Barium titanate particle powder and method for producing same
By generating barium titanate particle powder with specific particle size distribution and oil absorption properties in aqueous solvents, the problems of dispersion and burning reduction of barium titanate particles in MLCC are solved, and barium titanate particle powder is realized in MLCC uniform dispersion and high mechanical strength.
Patent Information
- Application Number
- CN202380030340.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-30
- Filing Date
- 2023-03-28
- Publication Date
- 2024-12-06
AI Technical Summary
In the prior art, barium titanate particles are difficult to disperse uniformly in aqueous and non-aqueous solvents, resulting in peeling easily during the sintering process between the dielectric layer and the internal electrode layer in MLCC, and the calcination reduction is large, which affects mechanical reliability. .
By generating barium titanate particle powder with specific particle size distribution and oil absorption properties in an aqueous solvent, the average primary particle size is 20 nm or more and 150 nm or less, the D95/D50 value is 5 or less, and the maximum oil absorption torque is 0.2N·m Below, high-purity barium titanate particle powder is generated by solution reaction in the aqueous solvent and hydrothermal treatment to ensure good dispersion and low calcination reduction in aqueous and non-aqueous solvents.
The barium titanate particle powder is uniformly dispersed in MLCC, reducing the thermal shrinkage difference between the electrode layer and the dielectric layer inside Ni, improving the mechanical strength and reliability of MLCC, and is suitable for resins with high dielectric constant and high refractive index. membrane.
Smart Images

Figure CN119095799A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a barium titanate particle powder and a method for producing the same. Specifically, the barium titanate particle powder is highly crystalline and fine, and is easily dispersed in both aqueous solvents and non-aqueous solvents, so it can be appropriately used as a raw material for small high-performance electronic parts or optical parts, and because it has a low ignition loss, it can also be appropriately used in MLCC. Background Art
[0002] In recent years, the miniaturization and lightening of electronic devices such as mobile phones and personal computers have been accelerating, and the miniaturization and increasing of the capacitance of capacitors in the circuits included therein and the miniaturization and increasing of the transmittance of optical films have been progressing.
[0003] As electronic and optical components become smaller, have higher capacity, and have higher transmittance, there is an increasing demand for barium titanate particle powders that are highly crystalline and fine and that are easily dispersible in both aqueous and non-aqueous solvents.
[0004] From the viewpoint of reducing the thickness of the resin film containing the barium titanate particle powder used in the above-mentioned parts, there is an increasing demand for the barium titanate particle powder to be easily dispersed in both aqueous solvents and non-aqueous solvents.
[0005] In a multilayer ceramic capacitor (hereinafter referred to as “MLCC”) in which dielectric layers and internal electrode layers are alternately stacked, barium titanate particle powder is used as a raw material for the dielectric layers, and Ni particle powder is used as a raw material for the internal electrode layers.
[0006] In recent years, MLCCs have been becoming smaller and larger in capacity, and the thickness of the dielectric layer and the internal electrode layer are both 1 μm or less. Therefore, the particle size of the barium titanate particle powder and the Ni particle powder used as raw materials is required to be submicron or less.
[0007] MLCC is usually made of slurry or paste for forming the dielectric layer and the internal electrode layer. Since the dried films of the slurry are alternately stacked and fired, the Ni particles of the internal electrode layer and the barium titanate particles of the dielectric layer are sintered at the same time.
[0008] However, Ni particles with a size of less than submicron are sintered at a temperature several hundred degrees lower than barium titanate particles of the same size. Therefore, there is a problem that the dielectric layer and the internal electrode layer after stacking are easily peeled off due to the difference in thermal shrinkage characteristics between Ni particles and barium titanate particles.
[0009] As a highly crystalline and fine barium titanate particle powder, if it can be easily dispersed in both aqueous solvents and non-aqueous solvents, it can be appropriately used as a raw material for small electronic parts and optical parts. In addition to the above characteristics, in the case of barium titanate particle powder with a small ignition loss, if it is used for MLCC sintering, the dielectric layer and the Ni internal electrode layer are not easily peeled off, and it can be expected that MLCC with high mechanical reliability can be manufactured.
[0010] Prior art literature
[0011] Non-patent literature
[0012] Non-patent document 1: Takeshi Nomura, supervisor, “Materials, manufacturing and mounting technologies and the latest trends in multilayer ceramic capacitors (MLCCs),” published by R&D Support Center Co., Ltd., October 30, 2020.
[0013] Non-patent document 2: Research Report No. 19, Inorganic Materials Research Institute, Science and Technology Agency, “Research on Titanium Oxide,” 1979.
[0014] Patent Literature
[0015] Patent Document 1: Japanese Patent Application Publication No. 2005-289668. Summary of the invention
[0016] Problems to be solved by the invention
[0017] Non-Patent Document 1 and Patent Document 1 describe the use of fine and highly dispersible barium titanate particles as a sintering retardant material for Ni particles.
[0018] However, in the technology described in Non-Patent Document 1 or Patent Document 1, it is necessary to use a large amount of a dispersant as a common material for dispersing the barium titanate particles in the Ni particles, or to perform strong mechanical uniform distribution for dispersion.
[0019] However, if a large amount of dispersant is used or the particles are evenly distributed with great force, the barium titanate particles and the Ni particles may be chipped, and thus the particles may not be used as raw materials for thin-layer ceramic capacitors or raw materials for small electronic parts or optical parts.
[0020] The inventors of the present invention have repeatedly conducted several trials and experiments to solve the above-mentioned problems. As a result, they have obtained the following remarkable insights and completed the above-mentioned technical problems: If the average primary particle size of the barium titanate particle powder is 20 nm or more and 150 nm or less, the 50% diameter D of the cumulative frequency distribution of the agglomerated particles in the aqueous solvent is 50 and 95% diameter D 95 D 95 / D 50If the value is 5 or less and the maximum torque of the oil absorption characteristic is 0.2 N·m or less, it is a highly crystalline and fine barium titanate particle powder, which can form barium titanate that is easily dispersed in both aqueous solvents and non-aqueous solvents and has a small ignition loss.
[0021] Technical solutions to solve problems
[0022] The above technical problems can be solved by the following present invention.
[0023] The present invention is a barium titanate particle powder, wherein the average primary particle size is 20 nm or more and 150 nm or less, and the 50% diameter D of the cumulative frequency distribution of agglomerated particles in an aqueous solvent is 50 and 95% diameter D 95 D 95 / D 50 The value of is 5 or less, and the maximum torque of the oil absorption characteristic is 0.2 N·m or less.
[0024] Furthermore, the present invention provides the barium titanate particle powder, wherein the work done by the twin-screw kneader in the oil absorption characteristic is 40 J / g or less.
[0025] Furthermore, the present invention provides the barium titanate particle powder, wherein the ignition loss is 4.0 wt% or less.
[0026] In addition, the present invention is a method for producing barium titanate particle powder, which comprises at least: a first step of generating a mixed titanic acid of orthotitanic acid and metatitanic acid by a solution reaction in an aqueous solvent; and a second step of mixing the mixed titanic acid and a barium compound at a temperature above 60° C. and below 105° C. to generate barium titanate.
[0027] The present invention is also a method for producing the barium titanate particle powder, wherein the first step is a step of subjecting orthotitanic acid generated from titanium chloride and a neutralizer to a dehydration reaction at 50° C. to 85° C. to generate a mixed titanic acid of orthotitanic acid and metatitanic acid.
[0028] Furthermore, the present invention is the method for producing the barium titanate particle powder, wherein the impurity elements contained in the mixed titanic acid in the first step are 1000 ppm or less.
[0029] In addition, the present invention is the method for producing the barium titanate particle powder, wherein when the mixed titanic acid is represented by TiO2·nH2O, n of the mixed titanic acid in the first step is 0.5≤n≤1.5.
[0030] The present invention is also a barium titanate particle powder having an average primary particle size of 20 nm or more and 150 nm or less, and a 50% diameter D of the cumulative frequency distribution of aggregated particles in an aqueous solvent. 50and 95% diameter D 95 D 95 / D 50 The value of is 5 or less, and the oil absorption at the maximum moment of the oil absorption characteristic is (36-0.08×average primary particle size) mL / 100 g or less.
[0031] In addition, the present invention is a dispersion comprising the barium titanate particle powder.
[0032] Effects of the Invention
[0033] The barium titanate particle powder of the present invention is fine, with an average primary particle size of 20nm to 150nm, and is highly crystalline, easily dispersible in both aqueous and non-aqueous solvents, and has a low ignition loss.
[0034] Therefore, when the barium titanate particle powder according to the present invention is added as a common material to a paste containing Ni particles for use in an internal electrode layer of an MLCC, the barium titanate particles can be uniformly dispersed around the Ni particles.
[0035] Since the barium titanate particles are uniformly dispersed, a Ni paste having a low viscosity can be prepared.
[0036] In addition, in the Ni dry film using the above-mentioned Ni paste, barium titanate particles uniformly dispersed around the Ni particles can be observed. Therefore, the thermal shrinkage of the above-mentioned Ni dry film due to sintering is reduced due to the particle growth inhibition effect of the Ni particles. Therefore, the difference in thermal shrinkage characteristics between the Ni internal electrode layer obtained from each paste dry film and the dielectric layer containing the barium titanate particle powder is reduced, and even if the Ni internal electrode layer and the dielectric layer are sintered at the same time, the Ni internal electrode layer and the dielectric layer are not easily peeled off.
[0037] In addition, since simultaneous firing is possible, mechanical strength is improved, and a highly reliable MLCC can be provided.
[0038] Furthermore, a slurry in which the barium titanate particle powder according to the present invention is dispersed forms a resin film having a high dielectric constant and a high refractive index. Furthermore, since a thin film can be formed, the slurry can be suitably used for capacitors or optical films. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 This is a scanning electron microscope (SEM) image of the barium titanate particle powder of Example 1 (25,000 times).
[0040] Figure 2 This is the particle size distribution of the primary particles of the barium titanate particle powder of Example 1 and the aggregated particles in the aqueous solvent.
[0041] Figure 3This is the oil absorption characteristic of 15 g of the barium titanate particle powder of Example 1.
[0042] Figure 4 This is a graph showing the dependency of the oil absorption at the maximum moment on the average primary particle size in Examples and Comparative Examples. DETAILED DESCRIPTION
[0043] As described below, the structure of the present invention will be described in more detail.
[0044] First, the barium titanate particle powder according to the present invention will be described.
[0045] The average primary particle size of the barium titanate particle powder according to the present invention is 20 nm to 150 nm, preferably 25 nm to 140 nm, and more preferably 30 nm to 130 nm.
[0046] This is because, if the particle size is less than 20 nm, it is difficult to industrialize, that is, to safely and mass-produce the barium titanate particle powder in the present invention that satisfies the necessary conditions of the maximum moment of the cumulative frequency distribution of the agglomerated particles or the oil absorption characteristics. In addition, if the particle size exceeds 150 nm, it may not be used for small electronic parts and optical parts.
[0047] The 50% diameter D of the cumulative frequency distribution of the aggregated particles of the barium titanate particle powder according to the present invention in the aqueous solvent is 50 and 95% diameter D 95 D 95 / D 50 The value of is 5 or less, preferably 1.9 or less, and more preferably 1.8 or less.
[0048] This is because if D 95 / D 50 When the value of exceeds 5, it may be difficult to disperse in an aqueous solvent.
[0049] The maximum moment of the oil absorption characteristic of the barium titanate particle powder according to the present invention is 0.2 N·m or less, preferably 1.9 N·m or less, and more preferably 1.8 N·m or less.
[0050] This is because if it exceeds 0.2 N·m, it may be difficult to disperse in a non-aqueous solvent.
[0051] The work of the twin-screw kneader in the oil absorption characteristics of the barium titanate particle powder according to the present invention is preferably 40 J / g or less, more preferably 38 J / g or less, and even more preferably 36 J / g or less.
[0052] This is because if it exceeds 40 J / g, it may be difficult to disperse in a non-aqueous solvent.
[0053] The ignition loss of the barium titanate particle powder according to the present invention is preferably 4.0 wt % or less, more preferably 3.8 wt % or less, and even more preferably 3.6 wt % or less.
[0054] This is because the main factors of the ignition loss include the thermal decomposition of unreacted barium carbonate in the sample, the release of crystal water and chemically adsorbed water. Therefore, if the ignition loss exceeds 4.0wt%, it is considered to be a sample with poor crystallinity and may not be used as a raw material for electronic parts and optical parts.
[0055] The barium titanate particle powder according to the present invention is preferably of high purity because it may affect electronic components and optical components using the barium titanate particle powder.
[0056] Examples of impurity elements that may have an influence include Si, S, Cl, Ca, Fe, and Sr derived from the main raw material and N, Na, and K derived from the neutralizer.
[0057] The impurity elements derived from the main raw material are preferably 500 ppm or less, more preferably 400 ppm or less, and further preferably 300 ppm or less.
[0058] The impurity elements derived from the neutralizer are each preferably 20 ppm or less, more preferably 18 ppm or less, and further preferably 16 ppm or less.
[0059] The Ba / Ti composition ratio of the barium titanate particle powder according to the present invention is preferably 0.980 to 1.020, more preferably 0.985 to 1.015, and even more preferably 0.990 to 1.010.
[0060] If it is less than 0.980, a large amount of unreacted titanium may remain, resulting in low crystallinity and a decrease in dielectric constant and refractive index. If it exceeds 1.020, unreacted barium carbonate may increase, resulting in a decrease in dielectric constant and refractive index.
[0061] The BET specific surface area of the barium titanate particle powder of the present invention is preferably 6.0 m 2 / g~70m 2 / g, more preferably 6.2m 2 / g~65m 2 / g.
[0062] This is because if the BET specific surface area is 6.0 m 2 / g~70m 2 / g, the particle size converted from the BET specific surface area and the true density is close to the average primary particle size, and thus the barium titanate particle powder is highly crystalline.
[0063] The crystallite size of the barium titanate particle powder according to the present invention is preferably 12 nm to 180 nm, more preferably 15 nm to 170 nm.
[0064] This is because when the crystallite size is 12 nm to 180 nm, each particle is close to a single crystal.
[0065] The oil absorption at the maximum moment of the barium titanate particle powder according to the present invention is preferably 45 mL / 100 g or less, and more preferably 42 mL / 100 g or less.
[0066] This is because if the oil absorption at the maximum torque exceeds 45 mL / 100 g, it may be difficult to disperse in a non-aqueous solvent.
[0067] In the case of barium titanate particles having an average primary particle size of 25 nm or more, the powder according to the present invention preferably has a lattice constant ratio c / a of 1.0010 to 1.0250, and more preferably 1.0030 to 1.0200.
[0068] This is because if the relative humidity is less than 1.0010, the dielectric constant and the refractive index may decrease due to the low crystallinity of barium titanate, and it is difficult to produce barium titanate exceeding 1.0250.
[0069] In addition, in the case of barium titanate particles having an average primary particle size of less than 25 nm, a particle size effect is obtained, so that the lattice constant ratio c / a is close to 1.
[0070] The oil absorption at the maximum moment of the oil absorption characteristic of the barium titanate particle powder according to the present invention is (36-0.08×average primary particle size) mL / 100 g or less.
[0071] Next, the method for producing the barium titanate particle powder according to the present invention will be described.
[0072] The method for producing the barium titanate particle powder according to the present invention is described by a solution reaction in an aqueous solvent. This is because a solution reaction in an aqueous solvent is generally considered to be the most suitable. However, it is not limited to the solution reaction, and may also be a solid phase method obtained by mixing, crushing, and calcining raw materials, and a sol-gel method obtained by hydrolyzing an alkoxide metal.
[0073] Generally, titanium tetrachloride TiCl 4 is used as a raw material for barium titanate particle powder.
[0074] Since Cl in titanium tetrachloride becomes an impurity element, there is known a technique for washing titanic acid from titanium tetrachloride with water to produce high-purity barium titanate.
[0075] Generally, in a solution reaction in an aqueous solvent, when titanic acid is generated using TiCl4 as a raw material, the neutralization reaction represented by the following (Formula A), the dehydration reaction represented by (Formula B), and the hydrolysis reaction represented by (Formula C) are representative reactions.
[0076] (Neutralization reaction)
[0077] (Formula A)TiCl4+4MOH→Ti(OH)4+4MCl
[0078] <In (Formula A), M is Na, K, NH4, etc., and MOH is a neutralizer. The neutralizer can be a hydroxide of a divalent metal such as Ca(OH)2, or a carbonate of M'CO3. >
[0079] (Dehydration reaction)
[0080] (Formula B)TiO2·nH2O→TiO2·(n-1)H2O+H2O
[0081] <In (Formula B), n≤2. Here, in TiO2·nH2O, when n=2, it is orthotitanic acid, when n=1, it is metatitanic acid, and when 1<n<2, it is a mixed titanic acid of orthotitanic acid and metatitanic acid. Orthotitanic acid can also be represented by Ti(OH)4, and metatitanic acid can also be represented by TiO(OH)2. In addition, orthotitanic acid can also be represented by H4TiO4, and metatitanic acid can also be represented by H2TiO2. >
[0082] Here, orthotitanic acid is an amorphous or low-crystalline titanic acid, and metatitanic acid is used as an aggregate of crystalline anatase microcrystals. The generated titanic acid TiO2·nH2O (n≤2) is in the state of a white precipitate or a white dispersion. Therefore, a mixed titanic acid of orthotitanic acid and metatitanic acid is represented by TiO2·nH2O (0<n<2).
[0083] (Hydrolysis reaction)
[0084] (Formula C)TiCl4+(m+2)H2O→TiO2·mH2O+4HCl
[0085] <In (Formula C), m depends on the concentration of titanium tetrachloride in the reaction solution, pH, impurities in the solution, etc. At a certain high temperature, if the pH is high, metatitanic acid with m≈1 is generated. >
[0086] Here, the hydrolysis reaction of titanium tetrachloride refers to the formation of a white precipitate or a white dispersion when water is added to a transparent solution of titanium tetrachloride, or the formation of a white precipitate or a white dispersion after a certain period of time has passed since water was added to titanium tetrachloride.
[0087] The first and second steps in the method for producing barium titanate particle powder according to the present invention will be described.
[0088] The production method of the present invention is based on the reactions of (Formula A) and (Formula B).
[0089] The method is characterized in that in the first step of the production method of the present invention, a mixed titanic acid of orthotitanic acid and metatitanic acid is generated, and in the subsequent second step, the generated mixed titanic acid is mixed with a barium compound at 60°C to 105°C to generate barium titanate through a solution reaction.
[0090] The manufacturing method of the present invention is described in more detail below.
[0091] In the production method of the present invention, titanium chloride as a main raw material can be titanium tetrachloride TiCl4 or industrial titanium chloride (Cl / Ti<4).
[0092] In the production method of the present invention, it is preferred that the dehydration reaction of (Formula B) be performed after the neutralization reaction of (Formula A).
[0093] That is, the neutralization reaction is preferably carried out by dropping a neutralizing agent into industrial titanium chloride (Cl / Ti<4) diluted with water at a low temperature, and the low temperature is preferably in the range of 10°C to 60°C, more preferably 20°C to 55°C.
[0094] This is because, when the reaction temperature of (Formula A) exceeds 60°C during the dropwise addition, the hydrolysis reaction of (Formula C) may proceed due to heat generation during neutralization of titanium chloride, and when it is lower than 10°C, industrial control is difficult.
[0095] In the production method according to the present invention, the ratio of the neutralizing agent MOH to Cl in the titanium chloride, that is, the MOH / Cl value [mol ratio], is preferably 0.60 to 1.50, more preferably 0.70 to 1.40, and even more preferably 0.80 to 1.30.
[0096] This is because, if the MOH / Cl value exceeds 1.50, titanate containing M may be generated, and it is difficult to remove M by water washing. In the obtained barium titanate particle powder, a large amount of impurity M remains. If the MOH / Cl value is lower than 0.60, unreacted titanium chloride may remain. As a result of washing away the titanium chloride during water washing, the yield of the obtained barium titanate particle powder will decrease.
[0097] In the method for producing barium titanate particle powder involved in the present invention, the concentration of Ti after the neutralization reaction of (Formula A) and during the dehydration reaction of (Formula B) is preferably 0.2 mol / L to 3.5 mol / L, more preferably 0.3 mol / L to 3.2 mol / L, and further preferably 0.35 mol / L to 3.0 mol / L.
[0098] After the neutralization reaction (Formula A), the dehydration reaction (Formula B) is preferably carried out at 50°C to 85°C, more preferably 52°C to 83°C.
[0099] This is because a dehydration reaction is unlikely to occur at a temperature lower than 50°C, and if the temperature exceeds 85°C, titanic acid having low reactivity with barium may be generated.
[0100] A part of orthotitanic acid is converted into metatitanic acid by the dehydration reaction, thereby forming a mixed titanic acid containing orthotitanic acid and metatitanic acid.
[0101] The neutralization reaction to the dehydration reaction is preferably performed in a state where the reaction solution is placed in a gas of an oxidizing atmosphere.
[0102] This is because, in the case of an inert gas atmosphere, impurities are likely to remain in the titanate obtained after the subsequent water washing step, and it is difficult to obtain a high-purity barium titanate particle powder.
[0103] The so-called oxidizing atmosphere may be a pure oxygen atmosphere or an air atmosphere. Alternatively, the reaction solution may be bubbled with air to actively place it in an oxidizing atmosphere.
[0104] The titanic acid obtained in the first step is preferably a mixed titanic acid of orthotitanic acid obtained by neutralization reaction (Formula A) and metatitanic acid obtained by dehydration reaction (Formula B), and preferably does not contain a hydrolyzate after being subjected to a strong acid atmosphere of titanium chloride (Formula C).
[0105] On the other hand, it is also possible to generate titanic acid at a pH of 0.5 to 3.5 and a temperature of 40°C to 80°C according to (Formula C), and mix it with a mixed titanic acid of orthotitanic acid obtained by a neutralization reaction (Formula A) and titanic acid obtained by a dehydration reaction (Formula B) to generate a mixed titanic acid.
[0106] The mixed titanic acid obtained immediately after the first step may be washed with water.
[0107] This is because impurity elements contained in the mixed titanic acid obtained in the first step can be washed away by water washing.
[0108] In the water washing, the impurity elements contained in the mixed titanic acid after the water washing can be measured when the conductivity of the filtrate reaches 200 μS / cm as the end point.
[0109] The impurity elements contained in the mixed titanic acid after washing are preferably 1000 ppm or less, more preferably 800 ppm or less, and further preferably 500 ppm or less.
[0110] This is because, if the impurity elements exceed 1000 ppm respectively, in the barium titanate particle powder obtained after the second step, any one of the impurity elements Si, S, Cl, Ca, Fe, and Sr from the main raw material may exceed 500 ppm, and any one of the alkali metal elements Na and K from the impurities of the neutralizer may exceed 20 ppm.
[0111] When the mixed titanic acid is represented by TiO2·nH2O, the mixed titanic acid in the first step preferably has a value of 0.5≤n≤1.5, and more preferably 0.55 to 1.4.
[0112] When n exceeds 1.5, washing with water becomes difficult, impurity elements tend to remain, the resulting barium titanate has low crystallinity, the particle surface is not smooth, and the oil absorption characteristics tend to deteriorate.
[0113] On the other hand, when n is less than 0.5, the reactivity with Ba in the second step is low, and barium titanate having a low reaction rate is likely to be obtained.
[0114] As a solution reaction model of barium titanate, when an alkaline barium solution is mixed with titanic acid, titanic acid dissolves and barium titanate particles are generated. Impurities in titanic acid and impurities in the generated barium titanate can also be explained by this model.
[0115] In the second step, a mixed titanic acid and a barium compound are reacted in an aqueous solution to produce barium titanate particles.
[0116] In the second step, the slurry containing the mixed titanic acid obtained in the first step is preferably mixed with the barium compound as the main raw material, and reacted in an alkaline environment at a temperature within a range of 60° C. to 105° C.
[0117] The barium compound is preferably of high purity.
[0118] The barium compound is not particularly limited, and barium hydroxide can be exemplified.
[0119] The gas in contact with the solution during the reaction is preferably an oxidizing gas not containing carbon dioxide gas or an inert gas such as high-purity nitrogen.
[0120] This is to avoid the formation of barium carbonate.
[0121] The barium titanate particles may be crystallized by hydrothermal treatment after the second step.
[0122] In order to remove impurities such as excess Ba derived from the main raw material from the obtained slurry containing barium titanate particles, water washing may be performed.
[0123] The barium titanate particles produced in the aqueous solution can be obtained as barium titanate particle powder by removing water used in the solution reaction.
[0124] At this time, it is preferable to prevent the barium titanate particles from being firmly aggregated by crosslinking with water.
[0125] Examples of methods for preventing aggregation include instantaneous drying of the slurry containing the barium titanate particles according to a common method, and drying by replacing the slurry with a solvent having a crosslinking force smaller than that of water.
[0126] In addition, the barium titanate particle powder obtained by drying the slurry can also be pulverized by a dry method to prevent the particles from firmly agglomerating.
[0127] The obtained particle powder can also be further calcined and pulverized to improve the crystallinity of barium titanate.
[0128] Next, the dispersion containing the barium titanate particle powder according to the present invention will be described.
[0129] As the dispersion medium according to the present invention, either an aqueous system or a non-aqueous system can be used.
[0130] As the dispersion medium of the aqueous dispersion, water or alcohol solvents such as methanol, ethanol, propanol, isopropanol, butanol, etc.; glycol ether solvents such as methyl cellosolve, ethyl cellosolve, propyl cellosolve, butyl cellosolve, etc.; ethylene oxide or propylene oxide addition polymers such as diethylene glycol, triethylene glycol, polyethylene glycol, dipropylene glycol, tripropylene glycol, polypropylene glycol, etc.; alkylene glycols such as ethylene glycol, propylene glycol, 1,2,6-hexanetriol, etc.; water-soluble organic solvents such as glycerol and 2-pyrrolidone can be used. These dispersion media for aqueous dispersions can be used alone or in combination of two or more according to the target application.
[0131] As the dispersion medium for the non-aqueous dispersion, there can be used aromatic hydrocarbons such as toluene and xylene; ketones such as methyl ethyl ketone and cyclohexanone; amides such as N,N-dimethylformamide, N,N-dimethylacetamide, and N-methylpyrrolidone; ether alcohols such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, diethylene glycol monomethyl ether, propylene glycol monomethyl ether, and propylene glycol monoethyl ether; ether acetates such as ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, propylene glycol monomethyl ether acetate, and propylene glycol monoethyl ether acetate; acetates such as ethyl acetate, butyl acetate, and isobutyl acetate; lactic acid esters such as methyl lactate, ethyl lactate, and propyl lactate; cyclic esters such as ethylene carbonate, propylene carbonate, and γ-butyrolactone; and various monomers.
[0132] These dispersion media for non-aqueous dispersions may be used alone or in combination of two or more, depending on the intended use.
[0133] The concentration of the barium titanate particle powder in the dispersion according to the present invention is preferably adjusted to 5 to 60 wt %, more preferably 10 to 55 wt %, and even more preferably 15 to 50 wt %.
[0134] This is because if it is less than 5% by weight, the productivity for the next step is low, and if it exceeds 60% by weight, it is not certain that a slurry with high fluidity will be obtained.
[0135] The dispersion of the present invention may also contain additives such as dispersants, resins, defoamers, and auxiliary agents as needed.
[0136] As the dispersant in the present invention, it can be appropriately selected and used according to the type of barium titanate particle powder or dispersion medium used, and can be alkoxysilane, silane coupling agent and organic silicon compound such as organic polysiloxane; titanate coupling agent and other organic titanium compound; aluminate coupling agent and other organic aluminum compound; zirconium compound such as zirconate coupling agent and other surfactants or polymer dispersants such as high molecular weight dispersants can be used, these dispersants can be used alone or in combination of two or more.
[0137] Examples of the organosilicon compound include alkoxysilanes such as methyltrimethoxysilane, methyltriethoxysilane, dimethyldiethoxysilane, phenyltriethoxysilane, ethyltriethoxysilane, propyltriethoxysilane, butyltriethoxysilane, hexyltriethoxysilane, octyltriethoxysilane, tetraethoxysilane, and tetramethoxysilane; silane coupling agents such as vinyltrimethoxysilane, vinyltriethoxysilane, γ-aminopropyltriethoxysilane, γ-glycidoxypropyltrimethoxysilane, γ-mercaptopropyltrimethoxysilane, γ-methacryloxypropyltrimethoxysilane, N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane, γ-glycidoxypropylmethyldimethoxysilane, and γ-chloropropyltrimethoxysilane; and organopolysiloxanes such as polysiloxane, methylhydrogenpolysiloxane, and modified polysiloxane.
[0138] Examples of the organic titanium compound include isopropyl triisostearoyl titanate, isopropyl tri(dioctyl pyrophosphate acyloxy) titanate, bis(dioctyl pyrophosphate acyloxy) oxyacetate titanate, isopropyl tri(N-aminoethylaminoethyl) titanate, tri(dioctyl pyrophosphate acyloxy) ethylene titanate, isopropyl dioctyl pyrophosphate titanate, isopropyl tri(dodecylbenzenesulfonyl) titanate, titanium tetra-n-butoxide, titanium tetra-2-ethylhexoxide, tetraisopropyl bis(dioctyl) pyrophosphate ester titanate, Bis(dioctyl pyrophosphate) oxyacetate titanate, bis(dioctyl pyrophosphate) oxyacetate titanate, bis(dioctyl pyrophosphate) ethylene titanate.
[0139] Examples of the organoaluminum compound include acetoalkoxyaluminum diisopropionate, diisopropoxymonoethylaluminum acetoacetate, triethylaluminum acetoacetate, and aluminum triacetylacetonate.
[0140] Examples of the organic zirconium compound include zirconium tetraacetylacetonate, dibutoxyzirconium diacetylacetonate, tetraethylaluminum acetylacetate, tributoxymonoethylacetylacetate, and tributoxyzirconium acetylacetonate.
[0141] Examples of the surfactant include anionic surfactants such as fatty acid salts, sulfate ester salts, sulfonates, and phosphate ester salts; polyethylene glycol type nonionic surfactants such as polyethylene oxide alkyl ethers and polyethylene oxide aryl ethers; nonionic surfactants such as polyol type nonionic surfactants such as sorbitan fatty acid esters; cationic surfactants such as amine salt type cationic surfactants and quaternary ammonium salt type cationic surfactants; alkyl betaines such as alkyl dimethylaminoacetic acid betaine, and amphoteric surfactants such as alkyl imidazolines.
[0142] Examples of the polymer dispersant include styrene-acrylic acid copolymers, styrene-maleic acid copolymers, polycarboxylic acids and salts thereof.
[0143] The amount of the dispersant added depends on the total surface area of the barium titanate particle powder in the dispersion and can be appropriately adjusted according to the application of the dispersion of the barium titanate particle powder and the type of the dispersant.
[0144] Generally, by adding 0.01 wt % to 100 wt % of a dispersant to the barium titanate particle powder in the dispersion medium, the barium titanate particle powder can be uniformly and finely dispersed in the dispersion medium, and the dispersion stability can also be improved.
[0145] The dispersant may be directly added to the dispersion medium, or may be pre-processed into barium titanate particle powder.
[0146] Example
[0147] Specific examples of the present invention will be described below, but the present invention is not limited to these examples.
[0148] The barium titanate particle powder of the present invention was evaluated as follows.
[0149] In order to observe the surface, shape and primary particles of the sample, SEM "S-4300" [manufactured by Hitachi High-Technologies Corporation] was used.
[0150] 500 primary particles in the obtained image were measured using image analysis type particle size distribution measurement software "Mac-View" [manufactured by Mountech Co., Ltd.], and the average primary particle diameter was calculated from the number average of the primary particle diameters.
[0151] The Ba / Ti composition ratio was measured using an X-ray fluorescence analyzer "Simultix12" (manufactured by Rigaku Corporation).
[0152] The BET specific surface area was measured by a fully automatic specific surface area measuring apparatus "Macsorb HM model-1208" (manufactured by Mountech Co., Ltd.) after drying and degassing at 250°C for 10 minutes under nitrogen.
[0153] The particle size of the aggregated particles in the aqueous solvent was measured using a particle size distribution analyzer "Microtrac MT3300EXII" [manufactured by Microtrac BEL Co., Ltd.] using a laser diffraction / scattering method or a particle size distribution analyzer "FPAR-1000" [manufactured by Otsuka Electronics Co., Ltd.] using a dynamic light scattering method. 2 In the case of 1.5 g / cm2, the latter dynamic light scattering method was used for analysis in the CONTIN mode.
[0154] The sample was dispersed in 20 mL of a 0.2 wt% aqueous solution of sodium hexametaphosphate dispersant by ultrasonication for 5 minutes, and then diluted with pure water to measure the particle size distribution of the aggregated particle size. 2 In the sample with a particle size of 1000 Å / g, when the dry aggregation between the particles was strong, a slurry containing the barium titanate particle powder before removing the water used in the solution reaction was used as a sample.
[0155] Based on the cumulative frequency distribution of the obtained particle size distribution, the 50% diameter D 50 and 95% diameter D 95 D 95 / D 50 The value of .
[0156] In order to identify the crystal phase of the sample and calculate the crystal structure parameters, the measurement was performed using a powder X-ray diffraction apparatus "SmartLab" (Rigaku Corporation).
[0157] The X-ray diffraction pattern was measured by a monochromator under the conditions of Cu—Kα, 40 kV, and 200 mA, and was measured at 15≤2θ(deg.)≤90, in a step of 0.02°, and at 3 deg. / min.
[0158] In order to calculate crystal parameters such as lattice constants, analysis was performed using the Rietveld method. The tetragonality, which indicates the crystallinity of barium titanate particles, is represented by the lattice constant ratio c / a.
[0159] In order to quantify the amount of impurities in the sample, an internal standard method was used in a high-frequency inductively coupled plasma optical emission spectrometer (ICP-OES) "Optima 8300" [PerkinElmer Japan Co., Ltd.].
[0160] When the impurity elements Si, S, Cl, Ca, Fe, and Sr measured by ICP-OES are 200 ppm or less, or the impurity alkali metal elements Na and K are 20 ppm or less, the evaluation is ○.
[0161] The oil absorption of the sample was measured using "S410D" (manufactured by ASAHI CO., LTD.).
[0162] 15 g of the sample was weighed and placed in a twin-screw kneader, which was rotated at a fixed speed of 200 rpm (angular velocity = 20.94 rad / s), and then dibutyl phthalate (DBP), an oil component, was added dropwise at a fixed speed of 1 mL / min.
[0163] The horizontal axis represents the amount of DBP added, and the vertical axis represents the moment during kneading, thereby obtaining the oil absorption characteristics.
[0164] The obtained oil absorption characteristics were fitted with five or less Gaussian functions to calculate the maximum torque, the oil absorption at the maximum torque, and the area of the oil absorption characteristics. In the oil absorption characteristics, the fitting was performed with the start of DBP drop addition as the starting point and the point where the torque value reached 0 [Nm] as the end point.
[0165] The product of the torque [Nm] and the angular velocity [rad / s] on the vertical axis is the power [J / s], and the DBP drop volume [mL] on the horizontal axis can be converted into time [s] by the drop speed of 1 mL / min.
[0166] Therefore, the work [J / g] of the twin-screw kneader per 1g of sample can be calculated from the area of the oil absorption characteristic.
[0167] In the present invention, the smaller the work [J / g] of the twin-screw kneader, the easier it is to dispersibly obtain the product in the non-aqueous solvent.
[0168] With reference to JIS K 6217-4, the oil absorption characteristics of carbon black SRB D-6 as a standard substance were evaluated by "S410D".
[0169] The sample weight was set to 8.0 g, the rotation speed of the kneader was set to 200 rpm, and the dropping speed was set to 1 mL / min.
[0170] The maximum torque is 0.953Nm, and the oil absorption at the maximum torque is 71.0mL / 100g.
[0171] In addition, the oil absorption at 70% torque was 66.7 mL / 100 g.
[0172] The oil absorption characteristics of the twelve types of carbon black of JIS Z 8901 test powder 1 were evaluated by "S410D".
[0173] The sample weight was set to 7.5 g, the rotation speed of the kneader was set to 200 rpm, and the dropping speed was set to 1 mL / min.
[0174] The maximum torque is 0.856Nm, and the oil absorption at the maximum torque is 33.3mL / 100g.
[0175] In addition, the oil absorption at 70% torque was 32.1 mL / 100 g, and the work done by the twin-screw kneader was 14.8 J / g.
[0176] The sample weight was set to 7.5 g, the rotation speed of the kneader was set to 125 rpm, and the dropping speed was set to 1 mL / min.
[0177] The maximum torque is 0.896Nm, and the oil absorption at the maximum torque is 33.6mL / 100g.
[0178] In addition, the oil absorption at 70% torque was 32.4 mL / 100 g, and the work done by the twin-screw kneader was 15.1 J / g.
[0179] The ignition loss of the samples was measured at 1200°C for 2 hours.
[0180] Measure 10g of sample and calculate its reduction value.
[0181] The moisture content of the cake obtained by dehydrating the slurry containing mixed titanic acid was calculated by drying 5 g of the cake at 50° C. for 12 hours and calculating the weight loss.
[0182] In addition, the ignition loss of the mixed titanic acid cake was calculated by the loss value due to heat treatment at 700°C for 2 hours.
[0183] The ignition loss of the mixed titanic acid cake was set as the amount of water obtained by dehydration of the water content determined and nH2O of the mixed titanic acid TiO2·nH2O, and the value of n was calculated.
[0184] Evaluation of the common material of the Ni internal electrode layer of the sample MLCC was performed as follows with the assistance of ECL.
[0185] As Ni particles, 0.2 μm-size "NFP-201S" (manufactured by JFE MINERAL CORPORATION) was used.
[0186] Ni paste was prepared by adding a dispersant and EC paint to DHTA solvent with 100 parts by weight of Ni and 20 parts by weight of the sample.
[0187] Here, at 30m 2 In the case of a fine particle sample having a particle size of 100 μm / g or more, a dispersant was added to an ethanol solvent, and the sample was pre-dispersed with 2 mmφ ZrO2 microbeads to generate a dispersion containing barium titanate particle powder.
[0188] As described above, the obtained dispersion was added so that the sample amount was 20 parts by weight to prepare a Ni paste.
[0189] The viscosity of the obtained Ni paste was measured under “conditions: 10 rpm, B-type viscometer “DV-2” (manufactured by Brookfield)”.
[0190] The obtained Ni paste was formed into a film by a doctor blade method to obtain a Ni dry film having a film thickness of about 40 μm.
[0191] The density of the Ni dry film was calculated by shape measurement and weight determination.
[0192] As the surface roughness of the Ni dry film, SURFCOM (manufactured by Tokyo Seimitsu Co., Ltd.) was used.
[0193] A disk of about 14 mm in diameter was produced from the Ni dry film, and the heat shrinkage rate of the disk diameter at 600°C to 1200°C was measured.
[0194] [Example 1]
[0195] Industrial titanium chloride (Ti concentration 16.5 wt %, Cl concentration 31 wt %) was used as the main raw material and diluted with water to prepare a titanium chloride solution.
[0196] For the solution reaction, an approximately 15 L titanium container was used.
[0197] As the barium compound of the main raw material, barium hydroxide octahydrate salt (manufactured by Kanto Chemical Co., Ltd., 97% Ba(OH)2·8H2O reagent special grade) was used. As the neutralizing agent, industrial NaOH was used.
[0198] Barium hydroxide octahydrate salt is dissolved in warm water, and barium carbonate is removed by a filter to use as a barium hydroxide solution.
[0199] Titanium chloride was metered so that Ti became 5 mol.
[0200] NaOH was metered so that NaOH / Cl=1.02.
[0201] In the first step, 4 L of the titanium chloride solution diluted with water was neutralized by adding 4 L of NaOH dropwise over 1 hour at a temperature not exceeding 60° C. in an air atmosphere.
[0202] After obtaining 8 L of orthotitanic acid slurry without hydrolyzing titanium chloride, a part of the orthotitanic acid was subjected to a dehydration reaction at 80° C. in the air for 1 hour.
[0203] The Ti concentration at this time was 0.625 mol / L.
[0204] The mixture is then cooled to obtain a mixed titanic acid slurry containing orthotitanic acid and metatitanic acid.
[0205] The obtained slurry was filtered and washed to remove impurity elements such as Na and Cl from the mixed titanic acid. Then, 5 g of the cake of the mixed titanic acid was taken and dried at 50°C to quantify the impurity elements and n of the mixed titanic acid TiO2·nH2O.
[0206] In addition, from the X-ray diffraction pattern of the dried sample, mixed titanic acid of metatitanic acid in an anatase crystal phase and orthotitanic acid having a broad peak and low crystallinity was confirmed.
[0207] The obtained mixed titanate TiO2·nH2O has an n of 1.2 and a maximum impurity element of Na, 410 ppm. The remaining mixed titanate cake is debonded to prepare a mixed titanate slurry.
[0208] In the second step, the mixed titanate slurry maintained at 80° C. and the barium hydroxide solution were mixed at a mol ratio of Ba / Ti=1.5 in a high-purity nitrogen atmosphere, and the solution was reacted at 80° C. for 3 hours to obtain a barium titanate slurry.
[0209] The concentration of Ti was 0.5 mol / L, and the reaction solution was 10 L.
[0210] The barium titanate-containing slurry was cooled, concentrated by sedimentation to 2 times, and 5 L of the slurry was hydrothermally treated at 170° C. for 8 hours.
[0211] The barium titanate particle powder of the present invention is obtained through filtration, water washing, cake drying / crushing.
[0212] Figure 1 : The SEM image obtained in Example 1 is shown in FIG.
[0213] according to Figure 1 The particle size distribution of primary particles was measured by SEM images, and the average primary particle size was calculated.
[0214] The particle size distribution of the aggregated particles in the aqueous solvent obtained by the laser diffraction / scattering method is also plotted and shown in FIG. Figure 2 .
[0215] The average primary particle size of the barium titanate particle powder in Example 1 was 83 nm, and the D 10 86.3nm, D 50 141.6nm, D95 It is 262.2nm.
[0216] The obtained D 95 / D 50 The value of was 1.9, which was evaluated as being easily dispersible in an aqueous solvent.
[0217] The Ba / Ti composition ratio obtained by fluorescent X-ray was 0.996 and the BET specific surface area was 14.2 m 2 / g, the crystallite size obtained by powder X-ray diffraction method was 85 nm, the lattice constant ratio c / a was 1.0058, the tetragonal degree was high, and the crystallinity was high.
[0218] According to ICP-OES, the impurity elements Si, S, Cl, Ca, Fe, and Sr derived from the main raw material were less than 200 ppm, and the alkali metal elements Na and K derived from the impurities of the neutralizer were less than 20 ppm, so it can be confirmed that it is high in purity.
[0219] The loss on ignition was 1.2 wt %, and thus it was confirmed that the sample had high crystallinity.
[0220] The oil absorption characteristics of the sample 15 g in the measurement are shown with the DBP oil absorption on the horizontal axis and the moment on the vertical axis. Figure 3 .
[0221] The fitting is performed using an approximate curve of the sum of five Gaussian functions f1 to f5.
[0222] The sum of the squares of the residuals between the measured data and the approximate curve is 0.0011, which enables high-precision fitting.
[0223] The maximum torque of the obtained oil absorption characteristics was 0.162 N·m, the oil absorption at the maximum torque was 28.3 mL / 100 g, and the work done by the twin-screw kneader was 26.7 J / g.
[0224] The barium titanate particle powder of Example 1 had a low maximum torque and a small oil absorption in terms of oil absorption characteristics, and the work of the twin-screw kneader was small, so it was evaluated to be easily dispersible in a non-aqueous solvent.
[0225] [Example 2]
[0226] The hydrothermal treatment was carried out under the same conditions as in Example 1 except that the hydrothermal treatment temperature was changed from 170°C to 130°C.
[0227] The obtained average primary particle size was 62 nm. In terms of oil absorption characteristics, the maximum torque was low, the oil absorption was also small, and the work of the twin-screw kneading machine was small, so it was evaluated to be easily dispersible in a non-aqueous solvent.
[0228] [Examples 3 to 5]
[0229] Examples 3 to 5 were carried out with the dehydration reaction temperature in the first step being 85°C.
[0230] In Example 3, the hydrothermal treatment temperature is set to 175°C.
[0231] Example 4 The hydrothermal treatment temperature was set to 175°C. After washing with water, the obtained slurry was evaporated to dryness and pulverized.
[0232] In Example 5, the hydrothermal treatment temperature was set to 125° C. The conditions not described above were the same as those in Example 1.
[0233] In terms of oil absorption characteristics, all barium titanate particle powders had low maximum torque, small oil absorption, and small work of the twin-screw kneading machine, and were therefore evaluated to be easily dispersible in a non-aqueous solvent.
[0234] [Example 6]
[0235] The dehydration reaction temperature in the first step was set to 70° C., the Ba / Ti ratio in the second step was set to 1.3 mol ratio, the Ti concentration was set to 0.59 mol / L, and the reaction solution was set to 9 L.
[0236] The hydrothermal treatment was performed at 105° C. for 3 hours, and the other synthesis conditions were the same as those in Example 1.
[0237] The obtained barium titanate particle powder had an average primary particle size of 35 nm. Since it was fine particles, the oil absorption in the oil absorption characteristics was small, the maximum torque was low, and the work of the twin-screw kneading machine was small, so it was evaluated to be easily dispersible in a non-aqueous solvent.
[0238] [Example 7]
[0239] Half the amount of the mixed titanic acid obtained in the first step of Example 6, i.e. 2.5 mol, is mixed in a slurry state with 2.5 mol of metatitanic acid obtained by hydrolysis of titanium chloride according to (Formula C) at pH 2 and temperature 60°C to obtain a total of 5 mol of mixed titanic acid (n=0.8) slurry.
[0240] In the second step, the Ti concentration was 0.59 mol / L and the reaction solution was 9 L.
[0241] After the solution reacted, it was concentrated to 1.75 times and subjected to hydrothermal treatment.
[0242] The other synthesis conditions were the same as those in Example 6.
[0243] The obtained barium titanate particles had an average primary particle size of 28 nm. In terms of oil absorption characteristics, the maximum torque was low, the oil absorption was small, and the work of the twin-screw kneader was small, so it was evaluated that the particles were easily dispersible in a non-aqueous solvent.
[0244] [Example 8]
[0245] Half the amount of the mixed titanic acid obtained in the first step of Example 6, i.e. 1 mol, is mixed in a slurry state with 4 mol of metatitanic acid obtained by hydrolysis of titanium chloride according to (Formula C) at pH 2 and temperature 60°C to obtain a total of 5 mol of mixed titanic acid (n=0.6) slurry.
[0246] The second step and the subsequent steps are the same as those in Example 7.
[0247] The obtained barium titanate particles had an average primary particle size of 27 nm. In terms of oil absorption characteristics, the maximum torque was low, the oil absorption was small, and the work of the twin-screw kneader was small, so it was evaluated that the particles were easily dispersible in a non-aqueous solvent.
[0248] The low ignition loss of 2.3 and high crystallinity are considered to be due to the low n value of 0.6 of the mixed titanic acid used.
[0249] [Example 9]
[0250] The mixed titanic acid (n=0.8) slurry obtained in the first step of Example 7 was used.
[0251] In the second step, the concentration of Ti was 0.625 mol / L, and the reaction solution was 8 L.
[0252] After the solution reaction, the solution was washed with water and concentrated to obtain 4 L of slurry with an electrical conductivity of 25 mS / cm, and then subjected to hydrothermal treatment. Other synthesis conditions were the same as those in Example 6.
[0253] The obtained barium titanate particles had an average primary particle size of 25 nm. In terms of oil absorption characteristics, the maximum torque was low, the oil absorption was small, and the work of the twin-screw kneader was small, so it was evaluated that the particles were easily dispersible in a non-aqueous solvent.
[0254] [Example 10]
[0255] The hydrothermal treatment temperature in the second step was set to 85° C., and the other synthesis conditions were the same as those in Example 9.
[0256] The obtained barium titanate particles had an average primary particle size of 20 nm. In terms of oil absorption characteristics, the maximum torque was low, the oil absorption was small, and the work of the twin-screw kneader was small, so it was evaluated that the particles were easily dispersible in a non-aqueous solvent.
[0257] [Comparative Example 1]
[0258] Referring to Example 1 of Japanese Patent No. 5765505, titanic acid was prepared as follows according to (Formula C).
[0259] Wherein, the main raw material, neutralizing agent and other experimental apparatuses are in accordance with Example 1 of the present invention.
[0260] In the reaction container, 4.8 L of pure water was maintained at 60° C., and 2.4 L of a titanium chloride solution (Ti: 5.63 mol) and 2.4 L of a neutralizing agent NaOH (NaOH / Cl=1.0 mol ratio) were simultaneously added dropwise while being exposed to the atmosphere.
[0261] The reaction solution in the reaction container was always maintained at pH = 1.7-2.3 and a temperature of 60°C, and the titanium chloride solution and NaOH were added dropwise at a constant rate over 2 hours.
[0262] The Ti concentration after the dropwise addition was completed was 0.6 mol / L.
[0263] The obtained slurry was washed with water, and 1 / 6 of the obtained cake was dried at 120°C and evaluated.
[0264] The obtained dried cake was measured by powder X-ray diffraction method and was confirmed to be anatase-type titanium oxide, which was metatitanic acid.
[0265] When represented by TiO2·nH2O, n is less than 0.5. That is, it is not a mixed titanic acid of orthotitanic acid and metatitanic acid in the present invention.
[0266] The impurity Na in the dried cake obtained was 500 ppm or less, indicating high purity, so the second step was carried out as follows.
[0267] The remaining 5 / 6 of the cake was hydrolyzed with pure water, placed in a nitrogen atmosphere, heated to 85°C, and then mixed with a barium hydroxide solution maintained at 85°C. At this time, the Ba / Ti ratio was 1.5 mol, and the Ti concentration was 0.5 mol / L. Under a nitrogen atmosphere, a barium titanate slurry was obtained at 85°C for 3 hours. After sedimentation and concentration to twice the obtained slurry, a hydrothermal treatment was performed at 170°C for 8 hours.
[0268] The same operation as in Example 1 was carried out, and barium titanate particle powder was obtained through filtration, water washing, cake drying and pulverization.
[0269] The average primary particle size of the obtained barium titanate particle powder was 101 nm. 95 / D 50 Since the value of was 1.9, it was evaluated that the dispersion was easily dispersible in an aqueous solvent.
[0270] However, in the oil absorption characteristics, the maximum torque is high, the oil absorption is also large, and the work done by the twin-screw mixer is large, so it is difficult to determine that it is easy to dispersible in non-aqueous solvents.
[0271] [Comparative Example 2]
[0272] The hydrothermal treatment was carried out under the same conditions as in Comparative Example 1 except that the hydrothermal treatment temperature was changed from 170°C to 130°C.
[0273] The obtained barium titanate particle powder had a high maximum torque and a large oil absorption, which were characteristics of large work done by the twin-screw kneader, and it was difficult to determine that it was easily dispersible in a non-aqueous solvent.
[0274] [Comparative Example 3]
[0275] Barium titanate particle powder was prepared with reference to Example 6 of Japanese Patent Application Laid-Open No. 2005-289668, wherein the main raw material, neutralizing agent and other experimental equipment were the same as those of Example 1 of the present invention.
[0276] The Ti concentration is 0.5 mol / L and the reaction solution is 10 L. The titanium chloride solution is neutralized with a barium hydroxide solution at Ba / Ti=1.5 to obtain orthotitanic acid. After that, it is mixed with a barium hydroxide solution at Ba / Ti=1.5 and reacted at 70°C for 2 hours. The slurry, which has been concentrated to 2 times by precipitation, is hydrothermally treated at 200°C for 8 hours, washed with water, dried and crushed. The average primary particle size of the obtained barium titanate particle powder is 96 nm, D 95 / D 50 Since the value of was as low as 2.0, it was evaluated that the dispersion was easily dispersible in an aqueous solvent.
[0277] However, in the oil absorption characteristics, the maximum torque is high and the oil absorption is large, which is a characteristic of the large work of the twin-screw kneading machine. Therefore, it is difficult to determine that it is easy to dispersible in non-aqueous solvents.
[0278] [Comparative Examples 4 and 5]
[0279] Barium titanate particle powder was prepared with reference to Example 1 of Japanese Patent Application Laid-Open No. 2005-289668. Specifically, barium hydroxide and metatitanic acid were used as main raw materials, and the hydrothermal treatment temperature was 190°C in Comparative Example 4 and 170°C in Comparative Example 5.
[0280] The obtained barium titanate particle powder has a high maximum torque and a large oil absorption in terms of oil absorption characteristics, which is a characteristic of large work done by the twin-screw kneader. Therefore, it is difficult to determine that the powder is easily dispersible in a non-aqueous solvent.
[0281] [Comparative Examples 6 and 7]
[0282] Comparative Example 6 was carried out under the same conditions as Comparative Example 3 except that the hydrothermal treatment temperature was changed from 200°C to 105°C. Comparative Example 7 was obtained by washing (the filtrate conductivity was 1 mS / cm as the end point) and drying without performing the hydrothermal treatment in Comparative Example 3.
[0283] D of Comparative Example 795 / D 50 The value is as high as 18.3, which makes it difficult to determine that it is easily dispersible in aqueous solvents.
[0284] The barium titanate particle powders of Comparative Examples 6 and 7 have a large oil absorption, which is a characteristic of large work done by the twin-screw kneading machine, and it is difficult to confirm that they are easily dispersible in a non-aqueous solvent.
[0285] Table 1 shows the synthesis conditions, and Table 2 shows the evaluation results.
[0286] The relationship between oil absorption and average primary particle size is shown in Figure 4 The straight line that distinguishes the Examples from the Comparative Examples, i.e., the oil absorption at the maximum moment = (36 - 0.08 x average primary particle size) mL / 100 g, is indicated by a dotted line.
[0287] It can be seen that the example is located below the dotted line, and the comparative example is located above the dotted line.
[0288] [Table 1]
[0289]
[0290] [Table 2]
[0291]
[0292] When the oil absorption was (36-0.08×average primary particle size) mL / 100 g or less, it was set to 0, and when it exceeded it, it was set to ×.
[0293] When the impurity elements Si, S, Cl, Ca, Fe, and Sr are 200 ppm or less, or the impurity alkali metal elements Na and K are 20 ppm or less, they are recorded as 0.
[0294] [Evaluation of Ni as a common material for internal electrode layers of MLCC]
[0295] The barium titanate particle powders obtained in Example 1, Example 2, and Comparative Example 3 were evaluated as a common material for the Ni internal electrode layer.
[0296] The results are shown in Table 3.
[0297] [Table 3]
[0298]
[0299] The viscosity of the Ni pastes of Examples 1 and 2 was reduced by about 10% compared to the viscosity of the Ni paste of Comparative Example 3. It is estimated that the common material of the easily dispersible barium titanate particle powder according to the present invention reduced the viscosity of the Ni paste.
[0300] The density of the Ni dry film is 5.1 g / cc, but the surface roughness of the Ni dry film of Examples 1 and 2 is about 10% lower than that of the Ni dry film of Comparative Example 3. It is speculated that the common material of the easily dispersible barium titanate particle powder involved in the present invention improves the dispersibility of Ni.
[0301] The thermal shrinkage rate of the disk diameter of the Ni dry films of Examples 1 and 2 showed a low value of about 2% to 3% from a low temperature of 600°C to a high temperature of 800°C, and the thermal shrinkage of Ni during sintering was suppressed.
[0302] Furthermore, even when fired at 1200°C, Examples 1 and 2 have lower thermal shrinkage than Comparative Example 3 and are superior in thermal shrinkage characteristics. This is presumably because the common material of the easily dispersible barium titanate particle powder according to the present invention is uniformly dispersed by the Ni particles.
[0303] The same 39m 2 The sample with a mass of 1000 μm and a mass of 2000 μm was evaluated as a common material for the Ni electrode.
[0304] A dispersion containing barium titanate particle powder was obtained by pre-dispersion. In order to evaluate the dispersion state of the sample in the dispersion, a coating film was formed and the surface roughness was measured.
[0305] The surface roughness of the coating films of the dispersions of Example 7 and Comparative Example 6 were 0.012 μm and 0.014 μm, respectively. The dispersion state of the samples of the dispersions prepared under the same conditions was different from that of Comparative Example 6.
[0306] Example 7 is better.
[0307] Using the obtained dispersions of Example 7 and Comparative Example 6, Ni pastes were prepared.
[0308] Compared with Comparative Example 6, the paste viscosity of Example 7 is slightly higher, but the density of the dried film is high and the surface roughness is low (Table 3). This is because the Ni particles and common materials of Example 7 are fully dispersed with each other compared with Comparative Example 6. The difference in dispersion state can also be confirmed in the SEM observation of the dried film. From the temperature dependence of the diameter heat shrinkage rate of the circular plate recorded in Table 3, it can be seen that compared with Comparative Example 6, the heat shrinkage of Example 7 is suppressed and the heat shrinkage characteristics are excellent.
[0309] Comparison between the examples and the comparative examples shows that, when the barium titanate particle powder according to the present invention is used as a common material for the Ni internal electrode layer of an MLCC, an MLCC having high mechanical strength can be obtained.
[0310] These results are presumably because, in the barium titanate particle powder according to the present invention, the unreacted product of barium and titanium is extremely small, and thus the crystallinity of the surface of the particle is further increased.
[0311] Industrial Applicability
[0312] The barium titanate particle powder involved in the present invention is fine, with an average primary particle size of 20nm to 150nm, and the particle size distribution of the agglomerated particle size in the aqueous solvent is narrow, so it is easily dispersible in the aqueous solvent. At the same time, the torque of the oil absorption characteristic is low, so it is also easily dispersible in the non-aqueous solvent.
[0313] In addition, since the ignition loss is low and the crystallinity is high, the barium titanate particle powder can be suitably used as a particle growth inhibitor during sintering of the Ni internal electrode layer of MLCC, a raw material for high-capacitance capacitors, or high-transmittance optical films.
[0314] Therefore, the present invention has high industrial applicability.
Claims
1. A barium titanate particle powder, wherein the average primary particle size is 20 nm or more and 150 nm or less, and the 50% diameter D of the cumulative frequency distribution of aggregated particles in an aqueous solvent is 50 and 95% diameter D 95 D 95 / D 50 The value of is 5 or less, and the maximum torque of the oil absorption characteristic is 0.2 N·m or less.
2. The barium titanate particle powder according to claim 1, wherein The work done by the twin-screw kneader in the oil absorption characteristics is 40 J / g or less.
3. The barium titanate particle powder according to claim 1 or 2, wherein The loss on ignition is 4.0 wt% or less.
4. A method for producing barium titanate particle powder, wherein: At least: In the first step, a mixed titanic acid of orthotitanic acid and metatitanic acid is produced by a solution reaction in an aqueous solvent; as well as In the second step, a barium compound is mixed at a temperature of 60° C. to 105° C. to generate barium titanate.
5. The method for producing barium titanate particle powder according to claim 4, wherein: The first step is a step of subjecting orthotitanic acid generated from titanium chloride and a neutralizing agent to a dehydration reaction at 50° C. to 85° C. to generate a mixed titanic acid of orthotitanic acid and metatitanic acid.
6. The method for producing barium titanate particle powder according to claim 4, wherein: The impurity elements contained in the mixed titanic acid in the first step are each 1000 ppm or less.
7. The method for producing barium titanate particle powder according to claim 4, wherein: When the mixed titanic acid is represented by TiO 2 ·nH 2 O, n of the mixed titanic acid in the first step is 0.5 ≤ n ≤ 1.
5.
8. A barium titanate particle powder, wherein the average primary particle size is 20 nm or more and 150 nm or less, and the 50% diameter D of the cumulative frequency distribution of agglomerated particles in an aqueous solvent is 50 and 95% diameter D 95 D 95 / D 50 The value of is 5 or less, and the oil absorption at the maximum moment of the oil absorption characteristic is (36-0.08×average primary particle size) mL / 100 g or less.