Modified polyolefin aqueous dispersions
By grafting and copolymerizing α,β-unsaturated carboxylic anhydrides and amino compounds on polyolefins and adding alkaline compounds to form a modified polyolefin aqueous dispersion, the polyolefin resin was solved under the short-term baking conditions of low temperature and short-term baking. The problems of adhesion and peel strength achieve excellent adhesion and water resistance.
Patent Information
- Application Number
- CN202380030507.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-29
- Filing Date
- 2023-03-27
- Publication Date
- 2024-12-06
AI Technical Summary
The adhesion of the polyolefin resin is reduced under low temperature and short-term baking conditions, and the peel strength is insufficient, making it difficult to achieve effective coating, printing and bonding.
Develop a modified polyolefin aqueous dispersion, by grafting copolymerizing α,β-unsaturated carboxylic anhydride and an amino compound with active hydrogen on the polyolefin, and adding basic compounds to form a modified poly(carboxylic and amide group) The olefin aqueous dispersion optimizes its adhesion and water resistance under short baking at 80°C.
It achieves excellent adhesion, water resistance and high peel strength of polyolefin substrates under short baking conditions of 80°C. It is suitable for coatings, inks, adhesives and primers.
Smart Images

Figure BDA0005060240320000171 
Figure BDA0005060240320000201
Abstract
Description
Technical Field
[0001] The present invention relates to a modified polyolefin aqueous dispersion having excellent adhesion to a non-polar substrate even under low-temperature and short-time baking conditions. Background Art
[0002] Since polyolefin resins such as polypropylene have excellent properties and are inexpensive, they are widely used in automobile parts, various films, various molded products, etc. However, polyolefin resins are difficult to paint and bond because they are crystalline and have no polarity on the surface.
[0003] Therefore, in order to realize the coating, printing, film lamination or adhesion of polyolefin-based resins, modified polyolefins such as acid-modified polyolefins and acid-modified chlorinated polyolefins have been developed, among which aqueous dispersion compositions of modified polyolefins considering environmental and hygienic aspects have been proposed (for example, Patent Documents 1 and 2).
[0004] However, since aqueous dispersions require a large amount of heat to dry water, it is difficult to dissipate the heat to melt the resin, and compared with solvent-based systems, adhesion to the substrate is reduced when baked at low temperatures and for short times, resulting in insufficient peel strength. [Prior art literature] [Patent Literature]
[0005] [Patent Document 1] Japanese Patent Application Laid-Open No. 8-176374 [Patent Document 2] Japanese Patent Application Laid-Open No. 1-256549 Summary of the invention [Problems to be solved by the invention]
[0006] The present invention provides a modified polyolefin aqueous dispersion which exhibits excellent adhesion (adhesion), water resistance and high peel strength to a polyolefin substrate even under the conditions of baking at 80°C for a short time.
Methods to solve the problem
[0007] The present inventors have conducted intensive studies to solve the above problems and have completed the present invention. That is, the present invention has the following configurations. Item 1. A modified polyolefin aqueous dispersion having the following characteristics (I), (II) and (III). (I) The modified polyolefin (A) has a carboxyl group and an amide group. (II) The carboxyl group and the amide group of the modified polyolefin (A) are derived from an α,β-unsaturated carboxylic acid anhydride (B) and an amino compound (C) having an active hydrogen on nitrogen, and the amino compound (C) contains an aliphatic hydrocarbon group or an aromatic hydrocarbon group. (III) The modified polyolefin aqueous dispersion contains a basic compound (D). Item 2. The modified polyolefin aqueous dispersion according to Item 1, wherein the modified polyolefin (A) has a melting point of 85° C. or less as measured by differential scanning calorimetry. Item 3. A coating material for a polyolefin substrate, comprising the modified polyolefin aqueous dispersion according to Item 1 or 2. Item 4. An ink for a polyolefin substrate, comprising the modified polyolefin aqueous dispersion according to Item 1 or 2. Item 5. An adhesive for a polyolefin substrate, comprising the modified polyolefin aqueous dispersion according to Item 1 or 2. Item 6. A primer for a polyolefin substrate, comprising the modified polyolefin aqueous dispersion according to Item 1 or 2. [Effects of the invention]
[0008] Since the modified polyolefin aqueous dispersion of the present invention exhibits excellent adhesion (adhesion), water resistance and high peel strength to polyolefin-based substrates even under short-time baking conditions at 80°C, it can be suitably used in coatings, inks, adhesives, sealants or primers. DETAILED DESCRIPTION
[0009] The present invention is described in detail below.
[0010] The present invention is a modified polyolefin aqueous dispersion having the following characteristics (I), (II) and (III). (I) The modified polyolefin (A) has a carboxyl group and an amide group. (II) The carboxyl group and amide group of the modified polyolefin (A) are derived from an α,β-unsaturated carboxylic acid anhydride (B) and an amino compound (C) having an active hydrogen on nitrogen, wherein the amino compound (C) contains an aliphatic hydrocarbon group or an aromatic hydrocarbon group. (III) The modified polyolefin aqueous dispersion contains a basic compound (D).
[0011] <Modified polyolefin (A)> The modified polyolefin resin (A) used in the present invention is preferably obtained by graft-copolymerizing an α,β-unsaturated carboxylic acid anhydride (B) and an amino compound (C) having active hydrogen on nitrogen onto at least one polyolefin selected from the group consisting of polypropylene, propylene-α-olefin copolymers, polyethylene, ethylene-α-olefin copolymers, poly-1-butene and 1-butene-α-olefin copolymers.
[0012] Here, the propylene-α-olefin copolymer refers to a copolymer obtained by copolymerizing propylene with an α-olefin as the main component. As the α-olefin, for example, ethylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-decene, 1-dodecene, 1-hexadecene, 4-methyl-1-pentene and other α-olefins having 2 or 4 to 20 carbon atoms can be cited. The content of the propylene component in the propylene-α-olefin copolymer is preferably 50 mol% or more, and more preferably 70 mol% or more. When the content of the propylene component is 50 mol% or more, the adhesion to the polypropylene substrate becomes good.
[0013] Ethylene-α-olefin copolymer refers to a copolymer in which ethylene is copolymerized with α-olefin as the main component. As α-olefin, for example, propylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-decene, 1-dodecene, 1-hexadecene, 4-methyl-1-pentene and other α-olefins with 3 to 20 carbon atoms can be cited. The content of the ethylene component in the ethylene-α-olefin copolymer is preferably 75 mol% or more. When the content of the ethylene component is 75 mol% or more, the adhesion to the polyethylene substrate becomes good.
[0014] 1-Butene-α-olefin copolymer refers to a copolymer in which 1-butene is copolymerized with α-olefin as the main component. As α-olefin, for example, ethylene, propylene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-decene, 1-dodecene, 1-hexadecene, 4-methyl-1-pentene and other α-olefins having 2 to 3 or 5 to 20 carbon atoms can be cited. The content of 1-butene component in 1-butene-α-olefin copolymer is preferably 65 mol% or more. When the content of 1-butene component is 65 mol% or more, the adhesion to polypropylene substrates and poly-1-butene substrates becomes good.
[0015] The modified polyolefin (A) may also be further modified by chlorination. As the chlorinated polyolefin, an acid-modified chlorinated polyolefin obtained by chlorinating the above-mentioned modified polyolefin is preferred. When the modified polyolefin (A) is chlorinated, from the viewpoint of solution stability and adhesion between the polyolefin substrate and the resin substrate or the metal substrate, the lower limit of the chlorine content is preferably 5% by mass, more preferably 8% by mass or more, further preferably 10% by mass or more, particularly preferably 12% by mass or more, and most preferably 14% by mass or more. When it is 5% by mass or more, the solution stability becomes good and becomes easy to emulsify. The upper limit is preferably 40% by mass or less, more preferably 38% by mass or less, further preferably 35% by mass or less, particularly preferably 32% by mass or less, and most preferably 30% by mass or less. When it is 40% by mass or less, the crystallinity of the chlorinated polyolefin becomes high and the bonding strength tends to become stronger.
[0016] The chlorine content of the chlorinated polyolefin can be measured by titration in accordance with JIS K-7229-1995.
[0017] The melting point of the modified polyolefin (A) in the present invention based on a differential scanning calorimeter (hereinafter referred to as DSC) is preferably 50° C. to 85° C. More preferably, it is 55° C. to 80° C., and particularly preferably 60° C. to 75° C. When the melting point is 50° C. to 85° C., the film-forming property and cohesive force due to crystallization under baking conditions at 80° C. for a short time become appropriate, and the adhesion to the polyolefin substrate, water resistance, and peel strength become good.
[0018] The melting point determination based on DSC in the present invention can be determined according to JIS K7121-2012, for example, under the following conditions. Using a DSC measuring device (manufactured by Seiko Instruments), about 5 mg of a sample is kept in a heated melting state at 150°C for 10 minutes, then cooled at a rate of 10°C / min, and after being stably maintained at -50°C, the temperature is further raised to 150°C at 10°C / min, and the melting peak temperature during melting is measured, and the temperature is evaluated as the melting point. In addition, the melting points in the following examples are values measured under the aforementioned conditions.
[0019] <α,β-Unsaturated carboxylic acid anhydride (B)> The carboxyl group constituting the modified polyolefin (A) of the present invention is derived from an α,β-unsaturated carboxylic anhydride (B), and preferably has a structure in which the α,β-unsaturated carboxylic anhydride is graft-copolymerized on the polyolefin. Examples of the α,β-unsaturated carboxylic anhydride include maleic anhydride, citraconic anhydride, itaconic anhydride, aconitic anhydride, and nadic anhydride. Among them, maleic anhydride and itaconic anhydride are preferred.
[0020] When the polyolefin (a) and the α,β-unsaturated carboxylic acid anhydride (b) are polymerized, the content of the α,β-unsaturated carboxylic acid anhydride (b) is preferably 0.5 to 10% by mass relative to 100 parts by mass of the acid-modified polyolefin in which the α,β-unsaturated carboxylic acid anhydride (b) is modified by the polyolefin (a). It is more preferably 0.7% by mass or more. In addition, it is more preferably 3% by mass, and further preferably 2% by mass or less. When the content of the α,β-unsaturated carboxylic acid anhydride (b) is within this range, the phase inversion emulsification of the polyolefin resin (A) becomes easy, and the adhesion and peel strength of the coating film obtained from the aqueous resin composition containing the polyolefin resin (A) become good. When a polyolefin is polymerized with an α,β-unsaturated carboxylic acid anhydride (B), the content of the α,β-unsaturated carboxylic acid anhydride (B) component is preferably 0.5 to 10% by mass relative to 100 parts by mass of the modified polyolefin formed by modifying the polyolefin with the α,β-unsaturated carboxylic acid anhydride (B). It is more preferably 0.7% by mass or more. In addition, it is more preferably 3% by mass or less, and further preferably 2% by mass or less. When the content of the α,β-unsaturated carboxylic acid anhydride component is 0.5 to 10% by mass, phase inversion emulsification becomes easy, and the adhesion and peel strength of the coating film obtained from the aqueous dispersion become good.
[0021] As a method for graft-copolymerizing an α,β-unsaturated carboxylic acid anhydride (B) onto a polyolefin, there are known methods such as a method of heating and melting the polyolefin to a temperature above its melting point in the presence of a free radical initiator and reacting the polyolefin (melt method), and a method of dissolving the polyolefin in an organic solvent and then heating and stirring the polyolefin in the presence of a free radical initiator and reacting the polyolefin (solution method).
[0022] <Amino compound (C)> The amide group constituting the modified polyolefin (A) of the present invention is derived from the amino compound (C), and preferably a structure derived from the amino compound (C) is added to the carboxyl group constituting the modified polyolefin (A).
[0023] The content of the amino compound (C) in the modified polyolefin (A) is preferably 0.5 to 15% by mass. More preferably, it is 0.7% by mass or more. In addition, it is more preferably 12% by mass or less, and further preferably 10% by mass or less. When the content of the amino compound (C) is 0.5 to 15% by mass, the adhesion and phase transition emulsification to water can be improved in a well-balanced manner.
[0024] The amino compound (C) used in the present invention contains an aliphatic hydrocarbon group or an aromatic hydrocarbon group. In addition, it has active hydrogen on at least one nitrogen. For example, methylamine, dimethylamine, ethylamine, diethylamine, n-propylamine, di(n-propyl)amine, isopropylamine, diisopropylamine, n-butylamine, di(n-butyl)amine, n-hexylamine, di(n-hexyl)amine, n-octylamine, di(n-octyl)amine, di-2-ethylhexylamine, di(2-ethylhexyl)amine, cyclohexylamine, dicyclohexylamine, laurylamine, oleylamine, tallowamine, ditallowamine and other primary amines and secondary amines containing aliphatic hydrocarbon groups, or benzylamine, dibenzylamine and other primary amines and secondary amines containing aromatic hydrocarbon groups, and compounds such as amines containing heteroatoms such as morpholine can be cited.
[0025] The amino compound (C) has a hydrocarbon structure. The hydrocarbon group may be a linear, branched or cyclic alkyl group or an aromatic group. The number of carbon atoms in the hydrocarbon group is preferably 2 or more in one hydrocarbon group, and the upper limit is preferably 22 or less, and more preferably 20 or less. When the number of carbon atoms is 2 or more and 22 or less, the adhesion and phase transition emulsification to water can be improved in a better balance.
[0026] When the amino compound (C) does not contain a hydrophilic polymer, or when it contains a hydrophilic polymer, the ratio of the amino compound containing the hydrophilic polymer is preferably 10% by mass or less relative to the total amino compound (C) contained in the modified polyolefin (A). In this case, since the hydrophilic polymer has a high affinity for water, it is easy to emulsify by phase inversion. On the other hand, since the affinity with the non-polar substrate is reduced, the adhesion and water resistance are sometimes reduced. It is more preferably 5% by mass or less relative to the total amino compound (C) contained in the modified polyolefin (A), and further preferably 3% by mass or less.
[0027] The hydrophilic polymer in the present invention refers to a polymer having an insoluble content of 1 wt % or less when dissolved in water at 25° C. at a concentration of 10 wt %. The hydrophilic polymer is not particularly limited, and examples thereof include poly(meth)acrylic acid resins, polyether resins, polyvinyl alcohol resins, and polyvinyl pyrrolidone resins.
[0028] The amino compound (C) has 1 or 2 active hydrogen atoms on nitrogen, more preferably 1. When the number of active hydrogen atoms is 1 or 2, the formation of imide bonds in the reaction with the α,β-unsaturated carboxylic anhydride (B) is further suppressed, and phase inversion emulsification becomes easy.
[0029] When an amino compound (C) having two active hydrogen atoms is used, the formation of an imide bond can be suppressed by adopting a low reaction temperature. The reaction temperature is preferably 60°C to 100°C, more preferably 70°C to 80°C.
[0030] The carboxyl group and amide group of the modified polyolefin (A) are derived from an α,β-unsaturated carboxylic acid anhydride (B) and an amino compound (C) having active hydrogen on nitrogen. The modified polyolefin (A) is preferably a structure in which a structure derived from an α,β-unsaturated carboxylic acid anhydride (B) is grafted onto a polyolefin, and a structure derived from an amino compound (C) is added via the carboxyl group derived from the α,β-unsaturated carboxylic acid anhydride (B). It is believed that by having this structure, in the modified polyolefin (A), the structure derived from the amino compound has a higher affinity with a non-polar substrate than the dicarboxylic acid generated when the polyolefin is generally dispersed in water, and the adhesion and peel strength are further excellent.
[0031] The carboxyl group and amide group in the modified polyolefin (A) of the present invention can be confirmed by infrared absorption spectroscopy. First, the modified polyolefin (A) is dissolved in an organic solvent to obtain a solution. Then, the solution is coated on a KBr plate and dried to form a thin film. The infrared absorption spectrum of 400 to 4000 cm is observed by FT-IR (e.g., "FT / IR-4100", manufactured by JASCO Corporation). -1The infrared absorption spectrum of . The analysis is performed using the attached software (e.g., "Spectro Manager", JASCO Corporation). Wave numbers of 1600 to 1700 cm -1 The peaks in the spectrum are attributed to the C=O stretching vibration of the amide group, with wave numbers ranging from 1700 to 1750 cm -1 The peaks appearing in the figure are attributed to the C=O stretching vibration derived from the carboxyl group, and it can be confirmed that the C=O stretching vibration peak derived from the acid anhydride near the wave number 1780 cm-1 is reduced and disappears.
[0032] The weight average molecular weight of the modified polyolefin (A) is preferably 15,000 to 300,000, more preferably 30,000 to 150,000, further preferably 30,000 to 120,000, particularly preferably 50,000 to 120,000. When the weight average molecular weight is within the above range, the ease of phase inversion emulsification, adhesion and peel strength can be improved in a balanced manner.
[0033] The modified polyolefin (A) may be further graft-modified with a radical polymerizable monomer. That is, the modifying component may contain a radical polymerizable monomer in addition to the α,β-unsaturated carboxylic acid anhydride (B) and the amino compound (C).
[0034] As free radical polymerizable monomers, (meth)acrylic acid compounds and vinyl compounds can be cited. (Meth)acrylic acid compounds refer to compounds containing at least one (meth)acryloyl group (meaning acryloyl group and / or methacryloyl group) in the molecule. As examples of free radical polymerizable monomers, (meth)acrylic acid, methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, cyclohexyl (meth)acrylate, hydroxyethyl (meth)acrylate, isobornyl (meth)acrylate, glycidyl (meth)acrylate, octyl (meth)acrylate, lauryl (meth)acrylate, tridecyl (meth)acrylate, stearyl (meth)acrylate, benzyl (meth)acrylate, phenyl (meth)acrylate, dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, hydroxyethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, N,N-(meth)acrylate -dimethylaminoethyl, (meth) acetoacetoxyethyl acrylate, N-methyl (meth) acrylamide, N-ethyl (meth) acrylamide, N-propyl (meth) acrylamide, N-isopropyl (meth) acrylamide, N-butyl (meth) acrylamide, N-isobutyl (meth) acrylamide, N-tert-butyl (meth) acrylamide, N,N-dimethyl (meth) acrylamide, N,N-dimethylaminopropyl (meth) acrylamide, N,N-methylenebis (meth) acrylamide, N-hydroxymethyl (meth) acrylamide, hydroxyethyl (meth) acrylamide, (meth) acryloyl morpholine, vinyl n-butyl ether, 4-hydroxybutyl vinyl ether, dodecyl vinyl ether, etc. Among them, preferably (meth) methyl acrylate, (meth) ethyl acrylate, (meth) cyclohexyl acrylate, (meth) lauryl acrylate, wherein their methacrylate is more preferred. These can be used alone or in combination of two or more, and the mixing ratio can be freely set.
[0035] <Basic compound (D)> The modified polyolefin aqueous dispersion of the present invention contains a basic compound (D). Preferably, the modified polyolefin (A) is dispersed in water by neutralizing the carboxyl group of the modified polyolefin (A) with the basic compound (D). For example, when the modified polyolefin (A) is subjected to phase inversion emulsification, the basic compound is allowed to coexist with the modified polyolefin (A). By allowing the basic compound to exist in the system, the dispersibility of the modified polyolefin (A) can be improved. Examples of the basic compound (D) include inorganic basic compounds such as sodium hydroxide, potassium hydroxide, sodium carbonate, potassium carbonate, and ammonium carbonate; amines such as triethylamine, N,N-dimethylethanolamine, aminoethanolamine, N-methyl-N,N-diethanolamine, isopropylamine, iminobispropylamine, ethylamine, diethylamine, 3-ethoxypropylamine, 3-diethylaminopropylamine, sec-butylamine, propylamine, methylaminopropylamine, allylamine, diallylamine, methyliminobispropylamine, 3-methoxypropylamine, monoethanolamine, diethanolamine, triethanolamine, morpholine, N-methylmorpholine, N-ethylmorpholine, 2-amino-2-methyl-1-propanol, and 2-dimethylamino-2-methyl-1-propanol; and ammonia.
[0036] The content of the basic compound (D) is preferably 0.3 to 4.0 times the chemical equivalent of the carboxyl group of the modified polyolefin (A), and more preferably 0.7 to 2.5 times the chemical equivalent. When the amount added is less than 0.3 times the chemical equivalent, the effect of the basic compound may not be exhibited. On the other hand, when it is greater than 4.0 times the chemical equivalent, the residual amount in the dried product of the target application composition may become too much.
[0037] The basic compound (D) preferably contains 0.1 parts by mass or more, more preferably 0.3 parts by mass or more, and further preferably 0.5 parts by mass or more relative to 100 parts by mass of the modified polyolefin aqueous dispersion. In addition, it is more preferably 2 parts by mass or less, and further preferably 1 part by mass or less. In this case, the dispersibility of the modified polyolefin (A) can be improved, the particle size of the dispersed particles does not become too large, the storage stability becomes good, and the residual amount in the dried product also becomes appropriate.
[0038] <Method for producing modified polyolefin aqueous dispersion> The method for producing the modified polyolefin aqueous dispersion in the present invention is not particularly limited, but preferably comprises a phase inversion emulsification method in which the carboxyl groups in the modified polyolefin (A) are neutralized with a basic compound (D) in an organic solvent, an aqueous medium is added, heated and stirred, and after cooling, the organic solvent is removed.
[0039] From the viewpoint of the handling property of the aqueous dispersion, the solid content concentration of the aqueous dispersion of the resin composition in the present invention is preferably 10 to 60% by mass, more preferably 20 to 50% by mass, and still more preferably 30 to 40% by mass relative to the total amount of the aqueous dispersion. In this case, the stability of the modified polyolefin aqueous dispersion becomes good, and the adhesion to the olefin substrate also becomes good.
[0040] <Surfactant> The modified polyolefin aqueous dispersion of the present invention may further contain a surfactant within the range that does not impair the performance of the present invention. Examples of the surfactant include nonionic surfactants, anionic surfactants, cationic surfactants, and amphoteric surfactants. Among them, from the viewpoint of the particle size of the dispersed particles and the water resistance of the coating film obtained from the target composition, it is preferred to use a nonionic surfactant or anionic surfactant, and more preferably a nonionic surfactant.
[0041] As the nonionic surfactant, for example, polyoxyethylene alkyl ether, polyoxypropylene alkyl ether, polyoxyethylene alkylphenyl ether, polyoxypropylene alkylphenyl ether, polyoxyethylene styrenated phenyl ether, polyoxypropylene styrenated phenyl ether, polyoxyethylene fatty acid ester, polyoxypropylene fatty acid ester, polyoxyethylene sorbitan fatty acid ester, polyoxypropylene sorbitan fatty acid ester, polyoxyethylene alkylamine ether, polyoxypropylene alkylamine ether, polyoxyethylene lanolin alcohol ether, polyoxypropylene lanolin alcohol ether, polyoxyethylene lanolin fatty acid ester, polyoxypropylene lanolin fatty acid ester, (polyoxyethylene oxypropylene) block copolymer, etc. As an example thereof, EMULMIN series (manufactured by Sanyo Chemical Industries, Ltd.), NOIGEN series (manufactured by Daiichi Kogyo Seiyaku Co., Ltd.), BLAUNON series (manufactured by Aoki Oil & Fats Industries, Ltd.), etc. can be cited.
[0042] In addition, as these nonionic surfactants, reactive surfactants having polymerizable double bonds in the molecule may also be used, and examples thereof include ADEKA REASOAP ER-10, ER-20, ER-30, and ER-40 (all manufactured by ADEKA Corporation).
[0043] Examples of the anionic surfactant include higher alkyl sulfates, alkylaryl polyoxyethylene sulfate salts, higher fatty acid salts, alkylaryl sulfonates, alkyl phosphates, etc. Examples thereof include NEOCOL series and HITENOL series (manufactured by Daiichi Kogyo Seiyaku Co., Ltd.).
[0044] In addition, as these anionic surfactants, reactive surfactants having polymerizable double bonds in the molecule can be used. As one example thereof, ADEKA REASOAP NE-10, NE-20, NE-30, NE-40, SE-10N (above, manufactured by ADEKA Co., Ltd.), AQUALON RN-20, RN-30, RN-50, HS-10, HS-20 (above, manufactured by Daiichi Kogyo Seiyaku Co., Ltd.), ELEMINOL JS-2, ELEMINOL RS-30 (above, manufactured by Sanyo Chemical Industries, Ltd.), etc. can be cited.
[0045] The above surfactants may be used alone or in combination of two or more.
[0046] In the present invention, from the viewpoint of the ease of phase inversion emulsification and the water resistance of the coating film, the surfactant is preferably used in an amount of 5 to 60 parts by mass relative to 100 parts by mass of the modified polyolefin (A). It is more preferably 40 parts by mass or less, further preferably 30 parts by mass or less, and particularly preferably 25 parts by mass or less.
[0047] The Z average particle diameter of the resin particles in the modified polyolefin aqueous dispersion obtained as described above is preferably more than 10nm and less than 500nm, more preferably less than 200nm, and further preferably less than 150nm. In addition, more preferably more than 65nm, more preferably more than 70nm. When the average particle diameter is greater than 500nm, defects may occur in the coating film after coating, which has a negative impact on each physical property, and particularly becomes difficult to be used in topcoat coatings, thereby being not preferred.
[0048] The modified polyolefin aqueous dispersion of the present invention can be used directly as a clear varnish, but for the purpose of further improving the coating properties, such as film forming properties, coating hardness, weather resistance, flexibility, etc., various coating additives can be mixed to the extent that the adhesion to the polyolefin substrate is not impaired. For example, film-forming aids such as propylene glycol monopropyl ether, dipropylene glycol monomethyl ether, and dipropylene glycol butyl ether, defoamers, anti-sagging agents, wetting agents, ultraviolet absorbers, etc. can be used.
[0049] Further, the modified polyolefin aqueous dispersion of the present invention can also be appropriately added with an adhesive agent as needed, for example, rosin, dammar resin, polymerized rosin, hydrogenated rosin, rosin ester, rosin modified maleic acid resin, polyterpene resin, petroleum resin, cyclopentadiene resin, phenolic resin, xylene resin, coumarone indene resin and other aqueous dispersions, thereby improving the dryness of the coating film and the adhesion to the polyolefin substrate. As an added amount, it is preferably 5 to 100 parts by mass of solid content relative to 100 parts by mass of the solid content of the modified polyolefin aqueous dispersion, and more preferably 10 to 50 parts by mass. When the added amount is less than 5 parts by mass, there may be no added effect. On the other hand, when it is greater than 100 parts by mass, too much added amount may cause reduced adhesion.
[0050] The modified polyolefin aqueous dispersion of the present invention can be suitably used for coatings, inks, adhesives, sealants, primers, etc. for various polyolefin substrates headed by polypropylene, but is not limited to these substrates. For example, it can also be applied on other plastics, wood, metals, etc. As polyolefin substrates, films, sheets, molded bodies, etc. can be cited. There is no particular limitation on the coating method. [Example]
[0051] Next, the present invention will be specifically described by way of examples, but the present invention is not limited to the examples.
[0052] (1) Determination of weight average molecular weight by high temperature GPC The solvent was o-dichlorobenzene, and the measurement was performed at 140° C. using GPC150-C PLUS manufactured by Waters (column: GMH6-HT+GMH6-HTL manufactured by Tosoh Corporation). The weight average molecular weight was calculated using polystyrene having a known molecular weight as a standard substance.
[0053] (2) Determination of melting point using differential scanning calorimetry (DSC) According to JIS K7121-2012, using a DSC measuring apparatus (manufactured by Seiko Instruments Inc.), about 5 mg of a sample was kept in a heated melt state at 150°C for 10 minutes, then cooled at a rate of 10°C / min and stably maintained at -50°C, and then further heated to 150°C at a rate of 10°C / min, and the melting peak temperature during melting was measured, and this temperature was evaluated as the melting point.
[0054] (3) Measurement of Z-average particle size (hereinafter simply referred to as average particle size). The average particle size (Z average particle size) based on the intensity distribution was measured by dynamic light scattering using a "Zetasizer Nano-ZS Model ZEN3600" manufactured by Malvern. The sample having the solid content of the aqueous dispersion composition adjusted to a concentration of 0.05 g / L was measured three times at 25°C and the average value was taken.
[0055] Production Example 1 280g of propylene-α-olefin copolymer (propylene content = 70 mol%), 15g of maleic anhydride as α,β-unsaturated carboxylic anhydride (B), 7g of diisopropylbenzene peroxide and 420g of toluene were added to an autoclave with a stirrer, and after nitrogen substitution for about 5 minutes, the reaction was carried out at 140°C for 5 hours while heating and stirring. After the reaction was completed, the reaction solution was put into a large amount of methyl ethyl ketone to precipitate the resin. The resin was further washed several times with methyl ethyl ketone to remove unreacted maleic anhydride. The obtained resin was dried under reduced pressure to obtain a solid (PO-1) of an acid-modified polyolefin. According to the results of the infrared absorption spectrum, the content of the maleic anhydride component was 1.1% by mass. In addition, the weight average molecular weight measured based on high temperature GPC was 90,000, and the melting point based on DSC was 70°C.
[0056] Production Example 2 A solid acid-modified polyolefin (PO-2) was obtained by the same method as in Production Example 1 except that a propylene-α-olefin copolymer (propylene content = 80 mol%) was used as the raw material resin. The content of maleic anhydride component was 1.1% by mass according to the infrared absorption spectrum measurement results. In addition, the weight average molecular weight measured by high temperature GPC was 90,000, and the melting point by DSC was 82°C.
[0057] Production Example 3 A solid acid-modified polyolefin (PO-3) was obtained by the same method as in Production Example 1 except that a propylene-α-olefin copolymer (propylene content = 85 mol%) was used as the raw material resin. The content of maleic anhydride component was 1.1% by mass according to the results of infrared absorption spectrum measurement. In addition, the weight average molecular weight measured by high temperature GPC was 90,000, and the melting point by DSC was 90°C.
[0058] Production Example 4 280 g of propylene-α-olefin copolymer (propylene content = 94 mol%), 14 g of maleic anhydride as α,β-unsaturated carboxylic anhydride (B), 5.6 g of diisopropylbenzene peroxide and 420 g of toluene were added to an autoclave with a stirrer, and after nitrogen substitution for about 5 minutes, the reaction was carried out at 140°C for 5 hours while heating and stirring. After the reaction was completed, the reaction solution was put into a large amount of methyl ethyl ketone to precipitate the resin. The resin was further washed with methyl ethyl ketone several times to remove the unreacted maleic anhydride. After drying under reduced pressure, 280 g of the obtained maleic anhydride-modified polyolefin and 2520 g of chloroform were added to an autoclave with a stirrer, and after nitrogen substitution for about 5 minutes, it was heated to 110°C to fully dissolve the resin. Then, 1.4 g of tert-butyl peroxy-2-ethylhexanoate was added, and a specified amount of chlorine gas was blown in. Chloroform as a reaction solvent was removed by reduced pressure distillation and dried to obtain a solid acid-modified chlorinated polyolefin (CPO-1) having a chlorine content of 21% by mass, a weight average molecular weight of 80,000, a melting point of 70° C. based on DSC, and a maleic anhydride content of 1.5% by mass.
[0059] Example 1 (Production of modified polyolefin aqueous dispersion (a)) 100 g of the acid-modified polyolefin resin (PO-1) obtained in Production Example 1 and 60 g of toluene were added to an autoclave equipped with a stirrer, and after nitrogen substitution for about 5 minutes, the mixture was heated and dissolved at 100°C for 30 minutes. Then, 2.2 g of diethylamine was added as an amino compound (C), and the mixture was reacted at 110°C for 2 hours while heating and stirring. The reaction solution was temporarily cooled and a portion of the reaction solution was taken out. After separation and purification of the unreacted product, infrared absorption spectrum measurement was performed, and it was confirmed that the 1780 cm-1 peak derived from the acid anhydride was 1780 cm-1. -1 The spectrum near the amide group disappears, and the peaks from the carboxyl group are 1647 cm -1 、1718cm -1 . In addition, the weight average molecular weight of the modified polyolefin is 90,000, and the melting point based on DSC is 70°C. Then, in a nitrogen atmosphere, 20 g of polyoxyethylene hexadecyl ether (manufactured by NOF Corporation, trade name "NONION P-210", nonionic surfactant) and 60 g of isopropyl alcohol were added to the autoclave, and after heating and stirring at 90°C for 30 minutes, 500 g of warm ion exchange water was added at 90°C. After maintaining 90°C and stirring for 20 minutes, 2.5 g of N,N-dimethylethanolamine was added and stirred for 15 minutes. Then, heating and stirring were performed for 1 hour, and the emulsion was cooled to 60°C. By removing the solvent under reduced pressure, an aqueous dispersion (a) with a resin concentration (solid content) of 30% by mass and an average particle size of resin particles of 70 nm was obtained.
[0060] Example 2 (Production of modified polyolefin aqueous dispersion (b)) A modified polyolefin (weight average molecular weight 90,000, melting point 70°C based on DSC) was obtained by the same method as in Example 1 except that the types and amounts of each component were changed to the composition shown in Table 1. Furthermore, an aqueous dispersion (b) having a resin concentration (solid content) of 30% by mass and an average particle size of resin particles of 140 nm was obtained. In the infrared absorption spectrum measurement, a 1780 cm-1 chromatographic peak derived from anhydride was confirmed. -1 The spectrum near the amide group disappears, and the peaks from the amide group and the carboxyl group are 1645 cm -1 、1714cm -1 .
[0061] Example 3 (Production of modified polyolefin aqueous dispersion (c)) A modified polyolefin (weight average molecular weight 90,000, melting point 70°C based on DSC) was obtained by the same method as in Example 1 except that the types and amounts of each component were changed to the composition shown in Table 1. Furthermore, an aqueous dispersion (c) having a resin concentration (solid content) of 30% by mass and an average particle size of resin particles of 95 nm was obtained. In the infrared absorption spectrum measurement, it was confirmed that the 1780 cm-1 peak from the acid anhydride -1 The spectrum near the amide group disappears, and the peaks from the amide group and the carboxyl group are 1655 cm -1 、1703cm -1 .
[0062] Example 4 (Production of modified polyolefin aqueous dispersion (d)) A modified polyolefin (weight average molecular weight 90,000, melting point 70°C based on DSC) was obtained by the same method as in Example 1 except that the type, amount and reaction temperature of each component were changed to the composition shown in Table 1. Furthermore, an aqueous dispersion (d) having a resin concentration (solid content) of 30% by mass and an average particle size of resin particles of 105 nm was obtained. In the infrared absorption spectrum measurement, it was confirmed that the 1780 cm-1 peak from the acid anhydride -1 The spectrum near the amide group disappears, and the peaks from the amide group and the carboxyl group are 1643 cm -1 、1708cm -1 .
[0063] Example 5 (Production of modified polyolefin aqueous dispersion (e)) A modified polyolefin (weight average molecular weight 90,000, melting point 82°C based on DSC) was obtained by the same method as in Example 1 except that the types and amounts of each component were changed to the composition shown in Table 1. Furthermore, an aqueous dispersion (e) having a resin concentration (solid content) of 30% by mass and an average particle size of resin particles of 105 nm was obtained. In the infrared absorption spectrum measurement, a 1780 cm-1 chromatographic peak derived from anhydride was confirmed. -1The spectrum near the amide group disappears, and the peaks from the amide group and the carboxyl group are 1645 cm -1 、1714cm -1 .
[0064] Example 6 (Production of modified polyolefin aqueous dispersion (f)) A modified polyolefin (weight average molecular weight 80,000, melting point 70°C based on DSC) was obtained by the same method as in Example 1 except that the type, amount and reaction temperature of each component were changed to the composition shown in Table 1. Furthermore, an aqueous dispersion (f) having a resin concentration (solid content) of 30% by mass and an average particle size of resin particles of 110 nm was obtained. In the infrared absorption spectrum measurement, a 1780 cm-1 chromatographic peak derived from anhydride was confirmed. -1 The spectrum near the amide group disappears, and the peaks from the amide group and the carboxyl group are 1645 cm -1 、1714cm -1 .
[0065] Comparative Example 1 (Production of Modified Polyolefin Aqueous Dispersion (g)) 100 g of the acid-modified polyolefin obtained in Preparation Example 1, 60 g of toluene, 60 g of isopropyl alcohol and 20 g of polyoxyethylene cetyl ether (manufactured by NOF Corporation, trade name "NONION P-210", nonionic surfactant) were added to a 2L four-necked flask equipped with a cooler, a thermometer, a stirrer and a dropping funnel, and the mixture was fully dissolved while being kept at 100°C. 4.0 g of N,N-dimethylethanolamine was added to the solution and stirred for 15 minutes. Then, 500 g of deionized water preheated to 90°C was added dropwise from the dropping funnel over 30 minutes under vigorous stirring to emulsify the acid-modified polyolefin by phase inversion. The emulsion was cooled to 60°C and desolventized under reduced pressure to obtain an aqueous dispersion (g) having a resin concentration (solid content) of 30% by mass and an average particle size of resin particles of 65 nm.
[0066] Comparative Example 2 (Production of Modified Polyolefin Aqueous Dispersion (h)) Except having changed the kind of each component into the composition of Table 1, the same method as Comparative Example 1 was carried out to obtain a water dispersion (h) having a resin concentration (solid content) of 30 mass % and an average particle diameter of resin particles of 45 nm.
[0067] Comparative Example 3 (Production of modified polyolefin aqueous dispersion (i)) A modified polyolefin (weight average molecular weight 90,000, melting point 90°C based on DSC) was obtained by the same method as in Example 1 except that the types and amounts of each component were changed to the composition shown in Table 1. Furthermore, an aqueous resin composition (i) having a resin concentration (solid content) of 30% by mass and an average particle size of resin particles of 85 nm was obtained. In the infrared absorption spectrum measurement, a 1780 cm-1 chromatogram derived from anhydride was confirmed. -1 The spectrum near the amide group disappears, and the peaks from the amide group and the carboxyl group are 1645 cm -1 、1714cm -1 In addition, JEFFAMINE (registered trademark) M-1000 (manufactured by HUNTSMAN) is an amino compound containing a hydrophilic polymer.
[0068] Comparative Example 4 (Production of modified polyolefin aqueous dispersion (j)) The same method as in Example 1 was used except that the types, amounts and reaction temperatures of the components were changed as shown in Table 1. However, an aqueous dispersion could not be obtained due to poor emulsification. In the infrared absorption spectrum measurement, a 1780 cm -1 The spectrum near 1720cm disappears, which is from the imine group -1 On the other hand, peaks derived from carboxyl groups and amide groups could not be confirmed.
[0069]
Table 1
[0070] The modified polyolefin aqueous dispersions (a) to (j) obtained in Examples 1 to 6 and Comparative Examples 1 to 4 were used to evaluate the following properties.
[0071] (1) Adhesion 2 g of propylene glycol monomethyl ether as a film-forming aid and 2 g of "DYNOL604" (manufactured by Air Products Japan Co., Ltd.) as a wetting agent were added to 100 g of modified polyolefin aqueous dispersion, and stirred with a magnetic stirrer for 30 minutes. The emulsion was sprayed on a polypropylene plate (manufactured by Japan Test Panel Co., Ltd.) cleaned with isopropyl alcohol in a dry coating thickness of 10 μm. After drying at 80°C for 5 minutes, 2K polyurethane coating (manufactured by Kansai Paint Co., Ltd., RETANPG White III) was sprayed as a protective film in a manner to make it 40 to 50 μm. After drying at 80°C for 5 minutes, it was placed in an atmosphere of 25°C and 60% relative humidity for 24 hours and used as a test plate. 100 grids were drawn on the test plate at intervals of 1 mm up to the base, and a cellophane tape was crimped on it and torn off at an angle of 90 degrees relative to the coating surface. Repeated 3 times, the case of no peeling was evaluated as A, the case of peeling at the third time was evaluated as B, and the case of peeling at the second time was evaluated as C.
[0072] (2) Water resistance After the test plate obtained by the method of (1) above was immersed in warm water at 40°C for 240 hours, the adhesiveness was evaluated by the same method as (1) above. In addition, the occurrence of blistering (peeling or blistering of the coating film) was confirmed from the appearance of the coating film. The case of no peeling or blistering was evaluated as A, the case of no peeling but blistering was evaluated as B, and the case of peeling was evaluated as C.
[0073] (3) Peel strength After preparing a test plate in the same manner as in the method (1) above, except that the protective film was spray-coated to a thickness of 100 μm, the test plate was placed in an atmosphere of 25° C. and a relative humidity of 60% for 48 hours to prepare a test plate. Strips of peeling pieces were prepared on the test plate at intervals of 1 cm, and a 50 mm, 180° peeling test was performed at a speed of 50 mm / min using a tensile testing machine (TENSILON RTG-1310 manufactured by A&D Corporation). The stress during the stretching was taken as the peel strength, and the average value of the five tests was taken as the measurement result. The evaluation results of the peel strength are as follows. A: 800gf / cm or more, B: 600gf / cm or more, less than 800gf / cm, C: 500gf / cm or more, less than 600gf / cm, D: less than 500gf / cm
[0074]
Table 2
[0075] [Review of the results of Table 1 and Table 2] As can be seen from Tables 1 and 2, the aqueous resin compositions (a) to (f) obtained in Examples 1 to 6 above showed high peel strength under the conditions of 80°C and short-time baking, and also had excellent adhesion and water resistance. In contrast, in Comparative Examples 1 and 2, where the modified polyolefin (A) did not have an amide group, the peel strength was reduced and the adhesion and water resistance to the polyolefin substrate were poor, and in Comparative Example 4, where the modified polyolefin (A) did not have a carboxyl group, the emulsification was impossible.
Claims
1. A modified polyolefin aqueous dispersion, characterized in that: Having the following characteristics (I), (II) and (III): (I) The modified polyolefin (A) has a carboxyl group and an amide group, (II) the carboxyl group and the amide group of the modified polyolefin (A) are derived from an α,β-unsaturated carboxylic acid anhydride (B) and an amino compound (C) having an active hydrogen on nitrogen, wherein the amino compound (C) contains an aliphatic hydrocarbon group or an aromatic hydrocarbon group, (III) The modified polyolefin aqueous dispersion contains a basic compound (D).
2. The modified polyolefin aqueous dispersion according to claim 1, characterized in that: The modified polyolefin (A) has a melting point of 85° C. or less as measured by differential scanning calorimetry.
3. A coating for a polyolefin substrate, characterized in that: A modified polyolefin aqueous dispersion comprising the modified polyolefin aqueous dispersion according to claim 1 or 2.
4. An ink for a polyolefin substrate, characterized in that: A modified polyolefin aqueous dispersion comprising the modified polyolefin aqueous dispersion according to claim 1 or 2.
5. An adhesive for a polyolefin substrate, characterized in that: A modified polyolefin aqueous dispersion comprising the modified polyolefin aqueous dispersion according to claim 1 or 2.
6. A primer for a polyolefin substrate, characterized in that: A modified polyolefin aqueous dispersion comprising the modified polyolefin aqueous dispersion according to claim 1 or 2.
Citation Information
Patent Citations
Aqueous dispersion of modified polyolefin
JP1989256549A
Amorphous polyolefin emulsion
JP1996176374A