristics of rechargeable lithium batteries, the increase in current density of the positive electrode plate will lead to a decrease in wettability of the electrolyte, which will lead to the precipitation of lithium dendritics, which will damage the battery's fast charging performance and cycle life.
By adding polyalkylene glycol copolymers as surfactant to the electrolyte, the current density of the positive electrode plate and the wettability of the electrolyte are improved, thereby uniformly forming a lithium cation interface and inhibiting lithium dendritics. precipitation.
It effectively improves the cycle life characteristics and fast charging performance of rechargeable lithium batteries, ensuring high capacity and long life of the battery.
Smart Images

Figure CN119092789A_ABST
Abstract
Description
Technical Field
[0001] Embodiments of the present disclosure relate to rechargeable lithium batteries. Background Art
[0002] Rechargeable lithium batteries are rechargeable, and their energy density per unit weight is three times or more that of lead-acid batteries, nickel-cadmium batteries, nickel-metal hydride batteries, nickel-zinc batteries, etc., and can also be charged at high rates. Therefore, they have been commercially manufactured for use in laptop computers, cellular phones, power tools, electric bicycles, etc., and research on improving their additional energy density is being actively conducted.
[0003] Such a rechargeable lithium battery is used by injecting an electrolyte into a battery cell including a positive electrode plate and a negative electrode plate.
[0004] The latest development direction of rechargeable lithium batteries has involved high capacity, cycle life characteristics, fast charging performance, etc. However, if the current density of the positive electrode plate is increased to achieve high capacity of the rechargeable lithium battery, the wettability of the positive electrode plate to the electrolyte is reduced, and lithium dendrites are precipitated on the surface of the negative electrode plate (e.g., the interface between the negative electrode plate and the electrolyte), thereby deteriorating the cycle life characteristics and fast charging performance of the battery.
[0005] Accordingly, an electrolyte for improving the cycle-life characteristics and fast-charging performance of rechargeable lithium batteries and achieving high capacity would be beneficial. Summary of the invention
[0006] Some embodiments of the present disclosure improve the cycle-life characteristics and fast-charging performance of a rechargeable lithium battery by using an electrolyte additive, and ensure high capacity of the rechargeable lithium battery by increasing the current density of a positive electrode plate.
[0007] Some embodiments of the present disclosure provide a rechargeable lithium battery comprising: a positive electrode plate; a negative electrode plate; and an electrolyte including an electrolyte additive, wherein the current density of the positive electrode plate is about 5.4 mA / cm 2 ~About 6.6mA / cm 2 ; and the electrolyte additive includes a polyalkylene glycol copolymer.
[0008] In some embodiments of the rechargeable lithium battery, the electrolyte additive is used as a surfactant. Accordingly, in the rechargeable lithium battery including the electrolyte additive, even if the current density of the positive electrode plate increases, the wettability of the positive electrode plate to the electrolyte can be improved.
[0009] In addition, if the wettability of the positive electrode plate to the electrolyte is improved, the lithium cation (Li +) is uniformly (or substantially uniformly) formed at the interface between the positive electrode plate and the electrolyte, inhibiting or reducing the precipitation of lithium dendrites on the surface of the negative electrode plate, and ultimately, ensuring the cycle life characteristics and fast charging performance of the rechargeable lithium battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0010] The accompanying drawings, together with the description, illustrate embodiments of the presently disclosed subject matter, and, together with the description, serve to explain principles of embodiments of the presently disclosed subject matter.
[0011] Figure 1 is a schematic diagram illustrating a rechargeable lithium battery according to some embodiments.
[0012] Description of Reference Numerals
[0013] 100: Rechargeable lithium battery
[0014] 112: Negative electrode plate
[0015] 113: Diaphragm
[0016] 114: Positive electrode plate
[0017] 120: Battery housing
[0018] 140: Sealing member DETAILED DESCRIPTION
[0019] If no specific definition is provided otherwise, "substituted" as used herein means that at least one hydrogen of a compound is replaced by a halogen atom (F, Cl, Br or I), a hydroxyl group, a C1-C20 alkoxy group, a nitro group, a cyano group, an amine group, an imino group, an azido group, a carboxamidino group, a hydrazine group, a hydrazone group, a carbonyl group, a carbamoyl group, a thiol group, an ester group, an ether group, a carboxyl group or a salt thereof, a sulfonic acid group or a salt thereof, a phosphate group or a salt thereof, a C1-C20 alkyl group, a C2-C20 alkenyl group, a C2-C20 alkynyl group, a C6-C30 aryl group, a C3-C20 cycloalkyl group, a C3-C20 cycloalkenyl group, a C3-C20 cycloalkynyl group, a C2-C20 heterocycloalkyl group, a C2-C20 heterocycloalkenyl group, a C2-C20 heterocycloalkynyl group, or a combination thereof.
[0020] If a specific definition is not otherwise provided, "heterocycloalkyl", "heterocycloalkenyl", "heterocycloalkynyl" and "heterocycloalkylene" as used herein refer to the presence of at least one N, O, S or P in the cycloalkyl, cycloalkenyl, cycloalkynyl or cycloalkylene ring compound.
[0021] In the chemical formulae in the present specification, unless a specific definition is provided otherwise, hydrogen is bonded to a position where a chemical bond is not drawn where a chemical bond should be given.
[0022] As used herein, “current density of an electrode plate” may refer to the magnitude (density) of current flowing per unit area of a positive electrode plate or a negative electrode plate.
[0023] As used herein, “loading amount of the electrode plate” may be a value calculated by dividing the weight of components (active material, conductive material, binder, etc.) other than the current collector in the positive electrode plate or the negative electrode plate by the area of the electrode plate.
[0024] As used herein, “mixture density of an electrode plate” may be a value calculated by dividing the weight of components (active material, conductive material, binder, etc.) other than the current collector in a positive electrode plate or a negative electrode plate by the volume of the electrode plate.
[0025] The “weight average molecular weight” as used herein may be a value measured by gel permeation chromatography (GPC, PL GPC220 (Agilent Technologies Inc.)) and calibrated with a cubic function using polystyrene.
[0026] Hereinafter, a rechargeable lithium battery according to some embodiments will be described in more detail with reference to the accompanying drawings. However, these embodiments are examples, the present disclosure is not limited thereto, and the present disclosure is defined by the scope of the claims and their equivalents.
[0027] In some embodiments, a rechargeable lithium battery comprises: a positive electrode plate; a negative electrode plate; and an electrolyte, including an electrolyte additive, wherein the current density of the positive electrode plate is about 5.4 mA / cm 2 ~About 6.6mA / cm 2 , and the electrolyte additive includes a polyalkylene glycol copolymer.
[0028] In some embodiments of the rechargeable lithium battery, the electrolyte additive is used as a surfactant. Accordingly, in the rechargeable lithium battery including the electrolyte additive, even if the current density of the positive electrode plate is increased (about 5.4 mA / cm 2 or higher), the wettability of the positive electrode plate to the electrolyte can also be improved.
[0029] In addition, if the wettability of the positive electrode plate to the electrolyte is improved, the lithium cation (Li + ) is uniformly (or substantially uniformly) formed at the interface between the positive electrode plate and the electrolyte, inhibiting or reducing the precipitation of lithium dendrites on the surface of the negative electrode plate, and ultimately, ensuring the cycle life characteristics and fast charging performance of the rechargeable lithium battery.
[0030] In a rechargeable lithium battery that does not include an electrolyte additive, if the current density of a positive electrode plate increases, wettability of the positive electrode plate to the electrolyte may be insufficient.
[0031] If the wettability of the positive electrode plate to the electrolyte is insufficient, lithium cations (Li + ), and sharp lithium dendrites are precipitated on the surface of the negative electrode plate, which may eventually hinder the cycle life characteristics and fast charging performance of the rechargeable lithium battery.
[0032] Some embodiments of the present disclosure increase the current density of a positive electrode plate to increase the capacity of a rechargeable lithium battery, and improve cycle life characteristics and fast charging performance by using an electrolyte additive.
[0033] Hereinafter, the rechargeable lithium battery will be described in more detail.
[0034] The current density of the positive electrode plate can be about 5.4 mA / cm 2 ~About 6.6mA / cm 2 , specifically about 5.4 mA / cm 2 ~About 6.3mA / cm 2 or for example about 5.4 mA / cm 2 ~About 5.8mA / cm 2 .
[0035] If the current density of the positive electrode plate is less than about 5.4 mA / cm 2 , there is a limit to achieving high-capacity rechargeable batteries. If the current density of the positive electrode plate exceeds about 6.6 mA / cm 2 , the thickness of the positive electrode plate may become too thick, and the wettability of the positive electrode plate to the electrolyte may decrease.
[0036] The electrolyte additive may include a polyalkylene glycol-based copolymer.
[0037] In some embodiments, the electrolyte additive may be a copolymer including repeating unit 1. Repeating unit 1 corresponds to an alkylene glycol repeating unit:
[0038] Repeating unit 1
[0039]
[0040] Wherein, in the repeating unit 1, R is a hydrogen atom or an alkyl group having 1 to 20 carbon atoms; and x is an integer of 1 to 20.
[0041] In some embodiments, the electrolyte additive may be a block copolymer including repeating units 1-1 and 1-2.
[0042] Repeating unit 1-1
[0043]
[0044] Repeating unit 1-2
[0045]
[0046] In repeating units 1-1 and 1-2, R 1 is an alkyl group having 1 to 20 carbon atoms; and x1 and x2 are each independently an integer of 1 to 20.
[0047] The repeating unit 1-1 corresponds to an ethylene glycol repeating unit.
[0048] In some embodiments, R 1 It may be an alkyl group having 1 carbon atom (eg, methyl group). In some embodiments, repeating unit 1-2 corresponds to a propylene glycol repeating unit.
[0049] In some embodiments, the electrolyte additive is a block copolymer represented by Chemical Formula 1, and is also represented as PEG-b-PPP-b-PEG.
[0050] Chemical formula 1
[0051]
[0052] In Chemical Formula 1, x11, x12, and x21 are each independently an integer of 1 to 20.
[0053] If the electrolyte additive is a block copolymer including three types of repeating units, the electrolyte additive may have a weight average molecular weight of about 800 to about 1500 g / mol, such as about 900 to about 1300 g / mol, or such as about 1000 to about 1200 g / mol.
[0054] If the weight average molecular weight of the electrolyte additive is greater than about 1500 g / mol, it becomes a block copolymer including four or more types (or species) of repeating units, which can excessively increase the viscosity of the electrolyte and hinder the cycle life characteristics and fast charging performance of the rechargeable lithium battery. If the weight average molecular weight of the electrolyte additive is less than about 800 g / mol, it becomes a block copolymer or homopolymer including two or fewer types (or species) of repeating units, and its effect as a surfactant is minimal, which may hinder the cycle life characteristics and fast charging performance of the rechargeable lithium battery.
[0055] The electrolyte additive may be included in an amount of about 0.03 wt % to about 0.5 wt % (eg, about 0.03 wt % to about 0.3 wt % or about 0.1 wt % to about 0.3 wt %) based on 100 wt % of the electrolyte.
[0056] If the content of the electrolyte additive in 100 wt% of the electrolyte exceeds about 0.5 wt%, the viscosity of the electrolyte may be excessively increased, and the cycle life characteristics and fast charging performance of the rechargeable lithium battery may be impaired. If the content of the electrolyte additive in 100 wt% of the electrolyte is less than about 0.03 wt%, the effect as a surfactant is minimal, which may hinder the cycle life characteristics and fast charging performance of the rechargeable lithium battery.
[0057] The lithium salt is dissolved in the non-aqueous organic solvent, supplies lithium ions to the battery, makes the rechargeable lithium battery basically operate, and improves the transmission of lithium ions between the positive electrode plate and the negative electrode plate. Examples of lithium salts may include those selected from LiPF6, LiBF4, LiDFOP, LiDFOB, LiPO2F2, LiSbF6, LiAsF6, Li(CF3SO2)2N, LiN(SO3C2F5)2, Li(FSO2)2N (lithium bis(fluorosulfonyl)imide: LiFSI), LiC4F9SO3, LiClO4, LiAlO2, LiAlCl4, LiN(C x F 2x+1 SO2)(C y F 2y+1 SO2) (wherein x and y are natural numbers, for example, integers of 1 to 20), at least one of LiCl, LiI and LiB(C2O4)2 (lithium bis(oxalato)borate: LiBOB). The concentration of the lithium salt may be in the range of about 0.1 M to about 2.0 M. If the concentration of the lithium salt is within the above range, the electrolyte has appropriate or suitable conductivity (for example, electrical conductivity and / or ionic conductivity) and viscosity, and thus can exhibit excellent electrolyte performance, and lithium ions can be effectively moved.
[0058] The nonaqueous organic solvent serves as a medium for transporting ions participating in the electrochemical reaction of the battery.
[0059] The non-aqueous organic solvent may include a carbonate solvent, an ester solvent, an ether solvent, a ketone solvent, an alcohol solvent and / or an aprotic solvent.
[0060] Carbonate solvents may include ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), ethyl methyl carbonate (MEC), ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), etc. Ester solvents may include methyl acetate, ethyl acetate, n-propyl acetate, tert-butyl acetate, methyl propionate, ethyl propionate, propyl propionate, decanoic acid lactone, mevalonate lactone, caprolactone, etc. Ether solvents may include dibutyl ether, tetraethylene glycol dimethyl ether, diethylene glycol dimethyl ether, dimethoxyethane, 2-methyltetrahydrofuran, tetrahydrofuran, etc. Ketone solvents may include cyclohexanone, etc. Alcohol solvents may include ethanol, isopropanol, etc. Examples of aprotic solvents include nitriles (such as R-CN (wherein R is a C2-C20 straight chain, branched and / or cyclic hydrocarbon group, and includes double bonds, aromatic rings and / or ether bonds)), amides (such as dimethylformamide), dioxolanes (such as 1,3-dioxolane), sulfolane, etc.
[0061] The nonaqueous organic solvent may be used alone or in a mixture, and if the nonaqueous organic solvent is used in a mixture, the mixing ratio may be controlled in accordance with appropriate or desired battery performance.
[0062] The carbonate solvent is prepared by mixing a cyclic carbonate and a chain carbonate. The cyclic carbonate and the chain carbonate are mixed together in a volume ratio of about 5:95 to about 50:50. If the mixture is used as a non-aqueous organic solvent, it can have excellent electrolyte performance.
[0063] For example, ethylene carbonate (EC) may be used as the cyclic carbonate, and ethyl methyl carbonate (EMC) and / or dimethyl carbonate (DMC) may be used as the chain carbonate.
[0064] For example, the non-aqueous organic solvent may include a carbonate-based solvent in which ethylene carbonate (EC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC) are mixed together. For example, a carbonate-based solvent in which ethylene carbonate (EC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC) are mixed together in a volume ratio of EC:EMC:DMC=1:0.5:5 to 5:3:10 may exhibit improved electrolyte performance.
[0065] The nonaqueous organic solvent may further include an aromatic hydrocarbon solvent in addition to the carbonate-based solvent. The carbonate-based solvent and the aromatic hydrocarbon solvent may be mixed together in a volume ratio of about 1:1 to about 30:1.
[0066] The aromatic hydrocarbon solvent may be an aromatic hydrocarbon compound represented by Chemical Formula 3.
[0067] Chemical formula 3
[0068]
[0069] In chemical formula 3, R 201 ~R 206 are the same or different and are selected from hydrogen, halogen, C1-C20 alkyl, C1-C20 haloalkyl, and combinations thereof.
[0070] Examples of aromatic hydrocarbon solvents may be selected from benzene, fluorobenzene, 1,2-difluorobenzene, 1,3-difluorobenzene, 1,4-difluorobenzene, 1,2,3-trifluorobenzene, 1,2,4-trifluorobenzene, chlorobenzene, 1,2-dichlorobenzene, 1,3-dichlorobenzene, 1,4-dichlorobenzene, 1,2,3-trichlorobenzene, 1,2,4-trichlorobenzene, iodobenzene, 1,2-diiodobenzene, 1,3-diiodobenzene, 1,4-diiodobenzene, 1,2,3-triiodobenzene, 1,2,4-triiodobenzene, toluene, fluorotoluene, 2,3-difluorotoluene, 2,4-difluorotoluene, 2,5-difluorotoluene, 2,3,4-trifluorotoluene, 2,3,5-trifluorotoluene, chlorotoluene, 2,3-dichlorotoluene, 2,4-dichlorotoluene, 2,5-dichlorotoluene, 2,3,4-trichlorotoluene, 2,3,5-trichlorotoluene, iodotoluene, 2,3-diiodotoluene, 2,4-diiodotoluene, 2,5-diiodotoluene, 2,3,4-triiodotoluene, 2,3,5-triiodotoluene, xylene, and combinations thereof.
[0071] The electrolyte may further include vinylene carbonate, vinyl ethylene carbonate, and / or an ethylene carbonate-based compound represented by Chemical Formula 4 as a cycle-life enhancing additive to improve the cycle life of the battery.
[0072] Chemical formula 4
[0073]
[0074] In chemical formula 4, R 207 and R 208 are the same or different and are selected from hydrogen, halogen, cyano (-CN), nitro (-NO2) or C1-C5 fluoroalkyl, provided that R 207 and R 208 At least one of them is halogen, cyano (-CN), nitro (-NO2) or C1-C5 fluoroalkyl, and R 207 and R 208 Not simultaneously (eg, synchronously) hydrogen.
[0075] Examples of ethylene carbonate compounds include difluoroethylene carbonate, chloroethylene carbonate, dichloroethylene carbonate, bromoethylene carbonate, dibromoethylene carbonate, nitroethylene carbonate, cyanoethylene carbonate, or fluoroethylene carbonate. The amount of the additive for improving the cycle life can be used within an appropriate or suitable range.
[0076] The loading of the positive electrode plate can be about 50.1 mg / cm 2 ~ about 65.0mg / cm 2 or for example about 50.1 mg / cm 2 ~about 59.1mg / cm 2 In some embodiments, the mixture density of the positive electrode plate may be from about 2.0 g / cc to about 6.0 g / cc, or for example, from about 3.0 g / cc to about 5.0 g / cc.
[0077] If each of the above ranges is satisfied, the energy density of a rechargeable lithium battery may be increased.
[0078] The positive electrode plate includes a positive electrode current collector and a positive electrode mixture layer on the positive electrode current collector, and the positive electrode mixture layer includes a positive electrode active material.
[0079] The positive electrode active material may include a lithiated intercalation compound that reversibly intercalates and deintercalates lithium ions.
[0080] For example, at least one composite oxide of metals of cobalt, manganese, nickel, or a combination thereof and lithium may be used.
[0081] A composite oxide having a coating on its surface can be used, or a mixture of a composite oxide and a composite oxide having a coating can be used. The coating can include a coating element compound of an oxide of a coating element, a hydroxide of a coating element, an oxyhydroxide of a coating element, an oxycarbonate of a coating element, or a hydroxycarbonate of a coating element. The compound used for the coating can be amorphous and / or crystalline. The coating element included in the coating can be Mg, Al, Co, K, Na, Ca, Si, Ti, V, Sn, Ge, Ga, B, As, Zr, or a mixture thereof. The coating process can include any suitable process (e.g., spray coating, dip coating) that a person of ordinary skill in the art should easily recognize after reading this disclosure, as long as it does not cause any side effects (e.g., any undesirable side effects) to the characteristics of the positive electrode active material, and therefore, it is not necessary to describe it in detail here.
[0082] For example, the positive electrode active material may include a lithium nickel-based composite oxide represented by Chemical Formula A1.
[0083] Chemical formula A1
[0084] Li a1 Ni x1 M 1 y1 M 2 z1 O 2-b1 X b1
[0085] In Chemical Formula A1, 0.9 ≤ a1 ≤ 1.8 (for example, 0.9 ≤ a1 ≤ 1.2), 0.7 ≤ x1 ≤ 1, 0 ≤ y1 ≤ 0.2, 0 ≤ z1 ≤ 0.2, 0.9 ≤ x1 + y1 + z1 ≤ 1.1, and 0 ≤ b1 ≤ 0.1; M 1 and M 2 are each independently one or more elements selected from Al, B, Ba, Ca, Ce, Co, Cr, Cu, Fe, Mg, Mn, Mo, Nb, Si, Sr, Ti, V, W, and Zr; and X is one or more elements selected from F, P, and S.
[0086] In some embodiments, in Chemical Formula A1, 0.75 ≤ x1 ≤ 1, 0 ≤ y1 ≤ 0.18, and 0 ≤ z1 ≤ 0.18; 0.85 ≤ x1 ≤ 1, 0 ≤ y1 ≤ 0.15, and 0 ≤ z1 ≤ 0.15; or 0.9 ≤ x1 ≤ 1, 0 ≤ y1 ≤ 0.1, and 0 ≤ z1 ≤ 0.1.
[0087] For example, the positive electrode active material may include a lithium nickel-based composite oxide represented by Chemical Formula A2. The compound represented by Chemical Formula A2 may be referred to as a lithium nickel cobalt-based composite oxide.
[0088] Chemical Formula A2
[0089] Li a2 Ni x2 Co y2 M 3 z2 O 2-b2 X b2
[0090] In Chemical Formula A2, 0.9 ≤ a2 ≤ 1.8, 0.7 ≤ x2 < 1, 0 < y2 ≤ 0.2, 0 ≤ z2 ≤ 0.2, 0.9 ≤ x2 + y2 + z2 ≤ 1.1, and 0 ≤ b2 ≤ 0.1, M 3 is one or more elements selected from Al, B, Ba, Ca, Ce, Cr, Cu, Fe, Mg, Mn, Mo, Nb, Si, Sr, Ti, V, W, and Zr, and X is one or more elements selected from F, P, and S.
[0091] In some embodiments, in Chemical Formula A2, 0.75 ≤ x2 ≤ 0.99, 0 ≤ y2 ≤ 0.15, and 0 ≤ z2 ≤ 0.15; 0.85 ≤ x2 ≤ 0.99, 0.01 ≤ y2 ≤ 0.15, and 0.01 ≤ z2 ≤ 0.15; or 0.9 ≤ x2 ≤ 0.99, 0.01 ≤ y2 ≤ 0.1, and 0.01 ≤ z2 ≤ 0.1.
[0092] For example, the positive electrode active material may include a lithium nickel-based composite oxide represented by Chemical Formula A3. The compound represented by Chemical Formula A3 may be referred to as a lithium nickel cobalt aluminum-based oxide or a lithium nickel cobalt manganese-based oxide.
[0093] Chemical formula A3
[0094] Li a3 Ni x3 Co y3 M 4 z3 M 5 w3 O 2-b3 X b3
[0095] In the chemical formula A3, 0.9≤a3≤1.8, 0.7≤x3≤0.98, 0.01≤y3≤0.19, 0.01≤z3≤0.19, 0≤w3≤0.19, 0.9≤x3+y3+z3+w3≤1.1, and 0≤b3≤0.1, M 4 is one or more elements selected from Al and Mn, M 5 is one or more elements selected from B, Ba, Ca, Ce, Cr, Cu, Fe, Mg, Mo, Nb, Si, Sr, Ti, V, W and Zr, and X is one or more elements selected from F, P and S.
[0096] In some embodiments, in Chemical Formula A3, 0.75≤x3≤0.98, 0.01≤y3≤0.16, 0.01≤z3≤0.16, and 0≤w3≤0.16; 0.85≤x3≤0.98, 0.01≤y3≤0.14, 0.01≤z3≤0.14, and 0≤w3≤0.14; or 0.9≤x3≤0.98, 0.01≤y3≤0.09, 0.01≤z3≤0.09, and 0≤w3≤0.09.
[0097] For example, the positive electrode active material may include a lithium nickel-based composite oxide represented by Chemical Formula A4. The compound represented by Chemical Formula A4 may be referred to as a cobalt-free lithium nickel manganese oxide.
[0098] Chemical formula A4
[0099] Li a4 Ni x4 Mn y4 M 6 z4 O 2-b4 X b4
[0100] In chemical formula A4, 0.9 ≤ a2 ≤ 1.8, 0.7 ≤ x4 < 1, 0 < y4 ≤ 0.2, 0 ≤ z4 ≤ 0.2, 0.9 ≤ x4 + y4 + z4 ≤ 1.1, and 0 ≤ b4 ≤ 0.1, M 6 is one or more elements selected from Al, B, Ba, Ca, Ce, Cr, Cu, Fe, Mg, Mo, Nb, Si, Sr, Ti, V, W, and Zr, and X is one or more elements selected from F, P, and S.
[0101] In the positive electrode plate of some embodiments, based on the total weight of the positive electrode mixture layer, the content of the positive electrode active material can be about 50 wt% to about 99 wt%, about 60 wt% to about 99 wt%, about 70 wt% to about 99 wt%, about 80 wt% to about 99 wt%, or about 90 wt% to about 99 wt%.
[0102] In some embodiments, the positive electrode mixture layer may optionally include a conductive material (e.g., a conductivity material) and a binder. At this time, based on the total weight of the positive electrode mixture layer, the contents of the conductive material and the binder can be about 1.0 wt% to about 5.0 wt% respectively.
[0103] The conductive material is used to impart conductivity (e.g., conductivity) to the positive electrode plate, and any suitable conductivity material can be used as the conductive material unless it causes chemical changes in the battery (e.g., undesirable chemical changes in a rechargeable lithium battery). Examples of the conductive material may include: carbon-based materials such as natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fiber, etc.; metal-based materials such as metal powders and / or metal fibers including copper, nickel, aluminum, silver, etc.; conductive polymers (e.g., conductivity polymers) such as polyphenylene derivatives; or mixtures thereof.
[0104] The binder improves the adhesion characteristics between the positive electrode active material particles and the adhesion characteristics between the positive electrode active material particles and the positive electrode current collector. Examples thereof may be polyvinyl alcohol, carboxymethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, a polymer containing ethylene oxide, polyvinylpyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene-butadiene rubber, acrylated styrene-butadiene rubber, epoxy resin, nylon, etc., but are not limited thereto.
[0105] Al can be used as the positive electrode current collector, but is not limited thereto.
[0106] The loading of the negative electrode plate can be about 28.2 mg / cm 2 ~ about 39.2 mg / cm 2 or for example about 28.2 mg / cm 2~about 33.5 g mg / cm 2 。
[0107] In some embodiments, the mixture density of the negative electrode plate can be 1.40 g / cc to 1.80 g / cc, such as about 1.0 g / cc to about 2.0 g / cc or about 1.54 g / cc to about 1.74 g / cc.
[0108] If each of the above ranges is satisfied, the energy density of the rechargeable lithium battery can be increased.
[0109] The negative electrode plate includes a negative electrode current collector and a negative electrode active material layer on the negative electrode current collector, and the negative electrode active material layer includes a negative electrode active material.
[0110] The negative electrode active material can be a material that reversibly intercalates / deintercalates lithium ions, lithium metal, a lithium metal alloy, a material capable of doping and dedoping lithium, and / or a transition metal oxide.
[0111] Materials that reversibly intercalate / deintercalate lithium ions include carbon materials. The carbon materials can be any suitable and commonly used carbon-based negative electrode active materials in rechargeable lithium batteries. Examples of the carbon materials include crystalline carbon, amorphous carbon, or a combination thereof. The crystalline carbon can be amorphous natural graphite and / or artificial graphite, and / or can be natural graphite and / or artificial graphite in the form of flakes, sheets, spheres, and / or fibers. The amorphous carbon can be soft carbon, hard carbon, mesophase pitch carbonization products, calcined coke, etc.
[0112] The lithium metal alloy can include metals selected from Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Si, Sb, Pb, In, Zn, Ba, Ra, Ge, Al, and Sn and lithium.
[0113] Materials capable of doping and dedoping lithium can include Si, SiO x (0 < x < 2), Si-Q alloys (where Q is selected from alkali metals, alkaline earth metals, Group 13 elements, Group 14 elements (excluding Si), Group 15 elements, Group 16 elements, transition metals, rare earth elements, and combinations thereof), Sn, SnO2, Sn-R alloys (where R is an alkali metal, alkaline earth metal, Group 13 element, Group 14 element (excluding Sn), Group 15 element, Group 16 element, transition element, rare earth element, or combination thereof), etc. At least one of the foregoing can be mixed with SiO2.
[0114] The elements Q and R can be selected from Mg, Ca, Sr, Ba, Ra, Sc, Y, Ti, Zr, Hf, Rf, V, Nb, Ta, Db, Cr, Mo, W, Sg, Tc, Re, Bh, Fe, Pb, Ru, Os, Hs, Rh, Ir, Pd, Pt, Cu, Ag, Au, Zn, Cd, B, Al, Ga, Sn (R does not include Sn), In, Tl, Ge, P, As, Sb, Bi, S, Se, Te, Po, and combinations thereof.
[0115] The transition metal oxide can be vanadium oxide, lithium vanadium oxide, etc.
[0116] In some embodiments, the negative electrode active material can include at least one selected from graphite and Si composites.
[0117] The Si composite can include a core including Si-based particles and amorphous carbon. For example, the Si-based particles can include at least one selected from Si particles, Si-C composites, SiO x (0 < x ≤ 2) and Si alloys.
[0118] For example, the Si-C composite can include a core including Si particles and amorphous carbon.
[0119] The central part of the core of the Si-C composite can include pores, and the radius of the central part can correspond to about 30% to about 50% of the radius of the Si-C composite.
[0120] The Si particles can have an average particle size of about 10 nm to about 200 nm.
[0121] As used herein, the average particle size (D50) can be the particle size at which the volume ratio is 50% in the cumulative size distribution curve.
[0122] If the average particle size of the Si particles is within the above range, volume expansion occurring during charging and discharging can be suppressed or reduced, and disconnection of the conduction path (e.g., the conductive path) due to particle breakage during charging and discharging can be prevented or reduced.
[0123] Based on the total weight of the Si-C composite, the Si particles can be included in an amount of about 1 wt% to about 60 wt% (e.g., about 3 wt% to about 60 wt%).
[0124] The central part may not include amorphous carbon, and the amorphous carbon may only be present on the surface part of the negative electrode active material.
[0125] As used herein, the surface part indicates the region from the outermost surface of the central part of the negative electrode active material to the outermost surface of the negative electrode active material.
[0126] In some embodiments, the Si particles are included substantially uniformly throughout the negative electrode active material, for example, present in a substantially uniform concentration in a central portion and a surface portion thereof.
[0127] The amorphous carbon may be soft carbon, hard carbon, a mesophase pitch carbonization product, calcined coke, or a combination thereof.
[0128] The negative electrode active material may further include crystalline carbon.
[0129] If the negative electrode active material includes both Si composite and crystalline carbon, the Si composite and crystalline carbon may be included in a mixture, and in some embodiments, the Si composite and crystalline carbon may be included in a weight ratio of about 1:99 to about 50:50. For example, the Si composite and crystalline carbon may be included in a weight ratio of about 3:97 to about 20:80 or about 5:95 to about 20:80.
[0130] The crystalline carbon may be, for example, graphite, and may be, for example, natural graphite, artificial graphite, or a mixture thereof.
[0131] The crystalline carbon may have an average particle size of about 5 μm to about 30 μm.
[0132] The amorphous carbon precursor may include coal pitch, mesophase pitch, petroleum-based pitch, coal-based oil, petroleum-based heavy oil, and / or a polymer resin (such as, for example, a phenol resin, a furan resin, and / or a polyimide resin).
[0133] In the negative electrode active material layer, the negative electrode active material may be included in an amount of about 95 wt % to about 99 wt % based on the total weight of the negative electrode active material layer.
[0134] In some embodiments, the negative electrode active material layer may include a binder and an optional conductive material (e.g., an electrically conductive material). In the negative electrode active material layer, the amount of the binder may be about 1 wt% to about 5 wt% based on the total weight of the negative electrode active material layer. If the negative electrode active material layer further includes a conductive material, it may include about 90 wt% to about 98 wt% of the negative electrode active material, about 1 wt% to about 5 wt% of the binder, and about 1 wt% to about 5 wt% of the conductive material.
[0135] The binder improves the binding properties between the negative electrode active material particles and between the negative electrode active material particles and the negative electrode current collector. The binder may be a water-insoluble binder, a water-soluble binder, or a combination thereof.
[0136] The non-water-soluble binder may be polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, polyamide-imide, polyimide or a combination thereof.
[0137] The water-soluble binder can be a rubber-based binder and / or a polymer resin binder. The rubber-based binder can be selected from styrene-butadiene rubber (SBR), acrylated styrene-butadiene rubber, acrylonitrile-butadiene rubber, acrylic rubber, butyl rubber, fluororubber and a combination thereof. The polymer resin binder can be selected from polytetrafluoroethylene, ethylene-propylene copolymer, polyethylene oxide, polyvinyl pyrrolidone, polyepichlorohydrin, polyphosphazene, polyacrylonitrile, polystyrene, ethylene-propylene-diene copolymer, polyvinyl pyridine, chlorosulfonated polyethylene, latex, polyester resin, acrylic resin, phenolic resin, epoxy resin, polyvinyl alcohol and a combination thereof.
[0138] If a water-soluble binder is used as a binder in the negative electrode active material layer, a cellulose compound may be further used as a thickener to provide or increase viscosity. The cellulose compound may include one or more of carboxymethyl cellulose, hydroxypropyl methyl cellulose, methyl cellulose, and alkali metal salts thereof. The alkali metal may be Na, K, and / or Li. Based on 100 parts by weight of the negative electrode active material, such a thickener may be included in an amount of about 0.1 parts by weight to about 3 parts by weight.
[0139] The conductive material is used to impart conductivity (e.g., electrical conductivity) to the electrode, and any suitable conductive material may be used as the conductive material unless it causes chemical changes in the battery (e.g., undesirable chemical changes in a rechargeable lithium battery). Examples of the conductive material may include: carbon-based materials such as natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fiber, etc.; metal-based materials such as metal powders and / or metal fibers including copper, nickel, aluminum, silver, etc.; conductive polymers (e.g., conductive polymers) such as polyphenylene derivatives; or mixtures thereof.
[0140] The negative electrode current collector may be selected from copper foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam, a polymer substrate coated with a conductive metal (eg, an electrically conductive metal), and combinations thereof.
[0141] According to the type (or kind) of the rechargeable lithium battery, the rechargeable lithium battery may further include a separator between the positive electrode plate and the negative electrode plate. Such a separator is a porous substrate; or it may be a composite porous substrate.
[0142] The porous substrate may be a substrate including pores, and lithium ions can move through the pores. The porous substrate may include, for example, a polyethylene separator, a polypropylene separator, a polyvinylidene fluoride separator, and multilayers thereof (such as, for example, a polyethylene / polypropylene double-layer separator, a polyethylene / polypropylene / polyethylene three-layer separator, and / or a polypropylene / polyethylene / polypropylene three-layer separator).
[0143] The composite porous substrate may have a form including a porous substrate and a functional layer on the porous substrate. From the perspective of ensuring additional functions, the functional layer may be, for example, at least one selected from a heat-resistant layer and an adhesive layer. For example, the heat-resistant layer may include a heat-resistant resin and an optional filler.
[0144] In some embodiments, the adhesive layer may include an adhesive resin and optionally a filler.
[0145] The filler may be an organic filler and / or an inorganic filler.
[0146] refer to Figure 1 According to some embodiments, a rechargeable lithium battery 100 includes a battery cell (the battery cell includes: a negative electrode plate 112, a positive electrode plate 114 facing the negative electrode plate 112, a separator 113 between the negative electrode plate 112 and the positive electrode plate 114, and an electrolyte (not shown) impregnating the negative electrode plate 112, the positive electrode plate 114 and the separator 113), a battery case 120 accommodating the battery cell, and a sealing member 140 sealing the battery case 120.
[0147] Hereinafter, embodiments and comparative examples of the present disclosure are described. However, these examples should not be interpreted as limiting the scope of the present disclosure in any sense.
[0148] Preparation of electrolyte for rechargeable lithium batteries
[0149] Preparation Example 1
[0150] As the nonaqueous organic solvent, a carbonate-based solvent prepared by mixing ethylene carbonate (EC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC) together at a volume ratio of EC:EMC:DMC=20:10:70 was used.
[0151] 1.5 M of lithium salt (LiPF6) was added to a non-aqueous organic solvent, and 0.03 wt % of a block copolymer represented by Chemical Formula 1 was added thereto as an electrolyte additive to finally obtain an electrolyte for a rechargeable lithium battery:
[0152] Chemical formula 1
[0153]
[0154] In Chemical Formula 1, x11, x12, and x21 are each independently an integer of 1 to 20.
[0155] The block copolymer represented by Chemical Formula 1 has a weight average molecular weight of about 1,100 g / mol, which is obtained by measuring using gel permeation chromatography (GPC, PL GPC220 (Agilent Technologies Inc.)) and calibrating with a cubic function using polystyrene.
[0156] In addition, the content (wt %) of the electrolyte additive indicates the content (wt %) based on 100 wt % of the electrolyte for a rechargeable lithium battery (non-aqueous organic solvent+lithium salt+additive). Hereinafter, this will also apply.
[0157] Preparation Example 2
[0158] An electrolyte for a rechargeable lithium battery was prepared in substantially the same manner as Preparation Example 1, except that the block copolymer represented by Chemical Formula 1 was added in an amount of 0.1 wt % as an electrolyte additive.
[0159] Preparation Example 3
[0160] An electrolyte for a rechargeable lithium battery was prepared in substantially the same manner as Preparation Example 1, except that the block copolymer represented by Chemical Formula 1 was added as an electrolyte additive in an amount of 0.3 wt %.
[0161] Preparation Example 4
[0162] An electrolyte for a rechargeable lithium battery was prepared in substantially the same manner as Preparation Example 1, except that the block copolymer represented by Chemical Formula 1 was added in an amount of 0.5 wt % as an electrolyte additive.
[0163] Comparative Preparation Example 1
[0164] An electrolyte for a rechargeable lithium battery was prepared in substantially the same manner as in Preparation Example 1, except that no electrolyte additive was added at all.
[0165] Comparative Preparation Example 2
[0166] The homopolymer including the repeating unit 1-1 was used as an electrolyte additive in an amount of 0.1 wt%.
[0167] Repeating unit 1-1
[0168]
[0169] In the repeating unit 1-1, x1 is an integer of 1-20.
[0170] The homopolymer including only the repeating unit 1-1 has a weight average molecular weight of about 1,000 g / mol, which is obtained by measuring using gel permeation chromatography (GPC, PL GPC220 (Agilent Technologies Inc.)) and calibrating with a cubic function using polystyrene.
[0171] Manufacturing of rechargeable lithium battery cells
[0172] Example 1-1
[0173] (1) Manufacturing of positive electrode plates
[0174] LiNi as the positive electrode active material 0.88 Co 0.07 Al 0.05 O2, polyvinylidene fluoride as a binder, and Ketjen black as a conductive material were mixed together in a weight ratio of 97:2:1, and then dispersed in N-methylpyrrolidone to prepare a positive electrode slurry.
[0175] The positive electrode slurry was coated on a 14 μm thick Al foil, dried at 110° C., and pressed to produce a positive electrode plate.
[0176] The positive electrode plate has a 50.1 mg / cm 2 loading, 4.0 g / cc mixture density and 5.4 mA / cm 2 of current density.
[0177] Each of the above-mentioned measuring methods is the same as the measuring methods in the following Examples and Comparative Examples.
[0178] (2) Manufacturing of negative electrode plates
[0179] A mixture of artificial graphite and Si composite in a weight ratio of 93:7 was prepared as a negative electrode active material, and the negative electrode active material, styrene-butadiene rubber binder, and carboxymethyl cellulose were dispersed in distilled water in a weight ratio of 97:1:2 to prepare a negative electrode slurry.
[0180] The Si composite has a core including artificial graphite and Si particles, and coal tar pitch coated on the surface of the core.
[0181] The negative electrode slurry was coated on a 10 μm thick Cu foil, dried at 100° C., and pressed to manufacture a negative electrode plate.
[0182] The negative electrode plate has 28.2 mg / cm 2 of loading and a mixture density of 1.64 g / cc.
[0183] Each of the above-mentioned measuring methods is the same as the measuring methods in the following Examples and Comparative Examples.
[0184] (3) Manufacturing of rechargeable lithium battery cells
[0185] A rechargeable lithium battery cell was manufactured by assembling a positive electrode plate and a negative electrode plate with a 25 μm thick polyethylene separator to obtain an electrode assembly, and injecting the electrolyte for a rechargeable lithium battery according to Preparation Example 1 thereinto.
[0186] Example 1-2
[0187] A rechargeable lithium battery cell was manufactured in substantially the same manner as in Example 1, except that the electrolyte for a rechargeable lithium battery according to Preparation Example 2 was injected.
[0188] Examples 1-3
[0189] A rechargeable lithium battery cell was manufactured in substantially the same manner as in Example 1, except that the electrolyte for a rechargeable lithium battery according to Preparation Example 3 was injected.
[0190] Examples 1-4
[0191] A rechargeable lithium battery cell was manufactured in substantially the same manner as in Example 1, except that the electrolyte for a rechargeable lithium battery according to Preparation Example 4 was injected.
[0192] Comparative Example 1-1
[0193] A rechargeable lithium battery cell was manufactured in substantially the same manner as in Example 1, except that the electrolyte for a rechargeable lithium battery according to Comparative Preparation Example 1 was injected.
[0194] Comparative Example 1-2
[0195] A rechargeable lithium battery cell was manufactured in substantially the same manner as Example 1, except that the electrolyte for a rechargeable lithium battery according to Comparative Preparation Example 2 was injected.
[0196] Examples 2 to 4 and Comparative Examples 2 to 8
[0197] The individual rechargeable lithium battery cells in Examples 2 to 4 and Comparative Examples 6 and 8 are manufactured in substantially the same manner as in Example 1-2, and the individual rechargeable lithium battery cells in Comparative Examples 2 to 5 and Comparative Example 7 are manufactured in substantially the same manner as in Comparative Example 1-1, except that at least one of the loading amount of the positive electrode plate, the current density of the positive electrode plate, and the loading amount of the negative electrode plate is changed as shown in Table 1.
[0198] Table 1
[0199]
[0200]
[0201] Evaluation 1: Evaluation of electrolyte impregnation characteristics
[0202] The impregnation characteristics of the electrolytic solution of each of the positive electrode plates of the example and the comparative example were evaluated, and the results are shown in Table 2.
[0203] Specifically, the electrolyte was prepared by mixing ethylene carbonate (EC), ethyl methyl carbonate (EMC) and dimethyl carbonate (DMC) together in a volume ratio of EC:EMC:DMC=2:2:4 to prepare a carbonate-based solvent and dissolving 1.0 M LiPF6 in the carbonate-based solvent.
[0204] The electrolyte was dropped on each of the positive electrode plate samples having a size of 3 cm×3 cm to measure the impregnation area of the electrolyte after immersion for 10 seconds.
[0205] Evaluation 2: Evaluation of cycle life characteristics
[0206] The cycle-life characteristics of each of the rechargeable lithium battery cells of the embodiment and the comparative example were evaluated, and the results are shown in Table 2.
[0207] The battery cell was charged and discharged 287 times at 25° C. under 0.33C charging condition (CC / CV, 4.45 V, 0.025C cutoff) and 1.0C discharging condition (CC, 2.5 V cutoff), and the capacity retention ratio was evaluated according to Equation 1.
[0208] Equation 1
[0209] Capacity retention rate = (discharge capacity after 287 cycles / discharge capacity after 1 cycle) × 100
[0210] Evaluation 3: Evaluation of Li precipitation amount
[0211] The Li precipitation amount of each of the rechargeable lithium battery cells according to the embodiment and the comparative example was evaluated, and the results are shown in Table 2.
[0212] The battery cells were charged to SOC 80% at 25°C to measure the charge capacity, and discharged at 1.0C (CC, 2.5V cutoff) to measure the lithium precipitation capacity on the negative electrode plate surface in the discharge platform portion, which was used to evaluate the Li precipitation amount according to Equation 2.
[0213] Equation 2
[0214] Li precipitation amount = lithium precipitation capacity (discharge platform part) / charging capacity (SOC80% charging capacity) × 100
[0215] Table 2
[0216]
[0217]
[0218] Referring to Table 2, if the positive electrode plate has the same current density, the rechargeable lithium battery cell including the polyalkylene glycol-based copolymer as an electrolyte additive exhibits increased cycle life characteristics compared to a battery cell that does not include the electrolyte additive at all. However, if the positive electrode plate has a current density of less than 5.4 mA / cm 2 If the current density is too high, there is usually a limitation in achieving high-capacity rechargeable batteries.
[0219] In some embodiments of the rechargeable lithium battery, the electrolyte additive acts as a surfactant. Accordingly, the rechargeable lithium battery including the electrolyte additive exhibits improved wettability of the positive electrode plate to the electrolyte even if the current density of the positive electrode plate increases.
[0220] In addition, if the wettability of the positive electrode plate to the electrolyte is improved, the lithium cation (Li + ) is uniformly (or substantially uniformly) formed at the interface between the positive electrode plate and the electrolyte, inhibiting or reducing the precipitation of lithium dendrites on the surface of the negative electrode plate, and ultimately, ensuring the cycle life characteristics and fast charging performance of the rechargeable lithium battery.
[0221] While the subject matter of the present disclosure has been described in connection with what are presently considered to be practical example embodiments, it should be understood that the disclosure is not limited to the disclosed embodiments, but on the contrary, the disclosure is intended to cover various modifications and equivalent arrangements included within the spirit and scope of the claims and their equivalents.
Claims
1. A rechargeable lithium battery comprising: Positive electrode plate; Negative electrode plate; and Electrolytes, including electrolyte additives, The current density of the positive electrode plate is 5.4 mA / cm 2 ~6.6mA / cm 2 ;and The electrolyte additive includes a polyalkylene glycol copolymer.
2. The rechargeable lithium battery of claim 1, wherein: The electrolyte additive is a copolymer comprising repeating unit 1: Repeating unit 1 Among them, in repeating unit 1, R is a hydrogen atom or an alkyl group having 1 to 20 carbon atoms; and x is an integer from 1 to 20.
3. The rechargeable lithium battery of claim 2, wherein: The electrolyte additive is a block copolymer comprising repeating units 1-1 and 1-2: repeating unit 1-1 Repeating unit 1-2 Wherein, in repeating units 1-1 and 1-2, R 1 is an alkyl group having 1 to 20 carbon atoms; and x1 and x2 are each independently an integer of 1-20.
4. The rechargeable lithium battery of claim 3, wherein: The electrolyte additive is a block copolymer represented by Chemical Formula 1: Chemical formula 1 Wherein, in Chemical Formula 1, x11, x12 and x21 are each independently an integer of 1-20.
5. The rechargeable lithium battery of claim 1, wherein: The content of the electrolyte additive in 100 wt % of the electrolyte is 0.03 wt % to 0.5 wt %.
6. The rechargeable lithium battery of claim 1, wherein: The electrolyte further includes a lithium salt and a non-aqueous organic solvent.
7. The rechargeable lithium battery of claim 6, wherein: The lithium salt includes LiPF6, LiBF4, LiDFOP, LiDFOB, LiPO2F2, LiSbF6, LiAsF6, Li(CF3SO2)2N, LiN(SO3C2F5)2, Li(FSO2)2N, LiC4F9SO3, LiClO4, LiAlO2, LiAlCl4, LiN(C x F 2x+1 SO2)(C y F 2y+1 SO2), at least one of LiCl, LiI and LiB(C2O4)2.
8. The rechargeable lithium battery of claim 6, wherein: The concentration of the lithium salt is in the range of 0.1M to 2.0M.
9. The rechargeable lithium battery of claim 6, wherein: The non-aqueous organic solvent includes carbonate solvents, ester solvents, ether solvents, ketone solvents, alcohol solvents and / or aprotic solvents.
10. The rechargeable lithium battery of claim 9, wherein: The non-aqueous organic solvent includes a carbonate solvent, and the carbonate solvent includes a cyclic carbonate and a chain carbonate mixed together in a volume ratio of 5:95 to 50:
50.
11. The rechargeable lithium battery of claim 10, wherein: The cyclic carbonate comprises ethylene carbonate, and The chain carbonates include ethyl methyl carbonate and dimethyl carbonate.
12. The rechargeable lithium battery of claim 1, wherein: The positive electrode plate includes a positive electrode mixture layer, and The loading capacity of the positive electrode plate is 50.1 mg / cm 2 ~65.0mg / cm 2 .
13. The rechargeable lithium battery of claim 12, wherein: The mixture density of the positive electrode plate is 2.0 g / cc to 6.0 g / cc.
14. The rechargeable lithium battery of claim 12, wherein: The positive electrode mixture layer includes a positive electrode active material, and The positive electrode active material includes a lithium nickel composite oxide represented by Chemical Formula A1: Chemical formula A1 Li a1 Ni x1 M 1 y1 M 2 z1 O 2-b1 X b1 Wherein, in chemical formula A1, 0.9≤a1≤1.8, 0.7≤x1≤1, 0≤y1≤0.2, 0≤z1≤0.2, 0.9≤x1+y1+z1≤1.1, and 0≤b1≤0.1; M 1 and M 2 Each is independently one or more elements selected from Al, B, Ba, Ca, Ce, Co, Cr, Cu, Fe, Mg, Mn, Mo, Nb, Si, Sr, Ti, V, W and Zr; and X is one or more elements selected from F, P and S.
15. The rechargeable lithium battery of claim 1, wherein: The negative electrode plate includes a negative electrode mixture layer, and The loading capacity of the negative electrode plate is 28.2 mg / cm 2 ~39.2mg / cm 2 .
16. The rechargeable lithium battery of claim 15, wherein: The mixture density of the negative electrode plate is 1.40 g / cc to 1.80 g / cc.
17. The rechargeable lithium battery of claim 15, wherein: The negative electrode mixture layer includes a negative electrode active material, and The negative electrode active material includes at least one selected from graphite and Si composite.
18. The rechargeable lithium battery of claim 17, wherein: The Si composite includes a core including Si-based particles and amorphous carbon.
19. The rechargeable lithium battery of claim 18, wherein: The core comprising the Si-based particles comprises a Si particle selected from Si particles, Si-C composites, SiO k and Si alloy, wherein 0 <k≤2。 20. The rechargeable lithium battery of claim 19, wherein: The Si—C composite includes a core including Si particles and amorphous carbon.