Perovskite thin film, perovskite LED device and preparation method thereof

By using ABX3 organic-inorganic perovskite films containing metal cations and calcium trifluoromethanesulfonate in perovskite LED devices, the problems of halogen segregation and phase separation in the device are solved, and the luminescence spectral stability and fluorescence intensity are improved. Improved device performance.

CN119095461AInactive Publication Date: 2024-12-06FUDAN UNIVERSITY
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410843117.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-27
Publication Date
2024-12-06
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Perovskite LED devices are prone to halogen segregation and phase separation problems during operation, resulting in luminescence color/spectrum offset and affecting luminescence performance.

Method used

Using ABX3 organic-inorganic perovskite film containing metal cations, the addition of metal ions such as calcium trifluoromethanesulfonate passes away the inherent defects in the film, inhibit the migration and phase separation of halogen ions, and form high-quality perovskite. The film increases the grain size and improves the stability of the luminescent spectrum.

Benefits of technology

It effectively inhibits the ion movement inside the perovskite, improves the stability and fluorescence intensity of the luminescence spectrum, extends the fluorescence life, and improves the performance of perovskite LED devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119095461A_ABST
    Figure CN119095461A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of perovskite devices, and particularly relates to a perovskite thin film, a perovskite LED device and a preparation method thereof. The perovskite thin film provided by the invention is obtained by coating a substrate with slurry consisting of an ABX3 organic-inorganic perovskite material and salt containing metal cations and then performing annealing treatment, the molar ratio of the salt containing the metal cations is 1 mol%-5 mol%; a is selected from PEA < + >, GA < + > and Cs < + >, B is Pb < 2 + >, and X is Br <-> or Cl <->; the salt containing the metal cations is calcium trifluoromethanesulfonate. According to the invention, anions of calcium trifluoromethanesulfonate are introduced to passivate internal defects of the perovskite thin film through Lewis acid-base interaction; the added calcium metal ions can enter perovskite crystal lattices in an interstitial doping mode, and due to the fact that the calcium ions have strong interaction with charged defects in the perovskite, ion movement in the perovskite can be effectively restrained. The migration of halide ions in the perovskite thin film and the device is inhibited, and the stability of a luminescent spectrum is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of perovskite devices, and in particular relates to a perovskite film, a perovskite LED device and a preparation method thereof. Background Art

[0002] Metal halide perovskite materials have the advantages of adjustable emission wavelength, high photoluminescence quantum efficiency, high color saturation, low cost and room temperature solution processing, and are expected to become a strong competitor in the next generation of full-color display and lighting. Since the electroluminescence effect of perovskites was first observed at room temperature in 2014, the external quantum efficiency of green, red and near-infrared perovskite light-emitting diodes has exceeded 20%. As an emerging lighting and display technology, perovskite blue light LEDs have the advantages of high efficiency, high brightness and wide wavelength control range, and have received widespread attention. At present, the methods for realizing blue light perovskite LEDs (PeLEDs) mainly include halogen doping component engineering and dimensional engineering based on quantum confinement effects. Adjusting the ratio of mixed halogens such as bromine and chlorine can adjust the emission peak position. By increasing the chlorine content, the emission peak position can be blue-shifted, which is currently the most widely used means to adjust to the blue light peak position.

[0003] However, during the operation of the device, the uniformly mixed halide perovskite easily forms a halide segregation phase with spatially non-uniform band gap and luminescent color. The halogen ions inside the perovskite easily migrate, resulting in phase separation of the perovskite film and the formation of perovskite phases with different band gaps. The phase separation problem will cause the perovskite LED to shift in color / spectrum, which seriously affects the luminescence performance of PeLED. So far, researchers at home and abroad have made many attempts to suppress the halogen segregation problem in the operation of mixed halide perovskite LED devices. Therefore, it is of great significance to study the suppression of halogen phase separation in perovskite blue LEDs. Summary of the invention

[0004] The object of the present invention is to provide a perovskite film capable of improving the stability of the luminescence spectrum and a preparation method thereof, and to provide a corresponding perovskite LED device and a preparation method thereof.

[0005] The perovskite film provided by the present invention comprises an ABX3 organic-inorganic perovskite material and a salt containing metal cations; in the perovskite film, the molar ratio of the salt containing metal cations is 1 mol% to 5 mol%; in the perovskite-type ABX3 organic-inorganic hybrid material, A is selected from PEA+, GA+, Cs+, B is Pb2+, and X is Br- or Cl-.

[0006] The metal cation-containing salt is calcium trifluoromethanesulfonate Ca(CF3SO3)2, but is not limited thereto and may also be a salt containing metal ions such as neodymium ions and sodium ions.

[0007] Since the multifunctional groups in triflate ions can passivate the inherent defects in the perovskite film through Lewis acid-base interactions, it helps to form a high-quality perovskite film with an increased grain size and reduced defect state density. In addition, under light, heat and bias, the continuous migration of halogen ions inside the perovskite will lead to the enrichment of chloride and bromide ions. The calcium metal ions of the additive can enter the perovskite lattice in the form of interstitial doping. Since calcium ions have a strong interaction with the charged defects in the perovskite, they can effectively inhibit the movement of ions inside the perovskite and improve the stability of the luminescence spectrum.

[0008] The present invention also provides a method for preparing the above-mentioned perovskite film, the specific steps of which are:

[0009] Step 1, dissolving guanidine chloride, cesium bromide, lead bromide, lead chloride, phenethylammonium bromide (PEABr), and calcium trifluoromethanesulfonate in a corresponding solvent, and then stirring at 20-30°C for 12-24 hours to dissolve the materials, thereby obtaining a perovskite solution;

[0010] Step 2, spin-coating the perovskite solution onto the substrate, and then annealing to remove the solvent, the annealing temperature is 50-60, the time is 10-12min, and the perovskite film is prepared on the surface of the substrate.

[0011] The molar ratio of guanidine chloride, cesium bromide, lead bromide, lead chloride, phenethylammonium bromide (PEABr), and calcium trifluoromethanesulfonate is 0.01:0.11:0.03:0.07:0.07:0.003, wherein the concentration of lead bromide is maintained at 0.1M;

[0012] The spin coating is performed at a rotation speed of 1000-1200 rpm for 5-8 s, and then at a rotation speed of 40000-5000 rpm for 120-130 s.

[0013] Wherein, the solvent is dimethyl sulfoxide (DMSO), N,N-dimethylformamide (DMF), or a mixture of the two;

[0014] Wherein, the substrate is ITO conductive glass, glass, quartz, silicon substrate and the like.

[0015] The present invention also provides a perovskite LED device, which includes a hole transport layer, a perovskite film and an electron transport layer;

[0016] The method for preparing the perovskite LED device comprises the following specific steps:

[0017] (1) Forming a hole transport layer on a substrate: the steps are as follows: dissolving TFB and PVK in a CB solvent at a mass ratio of X:(10-X), stirring to obtain a hole transport layer solution; coating the solution on the substrate, and annealing to obtain a thin film, namely the hole transport layer; X=0-10; preferably X=2-8, and more preferably X=2.5.

[0018] (2) forming a perovskite film on the hole transport layer using the perovskite film preparation method;

[0019] (3) forming an electron transport layer on the perovskite film

[0020] (4) forming an electrode on the electron transport layer. Specifically, a composite electrode is prepared on the surface of the electron transport layer by using aluminum and LiF as evaporation sources through a vapor deposition method.

[0021] The preparation method of the perovskite LED device is simple and easy to operate. The prepared perovskite LED film has good stability under working conditions, which provides a new method for preparing stably working perovskite LED devices. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 FIG. 1 is a schematic diagram of the structure of a perovskite LED device in one embodiment of the present invention.

[0023] Figure 2 The photoluminescence (PL) spectra prepared in Examples 2 to 4 of the present invention and Comparative Example 1 vary with time under light (excitation light wavelength: 365 nm).

[0024] Figure 3 Surface morphology of the perovskite films prepared in Examples 2 to 4 of the present invention and Comparative Example 1.

[0025] Figure 4 1 is an X-ray diffraction (XRD) graph of the perovskite films prepared in Examples 2 to 4 of the present invention and Comparative Example 1.

[0026] Figure 5 Graph showing the photoluminescence performance of the perovskite films prepared in Examples 2 and 3 of the present invention and Comparative Example 1.

[0027] Figure 6 1 and 2 are X-ray photoelectron spectroscopy (XPS) graphs of the perovskite films prepared in Example 2 of the present invention and Comparative Example 1.

[0028] Figure 7 Graphs of time-resolution fluorescence spectra (TRPL) of the perovskite films prepared in Examples 2 and 3 of the present invention and Comparative Example 1.

[0029] Figure 8This is a comparison chart of the efficiencies of the perovskite devices prepared in Examples 2 and 3 of the present invention and Comparative Example 1. DETAILED DESCRIPTION

[0030] The present invention is further described below by way of embodiments in conjunction with the accompanying drawings.

[0031] Embodiment 1, the preparation of perovskite film, comprises the following steps:

[0032] S1. Dissolve guanidine chloride, cesium bromide, lead bromide, lead chloride, PEABr, and calcium trifluoromethanesulfonate in corresponding solvents and stir them evenly to prepare a perovskite precursor solution. The molar ratio of guanidine chloride, cesium bromide, lead bromide, lead chloride, phenethylammonium bromide (PEABr), and calcium trifluoromethanesulfonate is 0.01:0.11:0.03:0.07:0.07:0.003, wherein the concentration of lead bromide is maintained at 0.1M.

[0033] S2. coating the perovskite solution onto the substrate and performing annealing treatment to obtain a perovskite film.

[0034] The substrate can specifically be ITO conductive glass, glass, quartz, silicon substrate, etc.; the coating can be spin coating, blade coating, etc.; the solvent is dimethyl sulfoxide (DMSO); trifluoromethanesulfonate ions can passivate the inherent defects in the perovskite film through Lewis acid-base interaction, and the volume of the particles in the precursor solution will increase after coordination, thereby forming a larger grain size.

[0035] Step S1 specifically comprises: dissolving guanidine chloride, cesium bromide, lead bromide, lead chloride, PEABr, and calcium trifluoromethanesulfonate in corresponding solvents, and then stirring at 20° C. for 12 to 24 hours to dissolve the materials, thereby obtaining a perovskite solution.

[0036] Step S2 is specifically as follows: spin coating the perovskite solution onto the substrate, and then heating at 60°C for 10 minutes to remove the DMSO solvent, thereby preparing a perovskite film on the substrate surface; wherein the spin coating speed is 1000 rpm, the spin coating time is 5 seconds, and then at a spin coating speed of 4000 rpm, the spin coating time is 120 seconds.

[0037] The present invention also provides a perovskite film, which is prepared by the above preparation method.

[0038] The present invention also provides a perovskite device, comprising the perovskite film prepared as above.

[0039] Specifically, the perovskite devices include light-emitting diodes (LEDs), lasers, photodetectors, field-effect transistors, and solar cells, and can greatly improve the performance of these devices; for example, the perovskite film can be used as the light-emitting layer of a light-emitting diode; the perovskite film can be used as the photosensitive layer of a solar cell;

[0040] When the light-emitting layer of a light-emitting diode adopts the perovskite film of the present invention, the energy loss caused by the non-radiative recombination of carriers is effectively reduced, the fluorescence intensity of the perovskite film and the life of the carriers are increased, thereby improving the performance of the light-emitting device.

[0041] Furthermore, the present invention also provides a perovskite LED device, such as Figure 1 As shown, including:

[0042] Substrate 1;

[0043] A hole transport layer 2, located on one side of the substrate 1;

[0044] The perovskite film 3 prepared as above is located on a side of the hole transport layer 2 away from the substrate 1;

[0045] The electron transport layer 4 is located on a side of the perovskite film 3 away from the substrate 1;

[0046] The metal electrode layer 5 is located on a side of the electron transport layer 4 away from the substrate 1;

[0047] The material of the hole transport layer 2 is TFB / PVK;

[0048] The material of the electron transport layer 4 is TPBi;

[0049] The material of the metal electrode layer 5 is LiF / aluminum.

[0050] The present invention also provides a method for preparing a perovskite LED device, comprising the following steps:

[0051] A1. Provide a substrate;

[0052] A2. Prepare a hole transport layer on one side of the substrate:

[0053] A3, preparing the above-mentioned perovskite film on the side of the hole transport layer away from the substrate;

[0054] A4, preparing an electron transport layer on a side of the perovskite film away from the substrate;

[0055] A5. Prepare a metal electrode layer on the side of the electron transport layer away from the substrate.

[0056] The substrate can be ITO conductive glass, glass, quartz, silicon substrate, etc., and the hole transport layer is prepared on the substrate, and the substrate is cleaned with deionized water, acetone, alcohol, and deionized water in sequence for 20 to 30 minutes (that is, each cleaning process is cleaned for 20 to 30 minutes), and then the cleaned substrate is blown dry with an ear bulb or nitrogen or argon, and then sent to a plasma cleaning machine for cleaning for 10 to 20 minutes; in step A3, the above-mentioned perovskite film is prepared on the side of the hole transport layer away from the substrate. The perovskite solution prepared above is coated on the side of the hole transport layer away from the substrate and heated, that is, the perovskite film is prepared on the side of the hole transport layer away from the substrate; specifically, the perovskite solution is spin-coated onto the hole transport layer, and then heated at 60°C for 10 minutes to remove the DMSO solvent, that is, the perovskite film is prepared on the hole transport layer: wherein the spin coating rotation speed is 1000 rpm, the spin coating time is 5 s, and then at a rotation speed of 4000 rpm, the spin coating time is 120 s.

[0057] Furthermore, the preparation method of the hole transport layer includes the following steps: dissolving TFB and PVK in a CB solvent, stirring to obtain a hole transport layer solution; coating the solution on the substrate, and annealing to obtain a thin film, namely the hole transport layer. Specifically, the mass ratio of TFB to PVK is 2.5:7.5.

[0058] Specifically, the TFB / PVK precursor is coated on the substrate, and the TFB / PVK film obtained after annealing is the hole transport layer; the coating method can be spin coating, scraper coating, etc., and the annealing temperature is 120° C. and the time is 15 minutes.

[0059] Furthermore, the method for preparing the electron transport layer is to form the electron transport layer on the perovskite film by using TPBi as an evaporation source through a vapor deposition method.

[0060] Specifically, during the evaporation process, the vacuum degree of the evaporation machine is reduced to 1*10 -4 Pa or less, and the vapor deposition is carried out at a current of 6 to 10 mA, and the thickness of the TPBi vapor deposition is 40 nm.

[0061] Furthermore, the preparation method of the metal electrode layer is: using LiF and aluminum as evaporation sources to prepare a composite electrode on the surface of the electron transport layer by evaporation; specifically, during the evaporation process, the vacuum degree of the evaporator is evacuated to 1*10 -4 Pa or less, and the vapor deposition is carried out at a current of 12 to 13 mA, the thickness of the LiF vapor deposition is 1 to 2 nm, and the thickness of the aluminum electrode vapor deposition is 90 to 110 nm; in practice, if it is necessary to prepare an array-arranged aluminum electrode layer on the surface of the electron transport layer, a mask corresponding to the array is set on the surface of the electron transport layer, and then it is placed in a vapor deposition machine for vapor deposition, and the array-arranged aluminum electrode layer can be obtained.

[0062] Obviously, in addition to the evaporation method, the metal electrode layer can also be prepared by magnetron sputtering, chemical vapor deposition, physical vapor deposition, etc. The following further describes the preparation method of the perovskite film and perovskite LED device of the present application with specific examples.

[0063] Example 2, preparation of a perovskite LED device, comprising the following steps:

[0064] A1. Provide an ITO conductive glass (2cm*2cm). Clean the ITO conductive glass with deionized water, acetone, alcohol, and deionized water for 25 minutes in sequence. Blow dry the cleaned conductive glass with nitrogen. Then, place it in a plasma cleaning machine (model DIENER PLASMA ATTO) for 15 minutes, and then blow dry it with nitrogen for standby use.

[0065] A2. Prepare a hole transport layer on one side of the ITO conductive glass;

[0066] A3, preparing a perovskite film on the side of the hole transport layer away from the ITO conductive glass;

[0067] A4, preparing an electron transport layer on the side of the perovskite film away from the ITO conductive glass;

[0068] A5. Prepare a metal electrode layer on the side of the electron transport layer away from the ITO conductive glass;

[0069] The method for preparing the hole transport layer in step A2 is as follows: dissolving TFB and PVK in a CB solvent, stirring to obtain a hole transport layer solution; coating the solution on the substrate, and annealing to obtain a thin film, namely the hole transport layer. Specifically, the ratio of TFB to PVK is 2.5:7.5.

[0070] The preparation method of the perovskite film in step A3 is specifically as follows: dissolve guanidine chloride, cesium bromide, lead bromide, lead chloride, phenethylammonium bromide, and 3%M calcium trifluoromethanesulfonate in 2ml of dimethyl sulfoxide solvent, stir at 20°C for 24h to dissolve the materials, and stand to obtain a perovskite solution: take 500uL of the perovskite solution and spin coat, the speed during spin coating is 1000rpm, the spin coating time is 5s, and then at a speed of 4000rpm, the spin coating time is 120s. Apply to the surface of the hole transport layer obtained in A2, and heat at 60°C for 10min after spin coating to obtain a perovskite film.

[0071] The preparation method of the electron transport layer in step A4 is specifically as follows: using TPBi as an evaporation source to form an electron transport layer on the perovskite film by evaporation. Specifically, during the evaporation process, the vacuum degree of the evaporator is evacuated to 1*10 -4Pa or less, and the vapor deposition is carried out at a current of 6 to 10 mA, and the thickness of the TPBi vapor deposition is 40 nm.

[0072] The preparation method of the metal electrode layer in step A5 is specifically as follows: placing a mask on the electron transport layer obtained in step A4, placing the device after step A4 in an evaporation machine, and using LiF and aluminum as evaporation sources to prepare a composite electrode on the surface of the electron transport layer by evaporation; specifically, during the evaporation process, the vacuum degree of the evaporation machine is evacuated to 1*10 -4 Pa or less, and the vapor deposition is carried out at a current of 12 to 13 mA, the thickness of the LiF vapor deposition is 1 to 2 nm, and the thickness of the aluminum electrode vapor deposition is 90 to 110 nm; in practice, if it is necessary to prepare an array-arranged aluminum electrode layer on the surface of the electron transport layer, a mask corresponding to the array is set on the surface of the electron transport layer, and then it is placed in a vapor deposition machine for vapor deposition, and the array-arranged aluminum electrode layer can be obtained.

[0073] The final structure of the perovskite LED device is as follows: Figure 1 shown.

[0074] Example 3, preparation of a perovskite LED device is the same as Example 2, except that 1%M calcium trifluoromethanesulfonate is added when preparing the perovskite film in step A3, and the rest of the process is the same as Example 2.

[0075] Example 4, a method for preparing a perovskite LED device, is the same as Example 2, except that 5%M calcium trifluoromethanesulfonate is added when preparing the perovskite film in step A3, and the rest of the process is the same as Example 2.

[0076] Comparative Example 1, a method for preparing a perovskite LED device is the same as that of Example 2, except that calcium trifluoromethanesulfonate is not added when preparing the perovskite film in step A3, and the rest of the process is the same as that of Example 2.

[0077] The photoluminescence PL of the perovskite films prepared in the above Examples 2 to 4 and Comparative Example 1 was tested to change with time under light (excitation light wavelength: 365 nm). The results are as follows: Figure 2 shown. Figure 2 0% is the PL spectrum of the perovskite film prepared in Comparative Example 1, 1% is the PL spectrum of the perovskite film prepared in Example 2, 3% is the PL spectrum of the perovskite film prepared in Example 3, and 5% is the PL spectrum of the perovskite film prepared in Example 4.

[0078] from Figure 2It can be seen that the photoluminescence PL of the perovskite film in Comparative Example 1 has a significant red shift with time under excitation light. The addition of calcium trifluoromethanesulfonate significantly inhibits the red shift, so that the spectrum peak is riveted at 463nm, slightly blue-shifted; and the PL intensity is the largest when 3% is added.

[0079] The surface morphology of the perovskite films prepared in Examples 2 to 4 and Comparative Example 1 was tested. The results are as follows: Figure 3 shown. Figure 3 0% is the surface morphology of the perovskite film prepared in Comparative Example 1, 1% is the surface morphology of the perovskite film prepared in Example 3, 3% is the surface morphology of the perovskite film prepared in Example 2, and 5% is the surface morphology of the perovskite film prepared in Example 4.

[0080] from Figure 3 It can be seen that calcium trifluoromethanesulfonate can significantly change the morphology of the perovskite film. When calcium trifluoromethanesulfonate is not added, the perovskite grains are very small and the film is too dense. When the amount of calcium trifluoromethanesulfonate added increases, the perovskite film becomes uniform and the crystal size of the perovskite increases. When the amount of calcium trifluoromethanesulfonate added is 3%, the quality of the perovskite film is the best.

[0081] The XRD curves of the perovskite films prepared in Examples 2 to 4 and Comparative Example 1 are tested, and the results are as follows: Figure 4 shown. Figure 4 0% represents the XRD curve of the perovskite film prepared in Comparative Example 1, 1% represents the XRD curve of the perovskite film prepared in Example 3, 3% represents the XRD curve of the perovskite film prepared in Example 2, and 5% represents the XRD curve of the perovskite film prepared in Example 4.

[0082] from Figure 4 It can be seen that the addition of calcium trifluoromethanesulfonate to the perovskite film will not change the position of the perovskite diffraction peak, but the addition of calcium trifluoromethanesulfonate can enhance the crystallinity of the perovskite film. When the addition amount of calcium trifluoromethanesulfonate is 3%, the XRD diffraction peak of the perovskite film is the strongest in the 100 direction.

[0083] The photoluminescence performance of the perovskite films prepared in Examples 2, 3 and Comparative Example 1 was tested. The results are as follows: Figure 5 As shown. The test method of photoluminescence performance uses a photoluminescence fluorescence spectrometer with an excitation wavelength of 325nm laser to measure the relative fluorescence intensity of the perovskite film.

[0084] Figure 50% represents the photoluminescence curve of the perovskite film prepared in Comparative Example 1, 1% represents the photoluminescence curve of the perovskite film prepared in Example 3, 3% represents the photoluminescence curve of the perovskite film prepared in Example 2, and 5% represents the photoluminescence curve of the perovskite film prepared in Example 4.

[0085] from Figure 5 It can be seen that the addition of calcium trifluoromethanesulfonate can greatly improve the fluorescence intensity of the perovskite film and has no effect on the perovskite peak position.

[0086] The XPS graphs of the perovskite films prepared in Example 2 and Comparative Example 1 were tested, and the results were as follows: Figure 6 shown. Figure 6 0% represents the XPS curve of the perovskite film prepared in Comparative Example 1, and 3% represents the XPS curve of the perovskite film prepared in Example 2. Figure 6 It can be seen that calcium trifluoromethanesulfonate makes Ca 2p The peak indicates that Ca 2+ Present in perovskite films. Pb 4f The electron density increases and shifts toward the direction of low binding energy, proving that the Pb ion coordinates with the lone pair of electrons of oxygen in the sulfur-oxygen double bond in trifluoromethanesulfonic acid.

[0087] The fluorescence lifetime of the perovskite films prepared in Example 2 and Comparative Example 1 was tested. The results are as follows: Figure 7 As shown. The test method uses a transient steady-state fluorescence spectrometer to measure the fluorescence lifetime of the perovskite film, where the fluorescence lifetime is obtained based on the second-order exponential fitting, and the formula is:

[0088]

[0089] Among them, A1 and A2 are constants, τ1 and τ2 are the fast fluorescence lifetime component and the slow fluorescence lifetime component, respectively, which are measured by the instrument. avg is the average fluorescence lifetime, which is given by the formula:

[0090]

[0091] Calculated.

[0092] It can be seen from the figure that the addition of calcium trifluoromethanesulfonate can significantly increase the fluorescence lifetime of the perovskite film, from the initial average fluorescence lifetime of 1.96ns to 5.46ns. The increase in fluorescence lifetime is related to the reduction of internal defect states in the perovskite film.

[0093] The efficiency of the perovskite LED device prepared in Example 2 was tested, and the results were as follows: Figure 80% represents the efficiency of the perovskite LED device prepared in Comparative Example 1, 1% represents the efficiency of the perovskite LED device prepared in Example 3, and 3% represents the efficiency of the perovskite LED device prepared in Example 2.

[0094] pass Figure 8 It can be seen that the addition of calcium trifluoromethanesulfonate can improve the EQE of the device. The average efficiency of the device with 3% calcium trifluoromethanesulfonate added is increased from 2.2% to 2.9%.

[0095] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A perovskite film, characterized in that: A slurry consisting of an ABX3 organic-inorganic perovskite material and a salt containing metal cations is coated on a substrate and then annealed; the molar ratio of the salt containing metal cations is 1 mol% to 5 mol%; in the perovskite-type ABX3 organic-inorganic hybrid material, A is selected from PEA+, GA+, Cs+, B is Pb2+, and X is Br- or Cl-; the salt containing metal cations is calcium trifluoromethanesulfonate Ca(CF3SO3)2.

2. A method for preparing a perovskite film as claimed in claim 1, characterized in that: The specific steps are: Step 1, dissolving guanidine chloride, cesium bromide, lead bromide, lead chloride, phenethylammonium bromide (PEABr), and calcium trifluoromethanesulfonate in a corresponding solvent, and then stirring at 20-30° C. for 12-24 hours to dissolve the materials, thereby obtaining a perovskite solution; Step 2, spin-coating the perovskite solution onto the substrate, and then annealing to remove the solvent, the annealing temperature is 50-60°C, and the time is 10-12min, so that a perovskite film is prepared on the surface of the substrate.

3. The method for preparing the perovskite thin film according to claim 2, characterized in that: The molar ratio of guanidine chloride, cesium bromide, lead bromide, lead chloride, phenethylammonium bromide (PEABr), and calcium trifluoromethanesulfonate is 0.01:0.11:0.03:0.07:0.07:0.003, wherein the concentration of lead bromide is maintained at 0.1M.

4. The method for preparing a perovskite thin film according to claim 2, characterized in that: The spin coating is performed at a rotation speed of 1000-12000 rpm for 5-8 seconds, and then at a rotation speed of 4000-5000 rpm for 120-130 seconds.

5. The method for preparing a perovskite thin film according to claim 2, characterized in that: The solvent is dimethyl sulfoxide (DMSO), N,N-dimethylformamide (DMF), or a mixture thereof.

6. The method for preparing a perovskite thin film according to claim 2, characterized in that: The substrate is selected from ITO conductive glass, glass, quartz, and silicon substrate.

7. A perovskite LED device, characterized in that: It comprises a hole transport layer, the perovskite film as claimed in claim 1 and an electron transport layer.

8. The method for preparing a perovskite LED device according to claim 7, characterized in that: The specific steps are: (1) Forming a hole transport layer on a substrate: dissolving TFB and PVK in a CB solvent at a mass ratio of X:(10-X), and stirring to obtain a hole transport layer solution; The solution is coated on the substrate, and a thin film is obtained after annealing, which is the hole transport layer; X is 0-10; (2) forming a perovskite film on the hole transport layer using the perovskite film preparation method according to any one of claims 2 to 5; (3) forming an electron transport layer on the perovskite film; (4) forming an electrode on the electron transport layer. Specifically, a composite electrode is prepared on the surface of the electron transport layer by using aluminum and LiF as evaporation sources through a vapor deposition method.

Citation Information

Patent Citations

  • Preparation method based on quasi-two-dimensional perovskite layer and solar cell

    CN114267796A

  • Perovskite photoelectric device using fluorine-containing sulfonate interface modifier and preparation method thereof

    CN116096112A

  • Organic light-emitting element

    JP2004335136A