Glass article manufacturing method and glass article

By cutting with non-pulse-sequence pulse oscillation laser along the imaginary line on the glass base material, the modified part is formed and broken, which solves the problem of cracks on the fracture surface during pulse-sequence cutting, and achieves high-quality glass cutting.

CN119095806APending Publication Date: 2024-12-06AGC INC
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202380036455.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-26
Filing Date
2023-04-21
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

In the prior art, when cutting glass using pulse train, cracks are easily generated on the fracture surface, resulting in poor quality of glass items.

Method used

By setting the imaginary line along the main surface of the base material, a plurality of modified parts are formed using a pulse oscillation laser in a non-pulse-spin-spin-type, and the base material is broken with these modified parts as the starting point. The pulse width of the laser is set to 15 ps or more And below 100 ps, ​​the relationship between the control pulse interval and width is P≦0.25×LB+3.5 to reduce cracks on the fracture surface.

Benefits of technology

The glass items are properly cut off and cracks on the fracture surface are significantly suppressed, the quality of the glass items is improved, and the surface roughness is ensured below 0.6 μm specified in ISO25178.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119095806A_ABST
    Figure CN119095806A_ABST
Patent Text Reader

Abstract

Provided is a glass article that is appropriately cut and that suppresses the occurrence of cracks in a fracture surface. The method for manufacturing a glass article includes: forming a plurality of modified portions (H) on a base material (10) along an imaginary line (T) set on a main surface (10A) of the base material (10) by irradiating the base material (10) with pulsed oscillation laser light along the imaginary line (T); and obtaining a glass article by cutting a portion from the base material (10) by breaking the base material (10) with the modified portion (H) along the imaginary line (T) as a starting point. The minimum pulse interval of the laser light is greater than 1 [mu] s, and the pulse width of the laser light is from 15 ps to 100 ps (inclusive).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for manufacturing a glass article and a glass article. Background Art

[0002] It is known that a method of cutting a glass article from a glass base material is performed by irradiating a base material with laser light to form a plurality of modified portions, and then breaking the base material along the plurality of modified portions. For example, Patent Document 1 describes the method of breaking a glass plate by perforating the glass plate with a laser in a pulse train method. The pulse train method refers to a method of outputting a pulse group having a plurality of pulse lights, called a pulse train, at a predetermined period. By using the pulse train method, a glass plate can be perforated appropriately.

[0003] Patent Document 1: Japanese Patent No. 6552503

[0004] However, for example, when a pulse train method is used, since pulse light is irradiated multiple times to a relatively close part, the fracture surface along the fracture of the modified part is exposed to multiple shock waves, and cracks may be generated on the fracture surface. Therefore, it is required to provide a glass article that can be properly cut and suppresses the generation of cracks on the fracture surface. Summary of the invention

[0005] The present invention has been made in view of the above-mentioned problems, and an object of the present invention is to provide a method for producing a glass article which is appropriately cut and in which cracks are suppressed from occurring on the fracture surface, and a glass article.

[0006] The manufacturing method of the glass article involved in the present disclosure includes: irradiating a pulsed laser along an imaginary line set on the main surface of the base material to form a plurality of modified portions along the imaginary line on the base material; and cutting out a portion from the base material by breaking the base material with the modified portion along the imaginary line as a starting point, wherein the minimum pulse interval of the laser is greater than 1μs, and the pulse width of the laser is greater than 15ps and less than 100ps.

[0007] The glass article involved in the present disclosure is a glass article having a main surface and an end surface, wherein a plurality of linear modified portions extending in the thickness direction of the glass article are formed on the end surface, and the surface roughness Sa of the end surface specified in ISO25178 is 0.6 μm or less.

[0008] According to the present invention, it is possible to provide a glass article which is appropriately cut and in which cracks are suppressed from occurring on the fracture surface. BRIEF DESCRIPTION OF THE DRAWINGS

[0009] Figure 1 It is a schematic cross-sectional view of the base material.

[0010] Figure 2This is a schematic diagram showing an example of an output waveform of a pulse train laser.

[0011] Figure 3 It is a schematic diagram showing an example of the output waveform of the laser light according to the present embodiment.

[0012] Figure 4 It is a schematic diagram for explaining the formation of the modified part.

[0013] Figure 5 It is a schematic diagram for explaining the formation of the modified part.

[0014] Figure 6 It is a schematic diagram for explaining the formation of the modified part.

[0015] Figure 7 It is a schematic diagram of a glass object.

[0016] Figure 8 It is a schematic diagram showing the end surface of a glass object.

[0017] Fig. 9 This is a schematic diagram showing an example of an end surface after chamfering.

[0018] Fig.10 It is a schematic diagram showing the vehicle-mounted display according to the present embodiment.

[0019] Fig.11 This is a schematic diagram for explaining the cutting out of a base material in the example.

[0020] Fig.12 This is a graph showing the correlation between the pulse width and the pitch in the non-pulse train method of Experiment 3. DETAILED DESCRIPTION

[0021] Hereinafter, the preferred embodiment of the present invention will be described in detail with reference to the accompanying drawings. In addition, the present invention is not limited to the embodiment, and in the case where there are multiple embodiments, an embodiment composed of a combination of the embodiments is also included. In addition, for numerical values, the range of rounding is included.

[0022] Furthermore, in this specification, "mass" and "weight" are synonymous.

[0023] In this embodiment, the base material 10 is irradiated with laser light L to form a modified portion H in the base material 10, and the base material 10 is fractured starting from the modified portion H, thereby cutting out the glass article 100 from the base material 10. The base material 10, a method for manufacturing the glass article 100 from the base material 10, and the glass article 100 are described below.

[0024] (Base Material)

[0025] Figure 1 is a schematic cross-sectional view of the parent material. Figure 1 As shown, the base material 10 is a transparent plate-like component. In addition, the plate-like shape here is not limited to a flat plate shape, and can refer to a shape in which the width of the main surface is longer than the thickness. The transparency here can refer to the transmission of visible light. In the following, the main surface of one side of the base material 10 is set as the main surface 10A, the main surface on the opposite side of the main surface 10A is set as the main surface 10B, and the thickness direction of the base material 10, that is, the direction connecting the main surface 10B and the main surface 10A is set as the Z direction. In addition, in the Z direction, the direction from the main surface 10B to the main surface 10A is set as the direction Z1, and the direction from the main surface 10B to the main surface 10A is set as the direction Z2. Figure 1 In the example, the base material 10 is a rectangular flat plate when viewed from the Z direction, but the shape of the base material 10 can be arbitrary. For example, the base material 10 is not limited to being a rectangle when viewed from the Z direction, and can also be a polygon, a circle, or an ellipse. Figure 1 In the example, the base material 10 is in the shape of a flat plate, but it is not limited to this, and it can also be a shape formed by bending a flat plate. That is, the base material 10 can also be a curved surface with the main surfaces 10A and 10B convex in the Z direction. In the case where the main surfaces 10A and 10B of the base material 10 are curved surfaces convex in the Z direction, the radius of curvature of the main surfaces 10A and 10B of the base material 10 is preferably less than 10000 mm, more preferably less than 5000 mm, and further preferably less than 3000 mm. In the case where the main surfaces 10A and 10B of the base material 10 are curved surfaces convex in the Z direction, the radius of curvature of the main surfaces 10A and 10B of the base material 10 is preferably greater than 10 mm, more preferably greater than 50 mm, further preferably greater than 100 mm, and particularly preferably greater than 200 mm. That is, the radius of curvature of the main surfaces 10A and 10B of the base material 10 is preferably in the range of 10 to 10000 mm.

[0026] The thickness DA of the base material 10 is preferably 0.1 mm or more, more preferably 0.7 mm or more, and further preferably 1.1 mm or more. In addition, the thickness DA of the base material 10 is preferably 0.7 mm or more and 5 mm or less, and more preferably 1.1 mm or more and 3 mm or less. According to the manufacturing method of this embodiment, such a relatively thick base material 10 can be properly cut, and cracks on the fracture surface can be suppressed. In addition, the thickness DA of the base material 10 refers to the length in the Z direction from the main surface 10A to the main surface 10B.

[0027] Fracture toughness value K of base material 10 IC Preferably 0.6 (MPa·m 0.5 ) or more, more preferably 0.6 (MPa·m 0.5 ) and above 1.00(MPa·m 0.5) or less, more preferably 0.65 (MPa·m 0.5 ) and above 0.70(MPa·m 0.5 ) or less. For the fracture toughness value K IC 0.6 (MPa·m 0.5 ) or more, it is difficult to cut using conventional methods, but according to the present manufacturing method, the fracture toughness value K IC The base material 10 within this range is properly cut and cracks on the fracture surface are suppressed. IC For example, it can be measured according to the Double Cleavage Drilled Compression (DCDC) method described in the non-patent document (NEW GLASS Vol. 15 No. 2 2000 p18).

[0028] The base material 10 is preferably glass, and more preferably alkali glass containing an alkali metal component. The base material 10 is the same material as the glass article 100 described later. On the other hand, as described later, the base material 10 is preferably glass before chemical strengthening, and the glass article 100 is preferably glass after chemical strengthening. However, as described later, in the case where the glass article 100 is chemically strengthened, the composition of the base material 10 is equivalent to the composition of the central part of the glass article 100 in the plate thickness direction. Specifically, if the element released by substitution during chemical strengthening is regarded as the pre-substitution element, and the element obtained by substitution through chemical strengthening is regarded as the substitution element, it can be said that the glass article 100 has a composition containing the pre-substitution element instead of the substitution element relative to the chemically strengthened surface layer of the glass article 100.

[0029] (Method for manufacturing glass article)

[0030] Next, a method for manufacturing the glass article 100 from the base material 10 will be described. Figure 1 As shown, in the present manufacturing method, laser L is irradiated from an irradiation device A onto the main surface 10A of the base material 10, and a modified portion H is formed in the base material 10. The modified portion H is a layer whose density or refractive index has changed by structural changes of the glass, or by melting and resolidification of the glass. The modified portion H may also include voids. In addition, the laser L forms the modified portion H, for example, by nonlinear absorption. Nonlinear absorption is also called multiphoton absorption. The probability of multiphoton absorption is nonlinear with respect to the photon density (power density of the laser L), and the higher the photon density, the more significantly the probability increases. For example, the probability of two-photon absorption is proportional to the square of the photon density.

[0031] In addition, a portion having at least one of a density, a refractive index, an asymmetric electron density, and a fictive temperature different from a portion of the base material 10 where the modified portion H is not formed (a portion not irradiated with the laser light L) may be regarded as the modified portion H. In addition, the portion where the modified portion H is not formed may refer to, for example, a position that is at a distance of 10 mm or more from an imaginary line T described later when viewed from the Z direction.

[0032] (Structure of irradiation device)

[0033] like Figure 1 As shown, the irradiation device A has a light source unit A1, an optical system A2, and a scanning mechanism A3. The light source unit A1 is a light source that generates laser light L. The light source unit A1 may be any device, but for example, a Nd-doped YAG crystal (Nd:YAG) or the like may be used. The optical system A2 is arranged on the side of the traveling direction of the laser light L relative to the light source unit A1, and the laser light L from the light source unit A1 is incident. The optical system A2 emits the incident laser light L toward the main surface 10A. The scanning mechanism A3 is a mechanism for scanning (scanning) the laser light L. That is, the scanning mechanism A3 scans (moves) the position irradiated to the main surface 10A of the laser light L, that is, the irradiation position in a direction parallel to the main surface 10A. The scanning mechanism A3 may be any mechanism as long as it can scan the laser light L, for example, it may be a galvanometer or the like. In addition, the structure of the irradiation device A is not limited to the above description, and may be any structure that can irradiate the laser light L while scanning the irradiation position in a direction parallel to the main surface 10A. For example, the position of the laser head irradiating the laser L such as the light source unit A1 and the optical system A2 may be fixed, and the base material 10 irradiated with the laser L may be moved to scan the irradiation position. In other words, it can be said that the irradiation position can be scanned by moving the relative position of the spot position of the laser L and the base material 10.

[0034] The scanning of the laser L is not limited to the direction parallel to the main surface 10A, and can also be implemented in the direction perpendicular to the main surface 10A, that is, in the thickness direction of the glass article 100. For example, when the thickness of the glass article 100 is 3 mm or more, by scanning in the thickness direction, it is easy to reduce the stress required for fracture. On the other hand, when the thickness of the glass article 100 is less than 3 mm, it is preferred not to scan in the thickness direction, but to form the modified portion by a single pulse irradiation. That is, it is preferred to form each modified portion by a single pulse irradiation (1 shot). By forming the modified portion by a single irradiation, it is possible to suppress the reduction in the quality of the cross section, such as the roughness of the cut surface and the increase in potential damage, due to the offset of the irradiation position caused by each pulse, which may cause steps to be generated in the cross section.

[0035] In addition, the laser light L can be focused into a linear shape by self-focusing caused by the nonlinear Kerr effect, or can be focused into a linear shape by the optical system A2. As a specific optical system A2 in this case, for example, an optical system using an axicon lens, an optical system using a birefringent material, an optical system using a diffractive optical element, or an optical system using optical aberrations can be used.

[0036] In particular, the optical system A2 irradiating the laser L is preferably an aberration optical system that generates aberrations. Since the aberration optical system is excellent in robustness against optical axis alignment deviation between optical elements, even if the optical axis alignment deviation between optical elements is slightly generated due to interference such as vibration and thermal contraction of the device, the light intensity distribution at the processing point is disturbed and the risk of deterioration of the cutting quality is small, and the cross-section quality remains stable for a long time. Therefore, from the perspective of production yield, the optical system 2A is preferably an aberration optical system.

[0037] In addition, the polarization state of the laser light L can use any one of linear polarization, elliptically polarized light, circularly polarized light, radial polarization, and azimuthally polarized light. The polarization state affects the reflectivity of the laser light when it is incident on the main surface A. Therefore, the intensity of the laser light intruding into the base material can be controlled by the combination of the polarization state and the incident angle, so that the focusing distribution of the laser light inside the base material can be adjusted.

[0038] For example, the symmetry in the circumferential direction is intentionally destroyed by incident linear polarized light or elliptically polarized light. By destroying the symmetry of the laser light distribution, the symmetry of the modified portion can be controlled, and the splitting property of the base material can be improved by matching the direction of the predetermined cutting line. By aligning the direction with high splitting property with the predetermined cutting line, the splitting can be performed with less laser input energy, and as a result, the cracks on the fracture surface after fracture can be reduced, and high-quality cutting can be achieved.

[0039] In addition, by injecting circularly polarized light, the symmetry in the circumferential direction is not destroyed and the isotropy can be maintained.

[0040] In addition, the symmetry of the laser may be destroyed due to the imperfection of the laser light source or the transmission optical system. However, by controlling the direction of the linearly polarized light or the elliptically polarized light, the destruction of the symmetry can be offset and compensated.

[0041] Furthermore, by using radially polarized light or azimuthally polarized light, it is possible to influence the intensity distribution in the radiation direction.

[0042] Furthermore, when the polarization state is changed, the light absorption rate at the focal point is also affected in addition to the reflectivity at the main surface A. This is because the light absorption rate at the focal point when the atoms constituting the matrix absorb the energy of the laser and approach the critical electron density is affected by the polarization state.

[0043] (laser)

[0044] Figure 2 1 is a schematic diagram showing an example of an output waveform of a pulse train laser. Figure 3 Schematic diagram showing an example of the output waveform of the laser involved in this embodiment. The laser L irradiated from the irradiation device A is pulsed, which can also be said to be a pulsed oscillating laser (pulsed laser). The laser L involved in this embodiment is a non-pulse train laser, in other words, a laser that performs pulse oscillation in a manner other than a pulse train.

[0045] Figure 2 An example of the waveform of the laser light LX using the pulse train method is shown. Figure 2 The horizontal axis is time, and the vertical axis is the laser output (W). Figure 2 As shown, the pulse train laser LX refers to a laser that outputs a pulse group LPXa having a plurality of small pulses LPX output in a short period at a predetermined period. Here, the period of the small pulses LPX in one pulse group LPXa, that is, the interval (time width) between the small pulses LPX in one pulse group LPXa, is usually set to, for example, several hundred ps to several tens of ns.

[0046] On the other hand, the irradiation device A according to the present embodiment outputs the laser light L in a non-pulse train mode. Figure 3 As shown in FIG. 1 , the non-pulse train laser L does not have a pulse group, but outputs a pulse light LP at a predetermined period. Here, when the interval (time width) between adjacent pulse lights LP in the time series is set as the interval LA, when the laser L is a non-pulse train laser, the minimum value of the interval LA between the pulse lights LP is greater than 1 μs. Figure 2 As in the example of , the minimum value of the interval between the small pulses LPX in the pulse train laser LX is equal to the interval between the small pulses LPX in a pulse group LPXa, and therefore does not satisfy the condition that the minimum value is greater than 1 μs. Figure 3 As shown, the interval LA of the laser light L may be, for example, the interval (time width) between the times when the outputs of the pulsed light LP adjacent to each other in time series reach the maximum value.

[0047] As a result, in the pulse train pulse, the areas irradiated by each small pulse LPX overlap in one pulse group LPXa, whereas in the non-pulse train pulse, the areas irradiated by each pulse LP do not overlap. In this embodiment, since the areas irradiated by each pulse LP do not overlap, the number of times the irradiated area is subjected to shock waves can be reduced, and the generation of cracks around the modified portion formed by irradiation can be suppressed.

[0048] In the irradiation device A, the width (pulse width) LB of the laser light L is set to be greater than or equal to 15 ps and less than or equal to 100 ps.

[0049] like Figure 2 As shown, the width LB of the laser light L may refer to the half-value width (the interval between two points where the intensity of the pulse light LP is half of the peak value) of the pulse light LP of the laser light L. By making the width LB within this range, the modified portion H can be appropriately formed on the base material 10, the base material 10 can be appropriately cut, and cracks on the fracture surface can be suppressed.

[0050] The laser irradiated into the inside of the matrix transfers energy to the valence electrons of the atoms constituting the matrix through multi-photon absorption, thereby increasing the number of free electrons. Therefore, during the width LB of the time of irradiation with the laser, the electron density of the matrix increases. Since the free electrons not only absorb multi-photons but also absorb single photons, if the electron density begins to rise, the light absorption rate also increases, and thus the electron density further increases, and the electron density rises at an accelerated rate. When the electron density rises and exceeds the critical electron density to become an overdense plasma, the electrons act like a mirror to the light and reflect most of the laser light, and no energy is absorbed. Therefore, the time after the critical electron density is exceeded in the width LB of the laser L cannot fully obtain the energy of the laser light.

[0051] On the other hand, since the energy of free electrons is converted into lattice vibration energy by phonon coupling in 1 to 10 ps, ​​the electron density decreases.

[0052] Therefore, in order to input enough energy into the base material to form a modified portion, it is necessary to design the width LB and pulse energy of the laser L to control the speed of the increase and decrease of the electron density without exceeding the critical electron density. In particular, in the case of implementing the method of the present application that does not use a pulse train but only uses the energy of a single pulse light to form a modified portion, the energy that should be input by a single pulse light is larger than that of a pulse train method in which multiple pulse energies are added together. Therefore, according to existing insights, simply increasing the pulse energy will easily exceed the critical electron density, resulting in a problem of not being able to absorb enough energy. In order to solve this problem, the inventors of the present application found that it is necessary to carefully control the above-mentioned electron density, which can be solved by designing the width LB.

[0053] Specifically, when the width LB is set to be greater than 15ps, which is greater than the phonon coupling time, that is, 1 to 10ps, the rate of increase of the electron density can be suppressed, and a balance can be achieved with the rate of decrease of the electron density caused by the conversion to lattice vibration energy, so that the electron density can be maintained within a certain range without exceeding the critical electron density during the width LB. Thus, the energy of the laser light input can be fully absorbed. On the other hand, if the width LB is set to be greater than 100ps, the photon density of the laser light decreases, so the probability of multiphoton absorption is reduced, and the electron density cannot be fully increased. Therefore, by making the width LB of the laser L greater than 15ps and less than 100ps, it can be properly cut off.

[0054] In addition, it is preferable that the width LB and the pitch P have the following relationship.

[0055] P≦0.25×LB+3.5

[0056] Here, P is a value expressed in μm, and LB is a value expressed in ps.

[0057] In addition, if Figure 4 As shown, the pitch P refers to the distance between the centers of the modified sections H adjacent to each other along the imaginary line T when viewed from the Z direction.

[0058] By satisfying the above formula, the maximum stress (hereinafter referred to as the fracture stress) when the base material is fractured can be set to 25MPa or less, so it is preferred. By making the fracture stress below 25MPa, even in the case of a curve with a small radius of curvature, it is possible to cut with a high yield, so it is preferred.

[0059] Here, the relationship between the spacing P and the width LB is explained. As described above, by setting the pulse width to be sufficiently larger than the phonon coupling time, that is, 1 to 10 ps, ​​the increase in the density of excited electrons is suppressed, and the energy converted to lattice vibration is increased. Here, if the lattice vibration energy increases, the band gap is reduced, and single-photon absorption becomes easier. Therefore, the lattice vibration energy of the part irradiated with the laser increases, that is, the temperature rises, and the light absorption of the part that first contacts the incident laser light in the part where the temperature rises increases, so the temperature further rises, and the volume of the modified part increases. Since the larger the pulse width, the more significant this phenomenon is, it is believed that the larger the pulse width, the greater the volume of the modified part. As a result, even if the irradiation spacing is increased, the fracture stress remains low.

[0060] On the other hand, the width LB of the laser light L is preferably set to 15 ps or more and 60 ps or less for the irradiation device A. By setting the width LB to 60 ps or less, the surface roughness of the fractured surface of the base material 10 after fracture can be suppressed, and a high-quality cut surface can be obtained.

[0061] The width LB is more preferably 55 ps or less, further preferably 50 ps or less, and particularly preferably 45 ps or less. On the other hand, the width LB is preferably 20 ps or more.

[0062] In addition, the irradiation device A may emit a laser L having a width (half-value width of pulse light) narrower than the above range from the light source unit A1, and expand the width of the laser L to be within the above range using the optical system A2, and irradiate the base material 10. In this case, the width of the laser L emitted from the light source unit A1 may be, for example, of the order of fs (femtoseconds).

[0063] The width LB can be measured by a pulse width measuring device for ultrashort pulses, such as an autocorrelator, FROG, or SPIDER.

[0064] Here, the energy (J) of one pulse light LP of the laser L per 1 mm thickness of the base material 10 to be irradiated by the laser L is set as the unit energy. That is, the unit energy can be said to be a value obtained by dividing the energy (J) of the pulse light LP by the thickness DA (mm) of the base material 10. In addition, the energy of the pulse light LP can refer to the integral value of the time waveform of the output (W) of the pulse light LP. In this case, the irradiation device A preferably irradiates the laser L in such a way that the unit energy becomes 200 μJ or more and 1500 μJ or less, more preferably the unit energy is 300 μJ or more and 1000 μJ or less, and further preferably the unit energy is 400 μJ or more and 800 μJ or less. By making the unit energy within this range, the modified portion H can be appropriately formed on the base material 10, the base material 10 can be appropriately cut, and cracks on the fracture surface can be suppressed.

[0065] The unit energy can be calculated by measuring the average output value of the laser light L at each moment using a power meter and dividing the energy (integral value of the time waveform) of the pulse light LP calculated using the measured average output value and the pulse repetition frequency by the thickness DA (mm) of the base material 10 .

[0066] The irradiation device A preferably irradiates laser light L having a wavelength that is transparent to the base material 10. That is, the wavelength of the laser light L is preferably within the wavelength range that is transparent to the base material 10. Transparency here means that when light is incident from the main surface 10A side of the base material 10 and emitted from the main surface 10B side, the attenuation rate ΔI of the light is 0.5 or less. In addition, the attenuation rate is set to the intensity I when the intensity of the incident light is ΔI. IN , set the intensity of the emitted light to intensity I OUT In the case of , it is represented by the following formula (1).

[0067] ΔI=(I IN -I OUT ) / I IN ··· (1)

[0068] Furthermore, the wavelength of the laser light L is preferably 250 nm to 3000 nm, more preferably 260 nm to 2500 nm, and even more preferably 350 nm to 1100 nm.

[0069] By setting the wavelength of the laser light L to be within this range, the laser light L can be transmitted through the base material 10 to a certain extent, and nonlinear absorption can be generated inside the base material 10 to appropriately form the modified portion H.

[0070] In addition, the wavelength of the laser light L can be measured by a laser wavelength meter.

[0071] The irradiation device A can irradiate the laser light L in such a manner that the laser light L has an arbitrary spot diameter DL. For example, the spot diameter DL of the laser light L is preferably 1 μm or more and 30 μm or less, more preferably 2 μm or more and 20 μm or less, and further preferably 3 μm or more and 10 μm or less. By making the spot diameter DL within this range, it is possible to form a modified portion H having a size that allows the base material 10 to be appropriately broken. In addition, if Figure 1 As shown, the spot diameter DL refers to the diameter of the laser light L at the most convergent position (the diameter at the focal position).

[0072] (Formation of Modified Section)

[0073] Figures 4 to 6 1 is a schematic diagram for explaining the formation of the modified portion. In the present manufacturing method, the base material 10 is irradiated with the laser light L while scanning the irradiation position, so that a plurality of modified portions H are formed at predetermined intervals along the scanning direction (movement direction) of the irradiation position. Specifically, Figure 4 As shown, in the present manufacturing method, a scanning trajectory of the irradiation position of the laser L, that is, an imaginary line T, is set on the main surface 10A of the base material 10. Then, in the present manufacturing method, by irradiating the laser L while scanning (moving) the irradiation position along the imaginary line T on the main surface 10A of the base material 10, a plurality of modified portions H arranged at predetermined intervals along the imaginary line T are formed. In addition, the imaginary line T can be set to any shape. The length of the imaginary line T can also be arbitrary, but for example, it is preferably 10 mm or more, more preferably 10 mm or more and 5000 mm or less, further preferably 100 mm or more and 5000 mm or less, and particularly preferably 800 mm or more and 2000 mm or less.

[0074] In the present manufacturing method, the diameter D of the modified portion H is preferably set to be 0.2 μm or more and 20 μm or less, more preferably 0.5 μm or more and 10 μm or less, and further preferably 1 μm or more and 5 μm or less. By setting the diameter D of the modified portion H to be within this range, the base material 10 can be appropriately fractured starting from the modified portion H.

[0075] like Figure 4 As shown, the distance between the centers of the modified portions H adjacent to each other along the imaginary line T when viewed from the Z direction is set to a pitch P. In the present manufacturing method, when viewed from the Z direction (a direction perpendicular to the main surface 10A), the modified portion H is preferably formed in such a manner that the pitch P is greater than or equal to 1 μm and less than or equal to 23 μm. By making the pitch P within this range, the modified portion H can be properly formed on the base material 10, the base material 10 can be properly cut, and cracks on the fracture surface can be suppressed. In addition, the pitch P can refer to the average value of the distances between the centers of 10 groups of adjacent modified portions H selected at random.

[0076] In the present manufacturing method, the pitch P may be made different for each shape of the imaginary line T according to the shape of the imaginary line T observed from the Z direction. Figure 5 As shown, when viewed from the Z direction, in the interval T1 where the imaginary line T becomes a straight line, the laser L can be irradiated so that the pitch P1 of the modified portion H becomes 9 μm or less. In addition, in the present manufacturing method, it is preferable to set the pitch P1 of the modified portion H in the interval T1 to be 1 μm or more and 8 μm or less, and more preferably to be more than 3 μm and 7 μm or less. In addition, the interval T1 where the imaginary line becomes a straight line is not limited to being completely straight, but the curvature radius R1 when viewed from the Z direction may be 100 mm or more, preferably 1000 mm or more, and more preferably 2500 mm or more.

[0077] In addition, for example, Figure 6 As shown, when observed from the Z direction, in the interval T2 where the imaginary line T becomes a curve, the laser L can be irradiated in a manner that the pitch P2 of the modified portion H becomes shorter than the pitch P1 in the interval T1. In addition, in the present manufacturing method, it is preferred that the pitch P2 of the modified portion H in the interval T2 is set to be greater than 5 μm and less than 7 μm, and more preferably greater than 5 μm and less than 6 μm. In addition, the interval T2 is preferably an interval continuous with the interval T1 (connected to the interval T1). The radius of curvature R2 of the interval T2 when observed from the Z direction can be less than 100 mm, preferably greater than 2 mm and less than 10 mm, and more preferably greater than 3 mm and less than 5 mm.

[0078] like Figure 1 As shown, in the present manufacturing method, it is preferred to form the modified portion H over the entire thickness (the entire section in the Z direction) of the base material 10. In other words, in the present manufacturing method, it is preferred to irradiate the laser light L so that the modified portion H is formed from the principal surface 10A to the principal surface 10B of the base material 10. By forming the modified portion H from the principal surface 10A to the principal surface 10B, the base material 10 can be appropriately cut with the modified portion H as the starting point.

[0079] (fracture starting from the opening)

[0080] Figure 7 Schematic diagram of a glass article. After forming a plurality of modified portions H along the imaginary line T, in the present manufacturing method, the glass article 100 is separated (cut out) from the base material 10 by causing the base material 10 to break with the modified portion H as the starting point. Since the modified portion H is formed along the imaginary line T, the base material 10 is broken along the imaginary line T by causing the base material 10 to break with the modified portion H as the starting point. Figure 7 As shown, the glass article 100 is cut out. Although the details will be described later, the glass article 100 has an end face 101 which is a fracture surface along the imaginary line T, and a modified portion HA corresponding to the modified portion H remains on the end face 101. Figure 6 In the figure, for the sake of convenience, only a part of the modified portion HA at the end face 101 (imaginary line T) is shown, but in fact, the modified portion HA can be formed over the entire section in the circumferential direction of the end face 101. In addition, the circumferential direction here refers to the circumferential direction when the direction along the central axis AX is the axial direction. The central axis AX refers to the axis passing through the center point of the glass article 100 when viewed from the Z direction and extending in the Z direction.

[0081] In the present embodiment, stress can be generated on the main surface 10A along the imaginary line T, so that the base material 10 is fractured starting from the modified portion H. For example, a CO2 laser is irradiated to the main surface 10A along the imaginary line T, so that stress is generated on the main surface 10A along the imaginary line T, thereby causing the base material 10 to fracture starting from the modified portion H. Among them, the method of causing the base material 10 to fracture starting from the modified portion H is preferably irradiation with a CO2 laser, but is not limited thereto, and a bending load can also be applied along the imaginary line T of the main surface 10A by mechanical means, thereby causing stress to be generated on the main surface 10A along the imaginary line T, and causing the base material 10 to fracture starting from the modified portion H. The mechanical means here refers to a situation where a bending load is physically generated, for example, the bending load can be generated by a machine, or it can be generated by manual operation of an operator.

[0082] In the present manufacturing method, the edge portion (the boundary portion between the end face 101 and the main surface) of the end face 101 of the glass article 100 cut out from the base material 10 may be ground to chamfer the end face 101. The grinding method is arbitrary, for example, a grindstone may be used. As described later, the end face 101 after chamfering includes an end cut surface 101S and a chamfered portion 101T.

[0083] (Chemical strengthening)

[0084] In this manufacturing method, the glass article 100 cut out from the base material 10 can also be subjected to chemical strengthening treatment, and a compressive stress layer is formed on the surface of the glass article 100. The chemical strengthening treatment can be carried out by any method, for example, by immersing the glass article 100 in a molten salt containing an alkali metal. As a typical method, a method of immersing the glass article 100 in a KNO3 molten salt and cooling it to near room temperature after ion exchange treatment can be cited. For the treatment conditions such as the temperature and immersion time of the KNO3 molten salt, it is sufficient to set the surface compressive stress and the thickness of the compressive stress layer to the desired value. In addition, the method for chemical strengthening is not limited to the method using potassium salts such as KNO3 molten salt, but can be any method. For example, chemical strengthening can also be carried out using sodium salts. In addition, the chemical strengthening treatment is preferably carried out after the glass article 100 is cut out, but is not limited thereto, and the base material 10 before cutting out can also be subjected to chemical strengthening treatment, and then the glass article 100 is cut out from the base material 10 after the chemical strengthening treatment.

[0085] (Glass Items)

[0086] Hereinafter, the properties of the glass article 100 will be described. The glass article 100 described below is manufactured by the manufacturing method described above, but any manufacturing method may be used as long as the glass article 100 has the properties described below.

[0087] like Figure 7 As shown in FIG. 1 , the glass article 100 includes a main surface 100A on one side and a main surface 100B on the other side. That is, the area cut out as the glass article 100 in the main surface 10A of the base material 10 becomes the main surface 100A of the glass article 100, and the area cut out as the glass article 100 in the main surface 10B of the base material 10 becomes the main surface 100B of the glass article 100. In addition, the glass article 100 includes an end surface 101 formed by breaking along the imaginary line T.

[0088] The thickness of the glass article 100, that is, the distance in the Z direction from the main surface 100A to the main surface 100B, may be the same as the thickness DA of the base material 10. Figure 7In the example of , the glass article 100 is in the shape of a flat plate, but the present invention is not limited thereto and the glass article 100 may be in the shape of a curved plate. That is, the glass article 100 may be in the shape of a curved surface with the main surfaces 100A and 100B convex in the Z direction. When the glass article 100 is in the shape of a curved surface with the main surfaces 100A and 100B convex in the Z direction, the radius of curvature of the main surfaces 100A and 100B of the glass article 100 is preferably 10000 mm or less, more preferably 5000 mm or less, and further preferably 3000 mm or less. When the main surfaces 100A and 100B of the glass article 100 are in the shape of a curved surface convex in the Z direction, the radius of curvature of the main surfaces 100A and 100B of the glass article 100 is preferably 10 mm or more, more preferably 50 mm or more, further preferably 100 mm or more, and particularly preferably 200 mm or more. That is, the radius of curvature of the main surfaces 100A and 100B of the glass article 100 is preferably in the range of 10 to 10000 mm.

[0089] (End face)

[0090] The end face 101 of the glass article 100 is a cross section formed by breaking the base material 10 along the imaginary line T. Therefore, at least a portion of the modified portion H formed on the base material 10 remains as the modified portion HA on the end face 101. The modified portion HA is a portion of the modified portion H formed by irradiation with the laser L, and can be said to be a linear damaged portion as an irradiation mark (laser mark) of the laser L. That is, a linear modified portion H extending in the Z direction (axial direction) is formed on the end face 101. On the end face 101, a plurality of modified portions HA are formed along the circumferential direction (i.e., along the imaginary line T) when the direction along the central axis AX is the axial direction.

[0091] In addition, a portion having a density, a refractive index, a fictive temperature, or an asymmetric electron density different from a portion of the glass article 100 having no modified portion HA formed therein may be defined as the modified portion HA. In addition, the portion of the glass article 100 having no modified portion HA formed therein may be, for example, a position at a distance of 10 mm or more from the end face 101 when viewed in the Z direction.

[0092] The width ΔH of the modified portion HA when viewed from the Z direction is preferably 20 μm or less, more preferably 10 μm or less, and further preferably 5 μm or less. In addition, the width ΔH refers to the distance from the end HAa to the end HAb of the modified portion HA in the main surface 100A. In addition, the end HAa is the end of one side of the modified portion HA in the circumferential direction of the end surface 101 (in the direction of the imaginary line T), and the end Hab refers to the end of the other side of the modified portion HA.

[0093] In addition, the distance between the centers of the adjacent modified portions HA in the circumferential direction of the end face 101 (in the direction along the imaginary line T) when viewed from the Z direction is set to a pitch PA. When viewed from the Z direction, the pitch PA is preferably greater than 1 μm and less than 23 μm. By setting the pitch PA to this range, a glass article is obtained that is properly cut from the base material 10 and that cracks are suppressed from occurring on the end face 101. In addition, the pitch P may refer to the average value of the distances between the centers of 10 groups of adjacent modified portions HA selected at random.

[0094] The glass article 100 may also be configured such that the spacing PA is different for each shape of the line (corresponding to the imaginary line T) connecting the centers of the modified parts HA when viewed from the Z direction. For example, when viewed from the Z direction, the line connecting the centers of the modified parts HA becomes a straight line in the interval 101A (corresponding to the interval T1), and the spacing PA1 of the modified parts HA may be 9 μm or less. In addition, the spacing PA1 of the modified parts HA in the interval 101A is preferably greater than 1 μm and less than 8 μm, and more preferably greater than 3 μm and less than 7 μm. In addition, the interval 101A, which is a line connecting the centers of the modified parts HA, is not limited to being completely straight. The radius of curvature R1 of the line connecting the centers of the modified parts HA in the interval 101A when viewed from the Z direction may be greater than 100 mm, preferably greater than 1000 mm, and more preferably greater than 2500 mm. In addition, the line connecting the centers of the modified parts HA may also be said to be a line along the end surface 101.

[0095] In addition, for example, in the interval 101B (corresponding to the interval T2) where the line connecting the centers of the modified parts HA is a curve when viewed from the Z direction, the spacing PA2 of the modified parts HA can be shorter than the spacing PA1 in the interval 101A. In addition, the spacing PA2 of the modified parts HA in the interval 101B is preferably greater than 5 μm and less than 7 μm, and more preferably greater than 5 μm and less than 6 μm. In addition, the interval 101B is preferably an interval continuous with the interval 101A (connected to the interval 101A). The radius of curvature R2 of the line connecting the centers of the modified parts HA in the interval 101B when viewed from the Z direction can be less than 100 mm, preferably greater than 2 mm and less than 10 mm, and more preferably greater than 3 mm and less than 5 mm.

[0096] The surface roughness Sa of the end face 101 as specified in ISO25178 is 0.6 or less, more preferably 0.3 or more and 0.6 or less, and further preferably 0.4 or more and 0.6 or less. When the surface roughness Sa is within this range, the glass article is suppressed from cracking on the end face 101. In addition, when the surface roughness Sa is within this range, the probability of damage when impact or stress is applied to the glass article 100 can be reduced.

[0097] The surface roughness Sa can be measured using a laser microscope Olympus OLS5000. The surface roughness Sa is measured at three or more points at the center of the end surface 101 in the thickness direction, for example, and the average value is used.

[0098] In this way, the glass article 100 has the modified portion HA formed on the end surface 101. However, the modified portion HA may be removed by polishing the end surface 101.

[0099] (Modification Department)

[0100] Figure 8 is a schematic diagram showing the end face of a glass object. Figure 8 As shown, the modified portion HA is preferably formed throughout the entire thickness (the entire section in the Z direction) of the glass article 100. In other words, the modified portion HA is preferably formed from the main surface 100A to the main surface 100B of the glass article 100. By forming the modified portion HA from the main surface 100A to the main surface 100B, the glass article is appropriately cut from the base material 10 and cracks are suppressed from occurring on the end surface 101.

[0101] In addition, the glass article 100 sometimes has a crack CR extending from the modified portion HA toward the outer side in a direction perpendicular to the Z direction, that is, in a radial direction. The radial direction here refers to the radial direction when the central axis AXa of the modified portion HA is the axial direction. The central axis AXa refers to an axis passing through the center point of the modified portion HA and extending in the Z direction when viewed from the Z direction. A plurality of cracks CR may be formed around the modified portion HA. In addition, the crack CR may extend to the inside of the modified portion HA.

[0102] Here, a position on the end face 101 which is 10% away from the main surface 10A toward the Z2 side by the thickness DA of the glass article 100 is set as a first position NA. Similarly, a position which is 10% away from the main surface 10B toward the Z1 side by the thickness of the glass article 100 is set as a second position NB. In the range from the main surface 100A to the first position NA and the range from the main surface 100B to the second position NB, the component of the radial length of the crack CR that is orthogonal to the end face 101 is set as the length LCR1. The length LCR1 refers to the distance from the central axis HA of the modified portion to the end of the crack CR on the opposite side (radially outer side) of the modified portion HA in the direction orthogonal to the end face 101. The length LCR1 can also be said to be the length of the crack CR in the direction parallel to the main surface of the glass article 100 and orthogonal to the imaginary line T. In this case, the length LCR1 is preferably 12 μm or less. In addition, as the value of the length LCR1, it is preferred to use the average value of the length LCR1 of the crack CR at three modified portions HA selected arbitrarily from the end face 101. By making the length LCR1 within this range, the glass article is suppressed from generating cracks at the end face 101. In addition, for the length LCR1 of the crack CR, the main surface 10A is observed using a digital microscope (e.g., VHX-6000 manufactured by KEYENCE), and the distance between the line K connecting the centers of the modified portions HA and the end on the opposite side of the modified portion HA can be measured as the length LCR1.

[0103] In addition, the length of the crack CR in the region from the first position NA to the second position NB of the end face 101 in the direction perpendicular to the end face 101 is set as the length LCR2. The length LCR2 can also be said to be the length of the crack CR in the direction parallel to the main surface of the glass article 100 and perpendicular to the imaginary line T. In this case, the length LCR2 of the crack CR is preferably 7 μm or less. In addition, as the length LCR2 of the crack CR in the region from the first position NA to the second position NB, it is preferable to use the average value of the lengths LCR2 of three cracks CR arbitrarily selected from the region from the first position NA to the second position NB. By making the length LCR2 within this range, the glass article in which the generation of cracks on the end face 101 is suppressed.

[0104] Usually, the length LCR1 is greater than the length LCR2. Near the surface of the substrate, a tiny amount of plume is generated outside the substrate during laser irradiation, and a shock wave is generated inside the substrate as a reaction force to the momentum of the plume. Therefore, when laser irradiation is performed in a state where a crack CR is formed by laser irradiation, the crack CR extends with the help of the stress of the shock wave. The shock propagates radially in the substrate in a spherical shape with the intersection of the center of the optical axis and the surface of the substrate as the center, so the substrate surface as the generation source is subjected to the strongest shock. Therefore, the length LCR1 of the crack CR near the surface is longer than the length LCR2 of the crack inside the substrate.

[0105] In the case of a pulse train, since the number of pulses is large, the extension number of cracks CR caused by the shock wave is large, and thus the length LCR1 becomes longer. On the contrary, in the case of a single pulse described in the present application, the number of shock waves is suppressed to a minimum, thereby suppressing the length LCR1 and obtaining a high-quality cut surface.

[0106] The crack CR in the region from the first position NA to the second position NB can be regarded as a latent flaw that is not exposed on the end surface 101 but is located inside the end surface 101. The crack CR in the region from the first position NA to the second position NB can be measured by the following method, for example.

[0107] First, an evaluation area (area where the length LCR2 of the crack CR is measured) of the end surface 101 of the glass article 100 is polished by a predetermined amount, cleaned, dried, and then etched to form a circular or elliptical pit, and the altered layer is observed using an optical microscope.

[0108] Here, the "process-damaged layer" refers to a layer having scratches, cracks, etc. generated in the glass plate during processing steps such as chamfering and grinding.

[0109] As an optical microscope, a laser microscope LEXT OLS5000 manufactured by Olympus can be used, and observation is performed using a 50-times objective lens with an observation field of 258 μm×258 μm.

[0110] The thickness of the glass article 100 removed by grinding and etching when the circular pit or elliptical pit at the same position is no longer observed in the evaluation area after repeating this process (latent flaw confirmation by grinding and etching) multiple times is defined as the length LCR2 of the crack CR at that position. That is, the maximum value of the distance of the crack CR in the evaluation area in the direction perpendicular to the end face 101 is measured as LCR2.

[0111] In addition, “etching” can be performed by immersing the entire glass plate in an etching solution at room temperature (25° C.) As the etching solution, an aqueous solution containing 5 mass % of hydrofluoric acid (HF) and 95 mass % of pure water can be used.

[0112] In addition, the above description is about the crack CR formed in the glass article 100 cut out from the base material 10, but the crack CR can also be formed in the base material 10 irradiated with the laser L to form the modified part H. In this case, since the base material 10 is not broken and the end face 101 is not formed, the crack CR can be observed and confirmed from the main surface 10A. In this case, the length LCR1 of the crack CR on the main surface 10A is preferably 12 μm or less. In addition, the length LCR1 of the crack CR on the main surface 10A can be the average value of the lengths LCR1 of three cracks CR selected arbitrarily from the main surface 10A.

[0113] Fig. 9 1 is a schematic diagram showing an example of an end face in which chamfering is performed. As described above, the end face 101 is sometimes chamfered. In this case, Fig. 9 As shown in FIG. 1 , the end face 101 includes an end cut face 101S and a chamfered portion 101T. The end cut face 101S is a surface of the end face 101 that has not been chamfered. The chamfered portion 101T is a surface of the end face 101 that has been chamfered. Fig. 9 As shown in the figure on the left side of FIG. 1 , the chamfered portion 101T may be formed in the Z direction at a position between the main surface 100A and the end cut surface 101S, and at a position between the main surface 100B and the end cut surface 101S. Fig. 9 As shown in the figure on the left side of FIG. 1 , the chamfered portion 101T is inclined in a manner that moves away from the main surface 100B in the Z direction toward the radial inner side of the glass article 100. Fig. 9 In the example of FIG. 1 , the chamfered portion 101T is flat and chamfered at right angles. However, the chamfering is not limited to right angles and may be rounded. In this case, the shape of the chamfered portion 101T becomes a curved surface.

[0114] Thus, when the end face 101 is chamfered, Fig. 9 As shown in the figure on the right side of FIG. 101 , the modified portion H is formed on the cut surface 101S (the modified portion H remains). On the other hand, since the modified portion H is removed by chamfering, the modified portion H is not formed on the chamfered portion 101T (the modified portion H does not remain).

[0115] (Material of glass items)

[0116] The glass article 100 is a transparent plate-shaped component. The material of the glass article 100 is glass. The glass article 100 may be an amorphous glass, or a crystallized glass containing crystals on the surface or inside. As the glass article 100, for example, alkali-free glass, sodium-lime glass, soda-lime silicate glass, aluminosilicate glass, borosilicate glass, lithium aluminosilicate glass, borosilicate glass, etc. can be used. In order to properly perform chemical strengthening, the material of the glass article 100 is preferably alkali glass. Further, as the glass article 100, it is preferred that aluminosilicate glass or lithium aluminosilicate glass, which can easily generate large stress through strengthening treatment even if the thickness is thin, and can obtain high strength even if it is thin, is used. It is also preferred to use a chemically strengthened glass based on aluminosilicate glass (for example, "Dragontrail (registered trademark)" manufactured by AGC Corporation).

[0117] In addition, as the base material 10, either glass before chemical strengthening or glass after chemical strengthening can be used, and glass before chemical strengthening is preferably used. More preferably, glass before chemical strengthening is used as the base material 10, and chemical strengthening is performed after the base material 10 is cut, so that a compressive stress layer is also formed on the cut surface, which is preferred. In the case of laser cutting of glass before chemical strengthening, cracks between irradiation intervals are less likely to develop than glass after chemical strengthening, but according to the cutting method in this embodiment, even glass before chemical strengthening can be properly cut.

[0118] (Composition of glass)

[0119] In terms of mole % based on oxides, the glass article 100 may contain 50% to 80% SiO2, 1% to 20% Al2O3, and 6% to 20% Na2O. In addition, in terms of mole % based on oxides, the glass article 100 may contain 50% to 80% SiO2, 0.1% to 25% Al2O3, 3% to 30% Li2O+Na2O+K2O, 0% to 25% MgO, 0% to 25% CaO, and 0% to 5% ZrO2. In addition, in terms of mole % based on oxides, the glass article 100 may contain 50% to 80% SiO2, 1% to 20% Al2O3, 6% to 20% Na2O, 0% to 11% K2O, 0% to 15% MgO, 0% to 6% CaO, and 0% to 5% ZrO2. The numerical range indicated by "~" refers to a range including the numerical values ​​before and after "~" as the lower limit and the upper limit. In addition, for example, 50% to 80% here means that when the mole % of the total amount of the glass article 100 is set to 100%, it is 50% or more and 80% or less, and the same applies to other numerical ranges. In addition, for example, Li2O+Na2O+K2O refers to the total content of Li2O, Na2O and K2O, and the same applies to other cases where "+" is used.

[0120] More specifically, as a more preferable composition of the glass article 100, the following glass compositions can be cited. For example, "containing 0% to 25% of MgO" means that MgO is not essential, but may be contained up to 25%. The glass of (i) is contained in soda-lime silicate glass, the glasses of (ii) and (iii) are contained in aluminosilicate glass, and the glasses of (iv), (v) and (vi) are contained in lithium aluminosilicate glass.

[0121] (i) Glass comprising, in terms of composition expressed in mol%, 63% to 73% SiO2, 0.1% to 5.2% Al2O3, 10% to 16% Na2O, 0% to 1.5% K2O, 0% to 5% Li2O, 5% to 13% MgO, and 4% to 10% CaO.

[0122] (ii) Glass whose composition, expressed in mol %, contains 50% to 74% of SiO2, 1% to 10% of Al2O3, 6% to 14% of Na2O, 3% to 11% of K2O, 0% to 5% of Li2O, 2% to 15% of MgO, 0% to 6% of CaO, and 0% to 5% of ZrO2, the total content of SiO2 and Al2O3 being less than 75%, the total content of Na2O and K2O being 12% to 25%, and the total content of MgO and CaO being 7% to 15%.

[0123] (iii) Glass whose composition, expressed in mol %, contains 68% to 80% of SiO2, 4% to 10% of Al2O3, 5% to 15% of Na2O, 0% to 1% of K2O, 0% to 5% of Li2O, 4% to 15% of MgO, and 0% to 1% of ZrO2.

[0124] (iv) Glass having a composition expressed in mol % comprising 67% to 75% SiO2, 0% to 4% Al2O3, 7% to 15% Na2O, 1% to 9% K2O, 0% to 5% Li2O, 6% to 14% MgO, and 0% to 1.5% ZrO2, the total content of SiO2 and Al2O3 being 71% to 75%, the total content of Na2O and K2O being 12% to 20%, and in the case of CaO being contained, its content is less than 1%.

[0125] (v) Glass whose composition, expressed in mol %, contains 56% to 73% SiO2, 10% to 24% Al2O3, 0% to 6% B2O3, 0% to 6% P2O5, 2% to 7% Li2O, 3% to 11% Na2O, 0% to 5% K2O, 0% to 8% MgO, 0% to 2% CaO, 0% to 5% SrO, 0% to 5% BaO, 0% to 5% ZnO, 0% to 2% TiO2, and 0% to 4% ZrO2.

[0126] (vi) Glass whose composition, expressed in mol %, contains 58% to 80% of SiO2, 13% to 18% of Al2O3, 0% to 5% of B2O3, 0.5% to 4% of P2O5, 3% to 10% of Li2O, 5% to 20% of Na2O, 0% to 2% of K2O, 0% to 11% of MgO, 0% to 20% of CaO, 0% to 20% of SrO, 0% to 15% of BaO, 0% to 10% of ZnO, 0% to 1% of TiO2 and 0% to 2% of ZrO2.

[0127] (Compressive stress layer)

[0128] When the chemical strengthening treatment is performed, the glass article 100 includes a compressive stress layer. The compressive stress layer is formed on the entire surface of the glass article 100, that is, here, it is formed on the main surface 100A, the main surface 100B, and the end surface 101. In addition, the glass article 100 is not limited to the compressive stress layer formed on all of the main surface 100A, the main surface 100B, and the end surface 101, and the compressive stress layer may be formed on at least one of the main surface 100A, the main surface 100B, and the end surface 101 (preferably, at least the main surface 100A).

[0129] The compressive stress layer is a layer in which compressive stress acts in the glass article 100. The glass article 100 has a compressive stress S acting on the surface, and the compressive stress decreases toward the center of the thickness direction of the glass article. For example, the compressive stress layer can be said to be a portion of the entire glass article 100 from the surface to the depth where the stress becomes 0. In addition, the glass article 100 has a tensile stress acting on a layer deeper than the depth where the stress becomes 0. Hereinafter, the compressive stress acting on the surface of the glass article 100, i.e., the surface of the compressive stress layer, is recorded as the surface compressive stress CS.

[0130] The surface compressive stress CS of the glass article 100 is preferably 500 MPa or more and 1200 MPa or less, more preferably 650 MPa or more, and further preferably 750 MPa or more. By making the surface compressive stress CS within this range, the reduction in impact resistance can be appropriately suppressed. In addition, the method for measuring the surface compressive stress CS is arbitrary, but for example, it can be measured by measuring the strain in the glass article 100 using a photoelastic analysis method. In this embodiment, for example, the surface compressive stress CS can also be measured using a surface stress meter FSM-6000LE manufactured by Orihara Manufacturing Co., Ltd.

[0131] The depth DOL of the compressive stress layer of the glass article 100 is preferably greater than 10 μm and less than 100 μm, more preferably greater than 15 μm, further preferably greater than 25 μm, and particularly preferably greater than 30 μm. The depth DOL refers to the thickness of the compressive stress layer in the glass article 100. That is, the depth DOL refers to the distance in the thickness direction from the surface of the glass article 100 on which the surface compressive stress CS acts to the depth at which the value of the compressive stress becomes 0. The glass article 100 can appropriately suppress the reduction in impact resistance by making the depth DOL within this range. In addition, the method for measuring the depth DOL is arbitrary, but for example, it can be measured by measuring the strain in the glass article 100 using a photoelastic analysis method. In the present embodiment, for example, the depth DOL can be measured using a surface stress meter FSM-6000LE manufactured by Orihara Manufacturing.

[0132] (Uses of glass items)

[0133] Fig.10 Schematic diagram showing a vehicle-mounted display according to the present embodiment. Fig.10 As shown, the glass article 100 according to the present embodiment is provided on a vehicle-mounted display 2 and is used as a cover material for the surface of the vehicle-mounted display. The vehicle-mounted display 2 is a display device provided on a vehicle, for example, provided in front of a steering shaft 1 in a vehicle. The vehicle-mounted display 2 displays, for example, a car navigation screen, various instruments such as a speedometer, and a start button. However, Fig.10The structure of is an example, and the vehicle-mounted display 2 using the glass article 100 may have any structure. In addition, the glass article 100 is not limited to being used as a cover material for the surface of the vehicle-mounted display, and can be used for any purpose.

[0134] (Effect)

[0135] As described above, the method for manufacturing the glass article 100 according to the present embodiment includes: forming a plurality of modified portions H along the imaginary line T set on the main surface 10A of the base material 10 by irradiating the base material 10 with pulsed laser light L along the imaginary line T; and cutting the glass article 100 from the base material 10 by breaking the base material 10 starting from the modified portion H along the imaginary line T. When forming the modified portion H, pulse oscillation is performed by a method other than a pulse train method, and the laser light having a pulse width (width LB) of 15 ps or more and 100 ps or less is irradiated.

[0136] Here, when the pulse train method is used, since the regions irradiated with small pulse lights overlap, the irradiated portion is exposed to a plurality of shock waves, and cracks may be generated on the fracture surface cut starting from the modified portion.

[0137] In contrast, according to the present manufacturing method, since the laser L is irradiated in a non-pulse train mode, it is possible to suppress the exposure of the irradiated portion to multiple shock waves and suppress the generation of cracks on the fracture surface. On the other hand, if it is a non-pulse train mode, the number of pulses irradiated at one irradiated portion is reduced compared to the pulse train mode, so the energy imparted to the base material 10 is reduced, and there is a possibility that the base material cannot be properly modified. However, according to the present manufacturing method, by setting the width LB to be greater than 15ps and less than 100ps, it is possible to fully ensure the energy imparted to the base material 10, and the base material can be properly modified and fractured. Furthermore, according to the present manufacturing method, by adopting a non-pulse train mode and setting the pulse width LB to the above range, the stress required for fracture can be reduced, and the base material 10 can be properly fractured. In addition, the surface roughness of the end face 101 (fracture surface) of the glass article 100 when fractured can be improved, and the generation of cracks on the end face 101 can be suppressed.

[0138] In addition, the glass article 100 according to the present embodiment has a main surface 100A and an end surface 101, and a plurality of linear modified portions HA extending in the thickness direction (Z direction) of the glass article 100 are formed on the end surface 101, and the surface roughness Sa of the end surface 101 as specified in ISO 25178 is 0.6 or less. The glass article 100 according to the present embodiment is appropriately cut, and the generation of cracks on the end surface 101 (fracture surface) is suppressed.

[0139] The present disclosure describes the following inventions, but is not limited thereto.

[0140] (1) A method for manufacturing a glass article, comprising: irradiating a base material with a pulsed laser along an imaginary line set on a main surface of the base material to form a plurality of modified portions along the imaginary line; and fracturing the base material with the modified portion along the imaginary line as a starting point to cut out a portion of the base material to obtain a glass article, wherein a minimum pulse interval of the laser is greater than 1 μs, and a pulse width of the laser is greater than 15 ps and less than 100 ps.

[0141] (2) According to the method for manufacturing a glass article described in (1), the pitch P and the pulse width LB have the following relationship: P≦0.25×LB+3.5, wherein P is a value expressed in μm and LB is a value expressed in ps.

[0142] (3) The method for producing a glass article according to (1) or (2), wherein the pulse width of the laser light is 15 ps to 60 ps.

[0143] (4) The method for producing a glass article according to any one of (1) to (3), wherein the wavelength of the laser light is a wavelength at which the base material becomes transparent.

[0144] (5) The method for producing a glass article according to any one of (1) to (4), wherein a pitch between the plurality of modified portions is 1 μm or more and 23 μm or less when viewed from a direction perpendicular to a main surface of the base material.

[0145] (6) The method for producing a glass article according to any one of (1) to (5), wherein the energy of one pulse of the laser light is 200 μJ or more and 1500 μJ or less per 1 mm thickness of the base material.

[0146] (7) According to the manufacturing method of a glass article described in any one of (1) to (6), when observed from a direction perpendicular to the main surface of the base material, the spacing between multiple modified parts in the interval where the imaginary line becomes a curve is shorter than the spacing between multiple modified parts in the interval where the imaginary line becomes a straight line.

[0147] (8) The method for producing a glass article according to any one of (1) to (7), wherein the modified portion is formed from a principal surface of the base material to an opposite principal surface.

[0148] (9) According to the manufacturing method of a glass article described in any one of (1) to (8), when a position that is 10% of the thickness of the glass article away from a first main surface on one side to a second main surface on the opposite side is set as a first position, for a crack extending from the above-mentioned modified portion in a region from the first main surface to the first position, the length in a direction parallel to the main surface of the glass article and orthogonal to the imaginary line is less than 12 μm.

[0149] (10) The method for producing a glass article according to any one of (1) to (9), wherein the thickness of the base material is 0.7 mm or more.

[0150] (11) A method for producing a glass article according to any one of (1) to (10), wherein the fracture toughness value K of the base material is IC 0.6 (MPa·m 0.5 )above.

[0151] (12) The method for producing a glass article according to any one of (1) to (11), wherein the thickness of the base material is less than 3 mm, and the plurality of modified portions are each formed by a single pulse irradiation.

[0152] (13) The method for producing a glass article according to any one of (1) to (12), wherein the optical system for irradiating the laser light is an aberration optical system.

[0153] (14) A glass article having a main surface and an end surface, wherein a plurality of linear modified portions extending in the thickness direction of the glass article are formed on the end surface, and the surface roughness Sa of the end surface as specified in ISO 25178 is 0.6 μm or less.

[0154] (15) According to the glass article described in (14), when a position that is 10% of the thickness of the glass article away from the first principal surface on one side to the second principal surface on the opposite side is set as the first position, for a crack extending from the modified portion in the area from the first principal surface to the first position, the length in the direction orthogonal to the end face is less than 12 μm.

[0155] (16) According to the glass article described in (14) or (15), when a position on the end surface that is 10% of the thickness of the glass article from the first principal surface on one side to the second principal surface on the opposite side is set as a first position, and a position on the end surface that is 10% of the thickness of the glass article from the second principal surface to the first principal surface is set as a second position, for a crack extending from the modified portion in the area from the first position to the second position of the end surface, the length in a direction perpendicular to the end surface is less than 7 μm.

[0156] (17) The glass article according to any one of (14) to (16), wherein a pitch of the modified parts is 1 μm or more and 23 μm or less when viewed from a direction perpendicular to the main surface.

[0157] (18) According to any one of (14) to (17), when the glass article is observed from a direction perpendicular to the main surface, the spacing of the modified parts in the interval where the line along the end surface is a curve is shorter than the spacing of the modified parts in the interval where the line along the end surface is a straight line.

[0158] (19) The glass article according to any one of (14) to (18), wherein the thickness is 0.7 mm or more.

[0159] (20) A glass article according to any one of (14) to (19), wherein the fracture toughness value K IC 0.6 (MPa·m 0.5 )above.

[0160] Example

[0161] Next, examples are described. Fig.11 Schematic diagram of the cutout of the base material of the embodiment. In the embodiment, a base material with a length of 50 mm and a width of 50 mm ( Fig.11 A base material with a width L1 and a thickness of 1.3 mm was used. As the base material, Dragontrail (registered trademark) manufactured by AGC Corporation was used. In addition, the base material used was a base material that was not chemically strengthened. Then, an imaginary line extending straightly from the center position of the base material in the horizontal direction (width direction) to the longitudinal direction was set so that the longitudinal length of the glass article cut out from the base material was 50 mm and the transverse width was 25 mm, and a pulsed laser was irradiated along the imaginary line. The following shows the irradiation conditions of the laser.

[0162] Irradiation conditions:

[0163] Wavelength: 1064nm

[0164] Output: 6W~10W

[0165] Collimation diameter: 8mm

[0166] Feed speed: 10~230mm / s

[0167] Oscillation frequency: 10000Hz

[0168] like Fig.11 As shown, a pair of cylindrical jigs Ja are used to support the main surface of the side of the base material irradiated with laser light for laser incidence, and a pair of cylindrical jigs Jb are lowered at a descending speed of 1 mm / min toward the main surface on the side of the laser light emission, so that the jigs Jb are in contact with the main surface on the upper side, thereby applying stress to the base material and cutting the base material along the imaginary line T. In addition, the jigs Ja are arranged on both sides of the imaginary line T in the width direction, and the interval L2 between the pair of jigs Ja is set to 30 mm. The jigs Jb are arranged on both sides of the imaginary line T in the width direction, and the interval L3 between the pair of jigs Jb is set to 10 mm.

[0169] (Experiment 1)

[0170] Table 1 shows the evaluation results of each example in Experiment 1. As shown in Table 1, in Example 1, as the laser irradiation condition, an optical system 1 (SmartCleave Classic Torch (hereinafter referred to as CL) of Coherent Company was used to irradiate the laser in a pulse train mode, and the pulse width (width LB in this embodiment) was set to 10ps. In addition, in Example 1, the number of pulse lights in one pulse group was set to four, the interval between the pulse lights in one pulse group was set to 13ns, and the irradiation period of the pulse group was set to 37.5kHz.

[0171] In Example 2, as the laser irradiation condition, an optical system 2 is used to irradiate the laser in a non-pulse train mode, the pulse width (width LB in this embodiment) is set to 20ps, the interval between the pulse lights is set to 100μs, and the spacing between the modified parts (spacing P in this embodiment) is set to 3μm. The other conditions are the conditions shown above. For Examples 3 to 6, in addition to the conditions shown in Table 1, the same conditions as in Example 2 are also set. In addition, the optical system 2 refers to the SmartCleave HighEfficiency Torch (hereinafter referred to as HE) of Coherent.

[0172] [Table 1]

[0173]

[0174] As shown in Table 1, for the glass articles obtained by breaking the base material under the conditions of Examples 1 to 6, the surface roughness Sa of the end face (fracture face) and the maximum crack depth (LCR2) from the first position NA to the second position NB of the end face were measured.

[0175] The surface roughness Sa was measured using a laser microscope OLS5000 manufactured by Olympus Corporation. The average value of three or more points was calculated at the center in the thickness direction.

[0176] In the measurement of the maximum crack depth LCR2, as described above, the end face (fracture surface) of the glass article 100 of each example is ground and etched, and the end face 101 is observed from a direction perpendicular to the main surface using a digital microscope (VHX-6000 manufactured by KEYENCE Corporation) to visually confirm the presence or absence of pits, and the removed thickness when the pits can no longer be confirmed is taken as the maximum crack depth.

[0177] In the evaluation of Experiment 1, the case where the surface roughness Sa satisfies 0.630 or less is qualified, and the case where it does not satisfy is unqualified. As shown in Table 1, it can be seen that Example 1 of the pulse train method as a comparative example is unqualified and cannot reduce the surface roughness at the fracture surface. On the other hand, it can be seen that in Examples 2 to 6 of the non-pulse train method as an embodiment, it is qualified and the surface roughness at the fracture surface can be reduced. In addition, as shown in Examples 1 and 2, it can be seen that by adopting the non-pulse train method, the maximum crack depth can also be suppressed.

[0178] (Experiment 2)

[0179] Table 2 shows the evaluation results of each example in Experiment 2. In Experiment 2, glass articles were manufactured in a non-pulse train mode with different pulse width and spacing conditions. Table 2 shows the conditions in each example. In addition, the unit energy in Table 2 refers to the unit energy described in this embodiment (the value obtained by dividing the energy (μJ) of the pulse light by the thickness (mm) of the base material 10).

[0180] [Table 2]

[0181]

[0182] In Experiment 2, the maximum stress value applied to the base material irradiated with laser light under the conditions of each example when the base material was fractured using the jigs Ja and Jb was measured as the fracture stress. More specifically, 20 samples of glass articles were manufactured according to the conditions of each example, and the average value of the maximum stress value applied to each sample was taken as the fracture stress. Table 2 shows the results. In addition, the table-top precision universal testing machine "Autograph AGS-X 10kN" manufactured by Shimadzu Corporation was used for the measurement of the maximum stress value.

[0183] As shown in Table 2, it can be seen that the base material can be broken appropriately in Examples 8 to 28, which are embodiments in which the pulse width is set to 15 ps or more and 100 ps or less. On the other hand, it can be seen that in Example 7, which is a comparative example in which the pulse width is set to 10 ps, ​​the base material cannot be broken under the conditions of this time, and the modified portion cannot be formed appropriately, so the base material cannot be broken appropriately.

[0184] (Experiment 3)

[0185] Next, the correlation between the pitch P and the pulse width LB was studied. Fig.12 , the evaluation results of each example in Experiment 3 are shown. In Experiment 3, glass articles were manufactured by changing the pulse width and pitch conditions in the non-pulse train method. Tables 3 and 4 show the conditions of each example.

[0186] In Example 29, as the laser irradiation condition, optical system 2 is used to irradiate the laser in a non-pulse train mode, the pulse width (width LB in this embodiment) is set to 32.9ps, the interval between the pulse lights is set to 100μs, and the spacing between the modified parts (spacing P in this embodiment) is set to 5μm. Other conditions are as shown above. For Examples 30 to 63 and Examples 68 to 75, in addition to the conditions shown in Table 3 or Table 4, the same conditions as in Example 29 are also set. In addition, optical system 2 refers to SmartCleave HighEfficiency Torch (hereinafter referred to as HE) of Coherent.

[0187] In Example 64, as the laser irradiation condition, the optical system 3 is used to irradiate the laser in a non-pulse train mode, the pulse width (width LB in the present embodiment) is set to 20ps, the interval between the pulse lights is set to 100μs, and the spacing between the modified parts (spacing P in the present embodiment) is set to 3μm. Other conditions are as shown above. For Examples 65 to 67, in addition to the conditions shown in Table 4, the same conditions as in Example 64 are also set. In addition, the optical system 3 refers to a synthetic quartz spherical plano-convex lens element with a focal length of 15mm, and refers to an optical system that incidents the laser from the flat surface side of the element and emits the laser from the spherical surface side.

[0188] In addition, the unit energy in Tables 3 and 4 refers to the unit energy described in this embodiment (a value obtained by dividing the energy (μJ) of the pulse light by the thickness (1.3 mm) of the base material 10).

[0189] The same test as in Experiment 2 was carried out to measure the breaking stress.

[0190] [Table 3]

[0191]

[0192] [Table 4]

[0193]

[0194] As shown in Tables 3-4 and Fig.12 As shown, in the embodiment satisfying the relational expression P≦0.25×LB+3.5, the maximum stress when the base material is fractured (hereinafter referred to as fracture stress) can be set to 25 MPa or less.

[0195] Above, the embodiments of the present invention have been described, but the embodiments are not limited to the contents of the present embodiments. In addition, the above-mentioned constituent elements include elements that can be easily thought of by those skilled in the art, substantially the same elements, and elements of so-called equivalent scopes. In addition, the above-mentioned constituent elements can be appropriately combined. In addition, various omissions, substitutions or changes of constituent elements can be performed without departing from the scope of the gist of the above-mentioned embodiments.

[0196] This application is based on the Japanese patent application (Japanese Patent Application No. 2022-072576) filed on April 26, 2022, and the contents thereof are incorporated into this specification as a reference.

[0197] Description of Reference Numerals

[0198] 10 ...base material; 10A, 10B ...main surfaces; 100 ...glass article; 101 ...end surface; H, HA ...modified portion; L ...laser; LB ...width (pulse width); T ...imaginary line.

Claims

1. A method for manufacturing a glass article, in, include: forming a plurality of modified portions along an imaginary line set on a main surface of a base material by irradiating the base material with a pulsed laser along the imaginary line set on the main surface of the base material; and The base material is fractured starting from the modified portion along the imaginary line, and a portion is cut out from the base material to obtain a glass article. The minimum pulse interval of the laser light is greater than 1 μs, and the pulse width of the laser light is greater than or equal to 15 ps and less than or equal to 100 ps.

2. The method for manufacturing a glass article according to claim 1, wherein: There is the following relationship between the pitch P and the pulse width LB: P≦0.25×LB+3.5, Here, P is a value expressed in μm, and LB is a value expressed in ps.

3. The method for manufacturing a glass article according to claim 1 or 2, wherein: The pulse width of the laser light is greater than or equal to 15 ps and less than or equal to 60 ps.

4. The method for manufacturing a glass article according to claim 1 or 2, wherein: The wavelength of the laser light is a wavelength at which the base material becomes transparent.

5. The method for manufacturing a glass article according to claim 1 or 2, wherein: When viewed from a direction perpendicular to the main surface of the base material, a pitch between the plurality of modified parts is 1 μm or more and 23 μm or less.

6. The method for manufacturing a glass article according to claim 1 or 2, wherein: The energy of one pulse of the laser light is 200 μJ or more and 1500 μJ or less per 1 mm thickness of the base material.

7. The method for manufacturing a glass article according to claim 1 or 2, wherein: When viewed from a direction perpendicular to the main surface of the base material, a pitch between the plurality of modified portions in a section where the imaginary line is a curve is shorter than a pitch between the plurality of modified portions in a section where the imaginary line is a straight line.

8. The method for manufacturing a glass article according to claim 1 or 2, wherein: The modified portion is formed from the main surface of the base material to the opposite main surface.

9. The method for manufacturing a glass article according to claim 1 or 2, wherein: When a position which is 10% of the thickness of the glass article away from the first main surface on the opposite side to the second main surface is defined as the first position, A crack extending from the modified portion in a region from the first main surface to the first position has a length of 12 μm or less in a direction parallel to the main surface of the glass article and perpendicular to the imaginary line.

10. The method for manufacturing a glass article according to claim 1 or 2, wherein: The thickness of the base material is greater than 0.7 mm.

11. The method for manufacturing a glass article according to claim 1 or 2, wherein: The fracture toughness value K of the parent material IC 0.6 (MPa·m 0.5 )above.

12. The method for manufacturing a glass article according to claim 1 or 2, wherein: The thickness of the base material is less than 3 mm, and the plurality of modified portions are each formed by a single pulse irradiation.

13. The method for manufacturing a glass article according to claim 1 or 2, wherein: The optical system for irradiating the laser light is an aberration optical system.

14. A glass article having a main surface and an end surface, wherein: A plurality of linear modified portions extending in a thickness direction of the glass article are formed on the end surface, and the surface roughness Sa of the end surface as specified in ISO 25178 is 0.6 μm or less.

15. The glass article according to claim 14, wherein: When a position which is 10% of the thickness of the glass article away from the first main surface on the opposite side to the second main surface is defined as the first position, A crack extending from the modified portion in a region from the first main surface to the first position has a length of 12 μm or less in a direction orthogonal to the end surface.

16. The glass article according to claim 14 or 15, wherein: When a position on the end surface that is 10% away from the second main surface on the opposite side of the first main surface on one side by a distance of 10% of the thickness of the glass article is set as a first position, and a position on the end surface that is 10% away from the first main surface on the side of the second main surface by a distance of 10% of the thickness of the glass article is set as a second position, A crack extending from the modified portion in a region of the end surface from the first position to the second position has a length of 7 μm or less in a direction perpendicular to the end surface.

17. The glass article according to claim 14 or 15, wherein: When viewed from a direction perpendicular to the main surface, a pitch of the modified parts is 1 μm or more and 23 μm or less.

18. The glass article according to claim 14 or 15, wherein: When viewed from a direction perpendicular to the main surface, a pitch of the modified portions in a section where a line along the end surface is a curved line is shorter than a pitch of the modified portions in a section where the line along the end surface is a straight line.

19. The glass article according to claim 14 or 15, wherein: The thickness is 0.7 mm or more.

20. The glass article according to claim 14 or 15, wherein: Failure toughness value K IC 0.6 (MPa·m 0.5 )above.

Citation Information

Patent Citations

  • High speed laser processing of transparent materials

    CN104968620A

  • Laser processing of transparent materials

    CN110121398A

  • Method of laser processing transparent workpiece using curved quasi-non-diffracting laser beam

    CN114364484A

  • Dividing processing method of hard and brittle plate and apparatus for it

    JP2005271563A

  • Method for manufacturing glass article, and glass article

    JP2021088474A