NiCrFe alloy material

By adding calcium and boron to the NiCrFe alloy material and meeting the specific element content relationship, the problem of welding cracks during welding is solved, and the weldability and corrosion resistance of the material are improved.

CN119095991APending Publication Date: 2024-12-06NIPPON STEEL CORPORATION
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380030258.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-30
Filing Date
2023-03-28
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Although the existing NiCrFe alloy materials have excellent corrosion resistance in petroleum and gas primary treatment equipment and chemical equipment, they are prone to welding cracks, especially deplastic cracks and liquefied cracks, which affect their welding properties.

Method used

By optimizing the chemical composition of NiCrFe alloy material, 0.0002-0.0040% calcium (Ca) and 0.0001-0.0050% boron (B) are added, and the specific element content relationship formula (8.5×Mn+19.5×Ni-12.43×Cr is satisfied. -42.4×Mo-10250×Ca+1250×B-74.3776<6.5) to suppress the generation of deplastic cracks and liquefied cracks.

Benefits of technology

It realizes that NiCrFe alloy material suppresses the generation of deplastic cracks and liquefied cracks during welding, improves its weldability, and maintains excellent corrosion resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119095991A_ABST
    Figure CN119095991A_ABST
Patent Text Reader

Abstract

Provided is a NiCrFe alloy material having excellent corrosion resistance and excellent weldability. The NiCrFe alloy material according to the present disclosure has a chemical composition of C: 0.002 to 0.030% by mass, Si: 0.05 to 0.50% by mass, Mn: 0.10 to 1.50% by mass, P: 0.050% or less, S: 0.0200% or less, Ni: 29.0 to 40.0% by mass, Cr: 24.00 to 30.00% by mass, Mo: 5.0 to 7.5% by mass, N: 0.20 to 0.40% by mass, Al: 0.50% or less, Ca: 0.0002 to 0.0040% by mass, and B: 0.0001 to 0.0050% by mass, with the balance being Fe and impurities, and satisfies formula (1). 0, 0, 0, 0; 8.5 * Mn + 19.5 * Ni-12.43 * Cr-42. 4 * Mo-10250 * Ca + 1250 * B-74.3776 lt, and the number of the components is larger than that of the components. 6.5 (1) Here, the corresponding element content is substituted in mass% at the element symbol in formula (1).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to NiCrFe alloy materials. Background Art

[0002] In equipment such as primary processing equipment and chemical equipment for oil and gas, the alloy materials used are in contact with process fluids containing sulfides and / or chlorides. Therefore, excellent corrosion resistance is required for the alloy materials used in these equipment. As materials requiring excellent corrosion resistance, there are, for example, 18-8 series stainless steel materials such as SUS304H, SUS316H, SUS321H, SUS347H, and NiCrFe alloy materials represented by Alloy800H, which is specified as NCF800H in the JIS standard. NiCrFe alloy materials have excellent corrosion resistance compared with 18-8 series stainless steel materials. NiCrFe alloy materials are also more economical than Ni-based alloy materials represented by Alloy617. Therefore, as an alloy material with excellent corrosion resistance, NiCrFe alloy materials are sometimes used.

[0003] Japanese Patent Application Laid-Open No. 2-217445 (Patent Document 1) and International Publication No. 2015 / 072458 (Patent Document 2) propose alloy materials having excellent corrosion resistance.

[0004] The alloy material described in Patent Document 1 is a Fe-Cr-Ni alloy, containing Ni: 27-32%, Cr: 24-28%, Cu: 1.25-3.0%, Mo: 1.0-3.0%, Si: 1.5-2.75%, Mn: 1.0-2.0%, limited to N: 0.015% or less, B: 0.10% or less, V: 0.10% or less, C: 0.10% or less, Al: 0.30% or less, P: 0.03% or less, S: 0.02% or less, and the balance is substantially composed of Fe and impurities. Patent Document 1 records that the alloy material has high strength, wear and seizure resistance and corrosion resistance under stress.

[0005] The alloy material described in Patent Document 2 is a Ni-Cr alloy material having the following chemical composition: in terms of mass%, Si: 0.01% to 0.5%, Mn: 0.01% to 1.0%, Cu: 0.01% to 1.0%, Ni: 48% to 55%, Cr: 22% to 28%, Mo: 5.6% to 7.0%, N: 0.04% to 0.16%, sol.Al: 0.03% to 0.20%, RE M: 0.01 to 0.074%, W: 0 to 8.0%, Co: 0 to 2.0%, one or more of Ca and Mg: 0.003 to 0.01% in total, one or more of Ti, Nb, Zr and V: 0 to 0.5% in total, the remainder is Fe and impurities, among the impurities, C: 0.03% or less, P: 0.03% or less, S: 0.001% or less, and O: 0.01% or less, the dislocation density ρ satisfies the formula (7.0×10 15 ≤ρ≤2.7×10 16 -2.67×10 17 ×[REM(%)]). Patent Document 2 states that the alloy material has excellent hot workability and toughness, and also has excellent corrosion resistance (stress corrosion cracking resistance at high temperatures exceeding 200°C and in an environment containing hydrogen sulfide), and a yield strength (0.2% yield strength) of 965 MPa or more.

[0006] Prior art literature

[0007] Patent Literature

[0008] Patent Document 1: Japanese Patent Application Laid-Open No. 2-217445

[0009] Patent Document 2: International Publication No. 2015 / 072458 Summary of the invention

[0010] Problem that the invention aims to solve

[0011] As described above, the alloy materials having excellent corrosion resistance are disclosed in Patent Documents 1 and 2. However, it is also possible to obtain NiCrFe alloy materials having excellent corrosion resistance by techniques other than those disclosed in Patent Documents 1 and 2.

[0012] However, in the construction and repair of equipment such as primary processing equipment for oil and gas, chemical equipment, etc., NiCrFe alloy materials are sometimes welded. Therefore, NiCrFe alloy materials used in equipment such as primary processing equipment for oil and gas, chemical equipment, etc. require not only excellent corrosion resistance but also excellent weldability. Here, excellent weldability means that welding cracks (cracks generated near the weld) are not easily generated. On the other hand, in the above-mentioned patent documents 1 and 2, the weldability of the alloy material is not studied.

[0013] An object of the present disclosure is to provide a NiCrFe alloy material having excellent corrosion resistance and excellent weldability.

[0014] Solutions for solving problems

[0015] The NiCrFe alloy material disclosed in the present invention has the following chemical composition:

[0016] Contains by mass%

[0017] C: 0.002~0.030%,

[0018] Si: 0.05-0.50%,

[0019] Mn: 0.10~1.50%,

[0020] P: 0.050% or less,

[0021] S: 0.0200% or less,

[0022] Ni: 29.0-40.0%,

[0023] Cr: 24.00~30.00%,

[0024] Mo: 5.0~7.5%,

[0025] N: 0.20~0.40%,

[0026] Al: 0.50% or less,

[0027] Ca: 0.0002-0.0040%, and

[0028] B: 0.0001~0.0050%,

[0029] Balance: Fe and impurities,

[0030] And satisfying formula (1),

[0031] 0.0<8.5×Mn+19.5×Ni-12.43×Cr-42.4×Mo-10250×Ca+1250×B-74.3776<6.5(1)

[0032] In the formula (1), the content of the corresponding element is substituted in mass % at the element symbol.

[0033] The NiCrFe alloy material disclosed in the present invention has the following chemical composition:

[0034] Contains by mass%

[0035] C: 0.002~0.030%,

[0036] Si: 0.05-0.50%,

[0037] Mn: 0.10~1.50%,

[0038] P: 0.050% or less,

[0039] S: 0.0200% or less,

[0040] Ni: 29.0-40.0%,

[0041] Cr: 24.00~30.00%,

[0042] Mo: 5.0~7.5%,

[0043] N: 0.20~0.40%,

[0044] Al: 0.50% or less,

[0045] Ca: 0.0002-0.0040%, and

[0046] B: 0.0001~0.0050%,

[0047] Also contains the freedom to choose

[0048] Cu: 0.40% or less,

[0049] W: 1.00% or less,

[0050] Sn: 0.50% or less,

[0051] Co: 0.50% or less,

[0052] V: 0.50% or less,

[0053] Nb: 0.50% or less,

[0054] Ti: 0.50% or less,

[0055] Zr: 0.200% or less,

[0056] Hf: 0.200% or less,

[0057] Ta: 0.50% or less, and

[0058] Rare earth elements: 0.0030% or less of one or more elements in the group consisting of

[0059] Balance: Fe and impurities,

[0060] And satisfying formula (1),

[0061] 0.0<8.5×Mn+19.5×Ni-12.43×Cr-42.4×Mo-10250×Ca+1250×B-74.3776<6.5 (1)

[0063] In the formula (1), the content of the corresponding element is substituted in mass % at the element symbol.

[0064] Effects of the Invention

[0065] The NiCrFe alloy material disclosed in the present invention has excellent corrosion resistance and excellent weldability. BRIEF DESCRIPTION OF THE DRAWINGS

[0066] Figure 1 This is a graph showing the relationship between the value of D (=8.5×Mn+19.5×Ni-12.43×Cr-42.4×Mo-10250×Ca+1250×B-74.3776) and the total length (mm) of the loss cracks in this example. DETAILED DESCRIPTION

[0067] First, the inventors studied the corrosion resistance of NiCrFe alloy materials from the perspective of chemical composition. As a result, the inventors believed that if the alloy contains C: 0.002-0.030%, Si: 0.05-0.50%, Mn: 0.10-1.50%, P: 0.050% or less, S: 0.0200% or less, Ni: 29.0-40.0%, Cr: 24.00-30.00%, Mo: 5.0-7.5%, N: 0.20-0.40%, Al: 0.50% or less, and Ni: 29.0-40.0%, Cr: 24.00-30.00%, Mo: 5.0-7.5%, N: 0.20-0.40%, Al: 0.50% or less, the corrosion resistance of NiCrFe alloy materials is better than that of NiCrFe alloy materials. % or less, Cu: 0-0.40%, W: 0-1.00%, Sn: 0-0.50%, Co: 0-0.50%, V: 0-0.50%, Nb: 0-0.50%, Ti: 0-0.50%, Zr: 0-0.200%, Hf: 0-0.200%, Ta: 0-0.50% and rare earth elements: 0-0.0030%, it is possible to improve the corrosion resistance of NiCrFe alloy materials.

[0068] Here, for the NiCrFe alloy material having the above chemical composition, welding cracks may sometimes occur when welding is performed. Specifically, for the NiCrFe alloy material having the above chemical composition, it is known through detailed research by the inventors that loss of plastic cracks are easily generated in welding cracks. Loss of plastic cracks are a type of welding cracks, which refers to the grain boundaries exposed to high temperatures caused by welding, resulting in reduced ductility and being unable to withstand thermal contraction caused by cooling and breaking. That is, if the grain boundaries of the NiCrFe alloy material having the above chemical composition can be strengthened, it is possible to suppress the generation of loss of plastic cracks.

[0069] Therefore, the present inventors have focused on calcium (Ca) and conducted research on the suppression of loss cracking. Specifically, for alloy materials having the above chemical composition, when welding is performed, sulfur (S) may segregate at the grain boundaries in the heat affected zone (hereinafter referred to as HAZ (Heat Affected Zone)) of the weld. If S segregates at the grain boundaries, the cohesive force of the grain boundaries decreases, and it may not be able to withstand the thermal shrinkage caused by cooling and break. In this way, the present inventors believe that the alloy materials having the above chemical composition will produce loss cracking. That is, the present inventors believe that if in addition to the above chemical composition, 0.0002 to 0.0040% Ca is contained, the S in the alloy material is fixed in the form of CaS, which may be able to suppress the loss cracking of the alloy material.

[0070] On the other hand, even alloy materials containing 0.0002 to 0.0040% Ca in addition to the above chemical composition may also cause welding cracks. Specifically, for alloy materials containing 0.0002 to 0.0040% Ca in addition to the above chemical composition, liquefaction cracks may occur in welding cracks. Liquefaction cracks are a type of welding cracks, which refer to ruptures caused by localized melting in the HAZ close to the fusion line.

[0071] Therefore, the inventors of the present invention have focused on boron (B) and studied the suppression of liquefaction cracking. Specifically, B strengthens the grain boundaries at high temperatures and suppresses liquefaction cracking. On the other hand, if the B content is too high, B segregates at the grain boundaries and melts in the high-temperature region near the melting line, which in turn promotes liquefaction cracking. That is, by containing 0.0001 to 0.0050% of B and 0.0002 to 0.0040% of Ca in addition to the above chemical composition, the occurrence of both loss of plasticity cracking and liquefaction cracking can be suppressed, and it is possible to improve the weldability of the alloy material.

[0072] That is, the present inventors believe that if, in terms of mass%, C: 0.002-0.030%, Si: 0.05-0.50%, Mn: 0.10-1.50%, P: 0.050% or less, S: 0.0200% or less, Ni: 29.0-40.0%, Cr: 24.00-30.00%, Mo: 5.0-7.5%, N: 0.20-0.40%, Al: 0.50% or less, Ca: 0.0002-0.0040%, B: 0.00 01~0.0050%, Cu: 0~0.40%, W: 0~1.00%, Sn: 0~0.50%, Co: 0~0.50%, V: 0~0.50%, Nb: 0~0.50%, Ti: 0~0.50%, Zr: 0~0.200%, Hf: 0~0.200%, Ta: 0~0.50%, rare earth elements: 0~0.0030%, and the balance is Fe and impurities. NiCrFe alloy material may be able to achieve both corrosion resistance and weldability.

[0073] The inventors of the present invention manufactured various NiCrFe alloy materials having the above chemical composition and further studied the generation of welding cracks in detail. As a result, the inventors of the present invention found that the NiCrFe alloy material having the above chemical composition, by satisfying the following formula (1), not only has excellent corrosion resistance, but also can suppress the generation of both loss cracking and liquefaction cracking.

[0074] 0.0<8.5×Mn+19.5×Ni-12.43×Cr-42.4×Mo-10250×Ca+1250×B-74.3776<6.5 (1)

[0076] Here, the content of the corresponding element is substituted in mass % at the element symbol in formula (1).

[0077] Defined as D = 8.5×Mn+19.5×Ni-12.43×Cr-42.4×Mo-10250×Ca+1250×B-74.3776. Figure 1 This is a graph showing the relationship between the value of D and the total length (mm) of the loss cracks in this example. Figure 1 It is made for the examples satisfying the above chemical composition in the examples described later, using the value of D and the total length of the plastic loss crack (mm). It should be noted that the total length of the plastic loss crack (mm) is obtained by the method described later. In addition, Figure 1 In all the examples described in, the occurrence of liquefaction cracks was not confirmed, and the steel had excellent corrosion resistance.

[0078] Reference Figure 1For the alloy material satisfying the above chemical composition, when D is less than 0.0, although the generation of liquefaction cracks can be suppressed, the total length of loss cracks is more than 4.0 mm, and the generation of loss cracks cannot be suppressed. Figure 1 , and for the alloy material satisfying the above chemical composition, when D is 6.5 or more, although the generation of liquefaction cracks can be suppressed, the total length of loss cracks is 4.0 mm or more, and the generation of loss cracks cannot be suppressed. That is, for the alloy material satisfying the above chemical composition, if D is greater than 0.0 and less than 6.5, it has excellent corrosion resistance, and the generation of both liquefaction cracks and loss cracks can be suppressed.

[0079] Therefore, the NiCrFe alloy material of the present embodiment has the above-mentioned chemical composition, and D is set to be greater than 0.0 and less than 6.5. As a result, the NiCrFe alloy material of the present embodiment can achieve both excellent corrosion resistance and excellent weldability.

[0080] The gist of the NiCrFe alloy material of the present embodiment completed based on the above findings is as follows. [1]

[0082] A NiCrFe alloy material having the following chemical composition:

[0083] Contains by mass%

[0084] C: 0.002~0.030%,

[0085] Si: 0.05-0.50%,

[0086] Mn: 0.10~1.50%,

[0087] P: 0.050% or less,

[0088] S: 0.0200% or less,

[0089] Ni: 29.0-40.0%,

[0090] Cr: 24.00~30.00%,

[0091] Mo: 5.0~7.5%,

[0092] N: 0.20~0.40%,

[0093] Al: 0.50% or less,

[0094] Ca: 0.0002-0.0040%, and

[0095] B: 0.0001~0.0050%,

[0096] Balance: Fe and impurities,

[0097] And it satisfies formula (1).

[0098] 0.0<8.5×Mn+19.5×Ni-12.43×Cr-42.4×Mo-10250×Ca+1250×B-74.3776<6.5(1)

[0099] In the formula (1), the content of the corresponding element is substituted in mass % at the element symbol. [2]

[0101] A NiCrFe alloy material having the following chemical composition:

[0102] Contains by mass%

[0103] C: 0.002~0.030%,

[0104] Si: 0.05-0.50%,

[0105] Mn: 0.10~1.50%,

[0106] P: 0.050% or less,

[0107] S: 0.0200% or less,

[0108] Ni: 29.0-40.0%,

[0109] Cr: 24.00~30.00%,

[0110] Mo: 5.0~7.5%,

[0111] N: 0.20~0.40%,

[0112] Al: 0.50% or less,

[0113] Ca: 0.0002-0.0040%, and

[0114] B: 0.0001~0.0050%,

[0115] Also contains the freedom to choose

[0116] Cu: 0.40% or less,

[0117] W: 1.00% or less,

[0118] Sn: 0.50% or less,

[0119] Co: 0.50% or less,

[0120] V: 0.50% or less,

[0121] Nb: 0.50% or less,

[0122] Ti: 0.50% or less,

[0123] Zr: 0.200% or less,

[0124] Hf: 0.200% or less,

[0125] Ta: 0.50% or less, and

[0126] Rare earth elements: 0.0030% or less of one or more elements in the group consisting of

[0127] Balance: Fe and impurities,

[0128] And it satisfies formula (1).

[0129] 0.0<8.5×Mn+19.5×Ni-12.43×Cr-42.4×Mo-10250×Ca+1250×B-74.3776<6.5 (1)

[0131] In the formula (1), the content of the corresponding element is substituted in mass % at the element symbol. [3]

[0133] The NiCrFe alloy material according to [2], wherein the chemical composition contains a selected

[0134] Cu: 0.40% or less,

[0135] W: 1.00% or less,

[0136] Sn: 0.50% or less, and

[0137] Co: One or more elements selected from the group consisting of 0.50% or less. [4]

[0139] The NiCrFe alloy material according to [2], wherein the chemical composition contains a selected

[0140] V: 0.50% or less,

[0141] Nb: 0.50% or less,

[0142] Ti: 0.50% or less,

[0143] Zr: 0.200% or less,

[0144] Hf: 0.200% or less, and

[0145] Ta: One or more elements selected from the group consisting of 0.50% or less. [5]

[0147] The NiCrFe alloy material according to [2], wherein the chemical composition contains rare earth elements: 0.0030% or less.

[0148] The gist of the NiCrFe alloy material of the present embodiment can also be described as follows.

[0149] [1] A NiCrFe alloy material, which is

[0150] C: 0.002~0.030%,

[0151] Si: 0.05-0.50%,

[0152] Mn: 0.10~1.50%,

[0153] P: 0.050% or less,

[0154] S: 0.0200% or less,

[0155] Ni: 29.0-40.0%,

[0156] Cr: 24.00~30.00%,

[0157] Mo: 5.0~7.5%,

[0158] N: 0.20~0.40%,

[0159] Al: 0.50% or less,

[0160] Ca: 0.0002~0.0040%,

[0161] B: 0.0001~0.0050%,

[0162] Cu: 0-0.40%,

[0163] W: 0~1.00%,

[0164] Sn: 0~0.50%,

[0165] Co: 0-0.50%,

[0166] V: 0~0.50%,

[0167] Nb: 0-0.50%,

[0168] Ti: 0-0.50%,

[0169] Zr: 0~0.200%,

[0170] Hf: 0~0.200%,

[0171] Ta: 0~0.50%,

[0172] Rare earth elements: 0 to 0.0030%, and

[0173] Balance: Fe and impurities,

[0174] And it satisfies formula (1).

[0175] 0.0<8.5×Mn+19.5×Ni-12.43×Cr-42.4×Mo-10250×Ca+1250×B-74.3776<6.5(1)

[0176] In the formula (1), the content of the corresponding element is substituted in mass % at the element symbol. [2]

[0178] The NiCrFe alloy material according to [1] contains

[0179] Cu: 0.01~0.40%,

[0180] W: 0.01~1.00%,

[0181] Sn: 0.01~0.50%,

[0182] Co: 0.01-0.50%,

[0183] V: 0.01~0.50%,

[0184] Nb: 0.01-0.50%,

[0185] Ti: 0.01~0.50%,

[0186] Zr: 0.001~0.200%,

[0187] Hf: 0.001~0.200%,

[0188] Ta: 0.01~0.50%, and

[0189] Rare earth elements: one or more elements selected from the group consisting of 0.0001 to 0.0030%.

[0190] Hereinafter, the NiCrFe alloy material of the present embodiment will be described in detail. It should be noted that "%" of an element means mass % unless otherwise specified.

[0191] [Chemical composition]

[0192] The chemical composition of the NiCrFe alloy material of the present embodiment contains the following elements.

[0193] C: 0.002~0.030%

[0194] Carbon (C) deoxidizes the alloy. C further improves the strength of the alloy material. If the C content is too low, the above-mentioned effects cannot be fully obtained even if the contents of other elements are within the range of the present embodiment. On the other hand, if the C content is too high, the heat affected zone of the weld is easily sensitized during welding even if the contents of other elements are within the range of the present embodiment. Therefore, the C content is 0.002 to 0.030%. The preferred lower limit of the C content is 0.003%, more preferably 0.005%, and more preferably 0.007%. The preferred upper limit of the C content is 0.025%, more preferably 0.023%, and more preferably 0.020%.

[0195] Si: 0.05-0.50%

[0196] Silicon (Si) deoxidizes the alloy. If the Si content is too low, even if the contents of other elements are within the scope of the present embodiment, the above-mentioned effects cannot be fully obtained. On the other hand, if the Si content is too high, even if the contents of other elements are within the scope of the present embodiment, inclusions are easily formed, and the corrosion resistance of the alloy material is reduced. Therefore, the Si content is 0.05 to 0.50%. The preferred lower limit of the Si content is 0.07%, more preferably 0.10%, and more preferably 0.12%. The preferred upper limit of the Si content is 0.35%, more preferably 0.30%, and more preferably 0.25%.

[0197] Mn: 0.10~1.50%

[0198] Manganese (Mn) deoxidizes the alloy. Mn is an austenite-forming element that stabilizes the austenite in the alloy material. If the Mn content is too low, even if the contents of other elements are within the scope of the present embodiment, the above-mentioned effects cannot be fully obtained. On the other hand, if the Mn content is too high, even if the contents of other elements are within the scope of the present embodiment, inclusions are easily formed, and the corrosion resistance of the alloy material is reduced. Therefore, the Mn content is 0.10 to 1.50%. The preferred lower limit of the Mn content is 0.20%, more preferably 0.30%, and more preferably 0.40%. The preferred upper limit of the Mn content is 1.40%, more preferably 1.30%, and more preferably 1.20%.

[0199] P: 0.050% or less

[0200] Phosphorus (P) is an impurity that is inevitably contained. That is, the lower limit of the P content exceeds 0%. P segregates at the grain boundaries. Therefore, if the P content is too high, even if the content of other elements is within the range of the present embodiment, the crack sensitivity of the alloy material increases and the weldability of the alloy material decreases. Therefore, the P content is 0.050% or less. The preferred upper limit of the P content is 0.045%, more preferably 0.040%, and more preferably 0.030%. The P content is preferably as low as possible. However, an extreme reduction in the P content will significantly increase the manufacturing cost. Therefore, considering industrial production, the preferred lower limit of the P content is 0.001%, more preferably 0.002%, more preferably 0.003%, and more preferably 0.005%.

[0201] S: 0.0200% or less

[0202] Sulfur (S) is an impurity that is inevitably contained. That is, the lower limit of the S content exceeds 0%. S segregates at the grain boundaries. Therefore, if the S content is too high, the crack sensitivity of the alloy material increases even if the content of other elements is within the range of the present embodiment. In this case, inclusions are further easily formed, and the corrosion resistance of the alloy material decreases. Therefore, the S content is less than 0.0200%. The preferred upper limit of the S content is 0.0100%, more preferably 0.0050%, and more preferably 0.0030%. The S content is preferably as low as possible. However, an extreme reduction in the S content will significantly increase the manufacturing cost. Therefore, considering industrial production, the preferred lower limit of the S content is 0.0001%, and more preferably 0.0003%.

[0203] Ni: 29.0~40.0%

[0204] Nickel (Ni) is an austenite forming element that stabilizes the austenite in the alloy material. Ni further improves the corrosion resistance of the alloy material. If the Ni content is too low, even if the content of other elements is within the scope of the present embodiment, the above-mentioned effect cannot be fully obtained. On the other hand, if the Ni content is too high, even if the content of other elements is within the scope of the present embodiment, the manufacturing cost is greatly increased. If the Ni content is too high, the weldability of the alloy material may be reduced. Therefore, the Ni content is 29.0 to 40.0%. The preferred lower limit of the Ni content is 29.5%, and more preferably 30.0%. The preferred upper limit of the Ni content is 39.0%, and more preferably 38.0%.

[0205] Cr: 24.00~30.00%

[0206] Chromium (Cr) improves the corrosion resistance of the alloy material. Cr sometimes improves the weldability of the alloy material. If the Cr content is too low, even if the content of other elements is within the range of the present embodiment, the above-mentioned effect cannot be fully obtained. On the other hand, if the Cr content is too high, even if the content of other elements is within the range of the present embodiment, it is easy to form intermetallic compounds represented by σ phase, and the corrosion resistance of the alloy material is reduced. If the Cr content is too high, the weldability of the alloy material may be reduced. Therefore, the Cr content is 24.00 to 30.00%. The preferred lower limit of the Cr content is 24.50%, and more preferably 25.00%. The preferred upper limit of the Cr content is 29.00%, and more preferably 28.00%.

[0207] Mo: 5.0~7.5%

[0208] Molybdenum (Mo) improves the corrosion resistance of the alloy material. If the Mo content is too low, even if the content of other elements is within the scope of the present embodiment, the above-mentioned effect cannot be fully obtained. On the other hand, if the Mo content is too high, even if the content of other elements is within the scope of the present embodiment, it is easy to form intermetallic compounds represented by σ phase, and the corrosion resistance of the alloy material is reduced. If the Mo content is too high, the weldability of the alloy material may be reduced. Therefore, the Mo content is 5.0 to 7.5%. The preferred lower limit of the Mo content is 5.1%, more preferably 5.3%, and more preferably 5.5%. The preferred upper limit of the Mo content is 7.4%, more preferably 7.2%, and more preferably 7.0%.

[0209] N: 0.20~0.40%

[0210] Nitrogen (N) is dissolved in the alloy material to improve the strength of the alloy material. N sometimes further improves the corrosion resistance of the alloy material. If the N content is too low, the above-mentioned effect cannot be fully obtained even if the content of other elements is within the range of the present embodiment. On the other hand, if the N content is too high, the weldability of the alloy material is reduced even if the content of other elements is within the range of the present embodiment. Therefore, the N content is 0.20 to 0.40%. The preferred lower limit of the N content is 0.21%, more preferably 0.22%, and more preferably 0.23%. The preferred upper limit of the N content is 0.39%, more preferably 0.37%, and more preferably 0.36%.

[0211] Al: 0.50% or less

[0212] Aluminum (Al) is an impurity contained in the alloy material to deoxidize the alloy. That is, the lower limit of the Al content exceeds 0%. If the Al content is too high, even if the content of other elements is within the scope of the present embodiment, Al oxides will be excessively generated and the corrosion resistance of the alloy material will be reduced. Therefore, the Al content is less than 0.50%. The preferred upper limit of the Al content is 0.45%, more preferably 0.40%, and more preferably 0.35%. However, an extreme reduction in the Al content will significantly increase the manufacturing cost. Therefore, considering industrial production, the preferred lower limit of the Al content is 0.01%, more preferably 0.03%, and more preferably 0.05%. It should be noted that the Al content referred to in this specification refers to the "total Al", that is, the content of T-Al.

[0213] Ca: 0.0002~0.0040%

[0214] Calcium (Ca) is harmless by fixing S in the alloy material in the form of sulfide, thereby suppressing the loss plastic cracking of the alloy material and improving the weldability of the alloy material. If the Ca content is too low, even if the content of other elements is within the scope of the present embodiment, the above-mentioned effect cannot be fully obtained. On the other hand, if the Ca content is too high, even if the content of other elements is within the scope of the present embodiment, coarse oxides will be formed in the alloy material, promoting the loss plastic cracking of the alloy material, and reducing the weldability of the alloy material. Therefore, the Ca content is 0.0002 to 0.0040%. The preferred lower limit of the Ca content is 0.0003%, more preferably 0.0005%, more preferably 0.0008%, and more preferably 0.0010%. The preferred upper limit of the Ca content is 0.0035%, and more preferably 0.0030%.

[0215] B: 0.0001~0.0050%

[0216] Boron (B) strengthens the grain boundary at high temperature, inhibits the liquefaction cracking of the alloy material, and improves the weldability of the alloy material. If the B content is too low, even if the content of other elements is within the scope of the present embodiment, the above-mentioned effect cannot be fully obtained. On the other hand, if the B content is too high, B segregates at the grain boundary, promotes the liquefaction cracking of the alloy material, and the weldability of the alloy material is reduced. Therefore, the B content is 0.0001 to 0.0050%. The preferred lower limit of the B content is 0.0003%, more preferably 0.0005%, more preferably 0.0008%, and more preferably 0.0010%. The preferred upper limit of the B content is 0.0045%, more preferably 0.0040%, and more preferably 0.0035%.

[0217] The balance of the chemical composition of the NiCrFe alloy material of the present embodiment is Fe and impurities. Here, impurities refer to substances that are mixed from ore, waste materials or manufacturing environment as raw materials when the NiCrFe alloy material is manufactured industrially, and are allowed within the range that does not cause significant adverse effects on the effects of the NiCrFe alloy material of the present embodiment.

[0218] [Any element]

[0219] The chemical composition of the NiCrFe alloy material of the present embodiment may further contain one or more elements selected from the group consisting of Cu, W, Sn, and Co in place of a portion of Fe. These elements all improve the corrosion resistance of the alloy material.

[0220] Cu: 0.40% or less

[0221] Copper (Cu) is an arbitrary element and may not be contained. That is, the Cu content can be 0%. When Cu is contained, Cu improves the corrosion resistance of the alloy material. As long as a small amount of Cu is contained, the above-mentioned effect can be obtained to some extent. However, if the Cu content is too high, the hot workability of the alloy material is reduced even if the content of other elements is within the scope of the present embodiment. Therefore, the Cu content is 0 to 0.40%, and the Cu content when Cu is contained is less than 0.40%. The preferred lower limit of the Cu content exceeds 0%, more preferably 0.01%, more preferably 0.02%, and more preferably 0.04%. The preferred upper limit of the Cu content is 0.38%, more preferably 0.35%, and more preferably 0.30%.

[0222] W: 1.00% or less

[0223] Tungsten (W) is an arbitrary element and may not be contained. That is, the W content may be 0%. When W is contained, W improves the corrosion resistance of the alloy material. W further improves the strength of the alloy material by solid solution strengthening. As long as a small amount of W is contained, the above-mentioned effect can be obtained to a certain extent. However, if the W content is too high, the hot workability of the alloy material is reduced even if the content of other elements is within the range of the present embodiment. Therefore, the W content is 0 to 1.00%, and the W content when W is contained is less than 1.00%. The preferred lower limit of the W content exceeds 0%, more preferably 0.01%, more preferably 0.03%, and more preferably 0.05%. The preferred upper limit of the W content is 0.95%, more preferably 0.90%, and more preferably 0.85%.

[0224] Sn: 0.50% or less

[0225] Tin (Sn) is an arbitrary element and may not be contained. That is, the Sn content may be 0%. When Sn is contained, Sn improves the corrosion resistance of the alloy material. As long as a small amount of Sn is contained, the above-mentioned effect can be obtained to a certain extent. However, if the Sn content is too high, the hot workability of the alloy material is reduced even if the content of other elements is within the range of the present embodiment. Therefore, the Sn content is 0 to 0.50%, and the Sn content when Sn is contained is less than 0.50%. The preferred lower limit of the Sn content exceeds 0%, more preferably 0.01%, more preferably 0.02%, and more preferably 0.03%. The preferred upper limit of the Sn content is 0.45%, more preferably 0.40%, and more preferably 0.35%.

[0226] Co: 0.50% or less

[0227] Cobalt (Co) is an arbitrary element and may not be contained. That is, the Co content can be 0%. When Co is contained, Co improves the corrosion resistance of the alloy material. As long as a small amount of Co is contained, the above-mentioned effect can be obtained to a certain extent. However, if the Co content is too high, the manufacturing cost will be extremely increased even if the content of other elements is within the scope of the present embodiment. Therefore, the Co content is 0 to 0.50%, and the Co content when Co is contained is less than 0.50%. The preferred lower limit of the Co content exceeds 0%, more preferably 0.01%, more preferably 0.03%, and more preferably 0.05%. The preferred upper limit of the Co content is 0.45%, more preferably 0.40%, and more preferably 0.35%.

[0228] The chemical composition of the NiCrFe alloy material of the present embodiment may further contain one or more elements selected from the group consisting of V, Nb, Ti, Zr, Hf and Ta to replace a portion of Fe. These elements all increase the strength of the alloy material.

[0229] V: 0.50% or less

[0230] Vanadium (V) is an arbitrary element and may not be contained. That is, the V content can be 0%. When V is contained, V forms carbonitrides with C and N, etc., and improves the strength of the alloy material. As long as a small amount of V is contained, the above-mentioned effect can be obtained to a certain extent. However, if the V content is too high, even if the content of other elements is within the range of the present embodiment, the strength becomes too high, and the loss of plastic cracking of the alloy material is promoted, thereby reducing the weldability of the alloy material. Therefore, the V content is 0 to 0.50%, and the V content when V is contained is less than 0.50%. The preferred lower limit of the V content exceeds 0%, more preferably 0.01%, more preferably 0.03%, and more preferably 0.05%. The preferred upper limit of the V content is 0.45%, more preferably 0.40%, and more preferably 0.35%.

[0231] Nb: 0.50% or less

[0232] Niobium (Nb) is an arbitrary element and may not be contained. That is, the Nb content can be 0%. When Nb is contained, Nb forms carbonitrides with C and N, etc., and improves the strength of the alloy material. As long as a small amount of Nb is contained, the above-mentioned effect can be obtained to a certain extent. However, if the Nb content is too high, even if the content of other elements is within the range of the present embodiment, the strength becomes too high, and the loss of plastic cracking of the alloy material is promoted, thereby reducing the weldability of the alloy material. Therefore, the Nb content is 0 to 0.50%, and the Nb content when Nb is contained is less than 0.50%. The preferred lower limit of the Nb content exceeds 0%, more preferably 0.01%, more preferably 0.03%, and more preferably 0.05%. The preferred upper limit of the Nb content is 0.45%, more preferably 0.40%, and more preferably 0.35%.

[0233] Ti: 0.50% or less

[0234] Titanium (Ti) is an arbitrary element and may not be contained. That is, the Ti content can be 0%. When Ti is contained, Ti forms carbonitrides with C and N, etc., and improves the strength of the alloy material. As long as a small amount of Ti is contained, the above-mentioned effect can be obtained to a certain extent. However, if the Ti content is too high, even if the content of other elements is within the range of the present embodiment, the strength becomes too high, and the loss of plastic cracking of the alloy material is promoted, thereby reducing the weldability of the alloy material. Therefore, the Ti content is 0 to 0.50%, and the Ti content when containing Ti is less than 0.50%. The preferred lower limit of the Ti content exceeds 0%, more preferably 0.01%, more preferably 0.03%, and more preferably 0.05%. The preferred upper limit of the Ti content is 0.45%, more preferably 0.40%, and more preferably 0.35%.

[0235] Zr: 0.200% or less

[0236] Zirconium (Zr) is an arbitrary element and may not be contained. That is, the Zr content may be 0%. When Zr is contained, Zr forms carbonitrides and improves the strength of the alloy material. As long as a small amount of Zr is contained, the above-mentioned effect can be obtained to some extent. However, if the Zr content is too high, even if the content of other elements is within the range of the present embodiment, the strength becomes too high, and the loss of plastic cracking of the alloy material is promoted, thereby reducing the weldability of the alloy material. Therefore, the Zr content is 0 to 0.200%, and the Zr content when Zr is contained is less than 0.200%. The preferred lower limit of the Zr content exceeds 0%, more preferably 0.001%, more preferably 0.002%, more preferably 0.003%, and more preferably 0.005%. The preferred upper limit of the Zr content is 0.180%, more preferably 0.150%, and more preferably 0.120%.

[0237] Hf: 0.200% or less

[0238] Hafnium (Hf) is an arbitrary element and may not be contained. That is, the Hf content may be 0%. When Hf is contained, Hf forms carbonitrides and improves the strength of the alloy material. As long as a small amount of Hf is contained, the above-mentioned effect can be obtained to some extent. However, if the Hf content is too high, even if the content of other elements is within the range of the present embodiment, the strength becomes too high, and the loss of plastic cracking of the alloy material is promoted, thereby reducing the weldability of the alloy material. Therefore, the Hf content is 0 to 0.200%, and the Hf content when Hf is contained is less than 0.200%. The preferred lower limit of the Hf content exceeds 0%, more preferably 0.001%, more preferably 0.002%, more preferably 0.003%, and more preferably 0.005%. The preferred upper limit of the Hf content is 0.180%, more preferably 0.150%, and more preferably 0.120%.

[0239] Ta: 0.50% or less

[0240] Tantalum (Ta) is an arbitrary element and may not be contained. That is, the Ta content may be 0%. When Ta is contained, Ta forms carbonitrides and improves the strength of the alloy material. As long as a small amount of Ta is contained, the above-mentioned effect can be obtained to a certain extent. However, if the Ta content is too high, even if the content of other elements is within the range of the present embodiment, the strength becomes too high, and the loss of plastic cracking of the alloy material is promoted, thereby reducing the weldability of the alloy material. Therefore, the Ta content is 0 to 0.50%, and the Ta content when Ta is contained is less than 0.50%. The preferred lower limit of the Ta content exceeds 0%, more preferably 0.01%, more preferably 0.03%, and more preferably 0.05%. The preferred upper limit of the Ta content is 0.45%, more preferably 0.40%, and more preferably 0.35%.

[0241] The chemical composition of the NiCrFe alloy material of the present embodiment may further contain a rare earth element in place of a portion of Fe.

[0242] Rare earth elements: 0.0030% or less

[0243] Rare earth elements (REM) are arbitrary elements and may not be contained. That is, the REM content may be 0%. When REM is contained, REM improves the hot workability of the alloy material by fixing S in the alloy material in the form of sulfide and rendering it harmless. As long as a small amount of REM is contained, the above-mentioned effect can be obtained to a certain extent. However, if the REM content is too high, even if the content of other elements is within the range of the present embodiment, coarse oxides will be formed in the alloy material, and the hot workability of the alloy material will be reduced. Therefore, the REM content is 0 to 0.0030%, and the REM content when REM is contained is less than 0.0030%. The preferred lower limit of the REM content exceeds 0%, more preferably 0.0001%, more preferably 0.0005%, more preferably 0.0008%, and more preferably 0.0010%. The preferred upper limit of the REM content is 0.0025%, more preferably 0.0020%.

[0244] It should be noted that REM in this specification refers to one or more elements selected from the group consisting of scandium (Sc) with an atomic number of 21, yttrium (Y) with an atomic number of 39, and lanthanum (La) with an atomic number of 57 to lutetium (Lu) with an atomic number of 71, which are lanthanoid elements. In addition, the REM content in this specification refers to the total content of these elements.

[0245] [About formula (1)]

[0246] The NiCrFe alloy material of the present embodiment has the above-mentioned chemical composition and satisfies the following formula (1).

[0247] 0.0<8.5×Mn+19.5×Ni-12.43×Cr-42.4×Mo-10250×Ca+1250×B-74.3776<6.5 (1)

[0249] In the formula (1), the content of the corresponding element is substituted in mass % at the element symbol.

[0250] D (=8.5×Mn+19.5×Ni-12.43×Cr-42.4×Mo-10250×Ca+1250×B-74.3776) is an index of loss cracking and liquefaction cracking in the NiCrFe alloy material having the above chemical composition. For the alloy material satisfying the above chemical composition, when D is less than 0.0, although the generation of liquefaction cracking can be suppressed, the generation of loss cracking cannot be suppressed. For the alloy material satisfying the above chemical composition, further when D is more than 6.5, although the generation of liquefaction cracking can be suppressed, the generation of loss cracking cannot be suppressed.

[0251] Therefore, for the NiCrFe alloy material of the present embodiment, D is set to be greater than 0.0 and less than 6.5 on the basis of having the above chemical composition. As a result, the NiCrFe alloy material of the present embodiment can achieve both excellent corrosion resistance and excellent weldability. The preferred lower limit of D is 0.1, more preferably 0.3, and more preferably 0.5. The preferred upper limit of D is 6.4, more preferably 6.2, more preferably 6.0, and more preferably 5.5.

[0252] [Corrosion resistance]

[0253] The NiCrFe alloy material of the present embodiment satisfies formula (1) on the basis of having the above-mentioned chemical composition. As a result, the NiCrFe alloy material of the present embodiment has excellent corrosion resistance. The corrosion resistance of the alloy material in the present embodiment can be evaluated by a four-point bending test. Specifically, a test piece is made from the NiCrFe alloy material of the present embodiment. When the alloy material is an alloy plate, a test piece is made from the central part of the plate thickness. When the alloy material is an alloy tube, a test piece is made from the central part of the wall thickness. The dimensions of the test piece are, for example, a thickness of 2 mm, a width of 10 mm, and a length of 75 mm. It should be noted that the length direction of the test piece is parallel to the rolling direction of the alloy material.

[0254] The test solution is a 25 mass % sodium chloride aqueous solution. According to ASTM G39-99 (2011), stress is applied to the test piece by four-point bending. The applied stress is controlled by a strain gauge, and the strain amount is 0.2%. The stress-loaded test piece is sealed in an autoclave together with the test fixture. The test solution is injected into the autoclave in a residual gas phase, and the autoclave is sealed to form a test bath. After the test bath is degassed, 1 atm of H2S gas is pressurized and sealed in the autoclave, and the test bath is stirred to saturate the H2S gas. The test bath is stirred at 216°C for 240 hours.

[0255] In the present embodiment, in the above four-point bending test, when no cracks are confirmed after 240 hours, it is judged that the alloy material has excellent corrosion resistance. It should be noted that in this specification, "no cracks are confirmed" means that no cracks are confirmed when the test piece after the test is observed by naked eyes.

[0256] [Weldability]

[0257] The NiCrFe alloy material of the present embodiment satisfies formula (1) on the basis of having the above-mentioned chemical composition. As a result, the NiCrFe alloy material of the present embodiment not only has excellent corrosion resistance, but also has excellent weldability. In the present embodiment, having excellent weldability means that the generation of liquefaction cracks and the generation of loss of plastic cracks can be suppressed. Specifically, the weldability of the NiCrFe alloy material of the present embodiment can be evaluated by the longitudinal adjustable restrained crack test described below.

[0258] The test piece is made from the NiCrFe alloy material of the present embodiment. When the alloy material is an alloy plate, the test piece is made from the center of the plate thickness. When the alloy material is an alloy tube, the test piece is made from the center of the wall thickness. The size of the test piece is, for example, 12 mm in thickness, 50 mm in width, and 300 mm in length. It should be noted that the length direction of the test piece is parallel to the rolling direction of the alloy material.

[0259] One end of the test piece in the longitudinal direction is fixed, and a flat plate is welded from the fixed end in the longitudinal direction of the test piece by gas tungsten arc welding (GTAW, Gas Tungsten Arc Welding). When the molten pool reaches the vicinity of the central part of the longitudinal direction of the test piece, a stress is applied to the unfixed end in the longitudinal direction of the test piece, so that the test piece is deformed along the curvature of the bending block. In this way, cracks are generated in the test piece. It should be noted that the welding conditions are a welding current of 200A, a welding voltage of 12V, a welding speed of 15cm / min, and a load strain of 2%.

[0260] After wet polishing the area where cracks have occurred in the test piece, observe it with an optical microscope to determine whether it is a liquefaction crack or a plastic loss crack. The magnification of the optical microscope observation is not particularly limited, as long as the entire crack can be observed. In addition, as long as the technicians in this field can determine the liquefaction crack and the plastic loss crack. Specifically, for example, a welding crack generated at the HAZ far away from the melting line can be judged as a plastic loss crack. For example, it can be further determined that the crack at the HAZ close to the melting line is a liquefaction crack. In this way, by observing with an optical microscope, it is determined whether the welding crack generated in the test piece is a liquefaction crack or a plastic loss crack.

[0261] When liquefaction cracks are confirmed as a result of optical microscope observation, it is judged that excellent weldability cannot be obtained. When liquefaction cracks are not confirmed as a result of optical microscope observation, the total length of loss cracks is calculated. The method for calculating the total length of loss cracks is not particularly limited. For example, a photograph generated by optical microscope observation can be used to measure the crack length with a ruler and calculate it from the ruler. For example, it can also be calculated by performing image analysis on a photograph generated by optical microscope observation.

[0262] In the present embodiment, when the result of the longitudinal adjustable restrained crack test performed under the above conditions shows that no liquefaction cracks are confirmed and the total length of the loss of plasticity cracks is less than 4.0 mm, it is determined that the weldability is excellent.

[0263] [Shape of alloy material]

[0264] The shape of the NiCrFe alloy material of the present embodiment is not particularly limited. The shape of the alloy material may be, for example, a tube shape, a rod shape, a wire shape, a thick plate shape, a thin plate shape, or a foil shape. When the alloy material is in the shape of a tube, the alloy material is preferably a seamless alloy tube.

[0265] [Application of alloy materials]

[0266] The use of the NiCrFe alloy material of the present embodiment is not particularly limited. The NiCrFe alloy material of the present embodiment can be used, for example, in equipment related to the petroleum industry, the gas industry, the petrochemical industry, and the chemical industry. Specifically, the NiCrFe alloy material of the present embodiment is suitable for use in equipment such as primary processing equipment for petroleum and gas, chemical equipment, etc.

[0267] [Manufacturing method]

[0268] An example of a method for manufacturing a NiCrFe alloy material according to the present embodiment is described. Hereinafter, as an example of a NiCrFe alloy material according to the present embodiment, a method for manufacturing a seamless alloy tube is described. The method for manufacturing a seamless alloy tube comprises: a step of preparing a billet (billet preparation step), a step of manufacturing a tube blank from the billet (hot working step), and a step of performing a solution treatment (solution treatment step). It should be noted that the method for manufacturing a NiCrFe alloy material according to the present embodiment is not limited to the manufacturing method described below.

[0269] [Blank material preparation process]

[0270] In the billet preparation process, a NiCrFe alloy having the above chemical composition is smelted. The NiCrFe alloy can be smelted in an electric furnace, or in an Ar-O2 mixed gas bottom blowing decarburization furnace (AOD furnace), or in a vacuum decarburization furnace (VOD furnace). The smelted NiCrFe alloy can be made into an ingot by an ingot casting method, or into a slab, bloom or billet by a continuous casting method. As needed, a slab, bloom or ingot can also be opened to produce a billet. The billet (slab, bloom or billet) is manufactured through the above process.

[0271] [Hot working process]

[0272] In the hot working step, the prepared billet is hot worked to produce an intermediate alloy material (tube billet). The method of hot working is not particularly limited and can be a known method. That is, in the present embodiment, the hot working can be hot rolling, hot extrusion, or hot forging. In the hot working, the heating temperature of the billet is, for example, 1100 to 1300°C.

[0273] For example, the tube blank may be manufactured by the Mannesmann method as a hot working. In this case, the perforation ratio is not particularly limited, and is, for example, 1.0 to 4.0. For example, the tube blank may be manufactured by the glass lubricant high-speed extrusion method or the Ehrlich method (i.e., hot extrusion) as a hot working. In addition, the manufactured tube blank may be subjected to hot rolling using a mandrel mill, a reducing mill, a sizing mill, or the like.

[0274] [Solution treatment process]

[0275] In the solution treatment process, the manufactured intermediate alloy material (tube blank) is subjected to solution treatment. The method of solution treatment is not particularly limited and may be a known method. For example, the tube blank is loaded into a heat treatment furnace, maintained at a desired temperature, and then rapidly cooled. It should be noted that in the case where the tube blank is loaded into a heat treatment furnace and maintained at a desired temperature and then rapidly cooled to perform solution treatment, the temperature for performing solution treatment (solution temperature) refers to the temperature (°C) of the heat treatment furnace used to perform solution treatment. In this case, the time for performing solution treatment (solution time) refers to the time for maintaining the tube blank at the solution temperature.

[0276] The solution temperature in the solution treatment process of the present embodiment is preferably set to 1100-1300°C. If the solution temperature is too low, precipitates (such as σ phases as intermetallic compounds) may remain in the tube blank after the solution treatment. In this case, the corrosion resistance of the manufactured NiCrFe alloy material may be reduced. On the other hand, even if the solution temperature is too high, the effect of the solution treatment is saturated. Therefore, in the present embodiment, the solution temperature in the solution treatment process is preferably set to 1100-1300°C.

[0277] When the blank tube is placed in a heat treatment furnace and held at a desired temperature and then rapidly cooled to perform a solution treatment, the solution treatment time is not particularly limited and can be performed under known conditions. The solution treatment time is, for example, 5 to 180 minutes. The rapid cooling method is, for example, water cooling.

[0278] [Other processes]

[0279] The NiCrFe alloy material of the present embodiment can be manufactured by the above manufacturing method. Other processes can also be performed on the NiCrFe alloy material of the present embodiment as needed. For example, cold working can also be performed on the intermediate alloy material after the hot working process and before the solution treatment process. Cold working can be cold rolling or cold drawing. In this case, it can be processed into a desired size. For example, cold working can also be performed on the manufactured NiCrFe alloy material. In this case, the strength of the NiCrFe alloy material is improved.

[0280] It should be noted that in the above-mentioned manufacturing method, a manufacturing method of a seamless alloy tube is described as an example. However, the NiCrFe alloy material of the present embodiment may also be in other shapes such as a plate. The manufacturing method of other shapes such as a plate also includes, for example, a blank preparation step, a hot working step, and a solution treatment step, as in the above-mentioned manufacturing method. Furthermore, the above-mentioned manufacturing method is an example, and the material may also be manufactured by other manufacturing methods.

[0281] Hereinafter, the present invention will be described in more detail by way of examples.

[0282] Example

[0283] Alloys having the chemical compositions shown in Tables 1 and 2 were melted by high-frequency vacuum melting. It should be noted that the "-" in Tables 1 and 2 means that the content of each element is at the impurity level. Specifically, the Cu content, W content, Sn content, Co content, V content, Nb content, Ti content and Ta content of Test No. 1 refer to 0% by rounding off the third decimal place. Furthermore, the Zr content and Hf content of Test No. 1 refer to 0% by rounding off the fourth decimal place. Furthermore, the REM content of Test No. 1 refers to 0% by rounding off the fifth decimal place. The chemical composition of the alloy of each test number and D obtained by the above definition are shown in Table 3.

[0284] [Table 1]

[0285] Table 1

[0286]

[0287] [Table 2]

[0288] Table 2

[0289]

[0290] [Table 3]

[0291] Table 3

[0292]

[0293] Using the alloy of each test number, a 50kg steel ingot is manufactured by vacuum melting. After heating the steel ingot of each symbol at 1200°C for 24 hours, hot forging is performed to manufacture square materials with a cross-section of 50mm×50mm. After heating the obtained square materials at 1200°C for 1 hour, hot rolling is performed to manufacture plates with a thickness of 30mm. The hot-rolled plates are cold rolled to manufacture plates (alloy plates) with a thickness of 15mm. For the alloy plates of each test number obtained, a solution treatment is performed by heating at 1200°C for 1 hour and then water cooling. Through the above process, alloy plates of each test number are manufactured.

[0294] [Evaluation test]

[0295] The alloy plates having the respective test numbers were subjected to the corrosion resistance test and weldability test described below.

[0296] [Corrosion resistance test]

[0297] For the alloy plates of each test number, a four-point bending test was performed using the above method to evaluate corrosion resistance. Specifically, a test piece with a thickness of 2 mm, a width of 10 mm, and a length of 75 mm was made from the central portion of the plate thickness of the alloy plates of each test number. The length direction of the test piece is equivalent to the rolling direction of the alloy plate. The test solution is a 25 mass % sodium chloride aqueous solution. According to ASTMG39-99 (2011), the test piece loaded with a stress of 0.2% strain by four-point bending is sealed in an autoclave together with the test fixture.

[0298] The test solution is injected into the autoclave in a manner that the gas phase remains, and the autoclave is sealed to form a test bath. After the test bath is degassed, 1atm of H2S gas is pressurized and sealed in the autoclave, and the test bath is stirred to saturate the H2S gas. The test bath is stirred at 216°C for 240 hours. As a result of the four-point bending test performed under the above conditions, if no cracks are confirmed in the test piece after 240 hours, it is judged that the alloy plate of the test number has excellent corrosion resistance ("E" (Excellent) in the "Corrosion Resistance" column in Table 3). On the other hand, if cracks are confirmed in the test piece after 240 hours, it is judged that the alloy plate of the test number does not have excellent corrosion resistance ("NA" (Not Acceptable) in the "Corrosion Resistance" column in Table 3).

[0299] [Weldability test]

[0300] In each test number, the weldability was evaluated for the test number judged to have excellent corrosion resistance. That is, for the test number judged not to have excellent corrosion resistance, the weldability was not evaluated ("-" (no evaluation) in the "liquefaction crack" column in Table 3). Specifically, for the alloy plates of the test number evaluated to have excellent corrosion resistance, the longitudinal adjustable restrained crack test was performed by the above-mentioned method to evaluate the weldability.

[0301] More specifically, a test piece with a thickness of 12 mm, a width of 50 mm, and a length of 300 mm is made from the central part of the plate thickness of the alloy plate of the test number of the object. The length direction of the test piece is equivalent to the rolling direction of the alloy plate. One end of the test piece in the length direction is fixed, and flat plate surfacing is performed in the length direction of the test piece from the fixed end using GTAW. When the molten pool reaches the vicinity of the central part of the length direction of the test piece, a stress is applied to the unfixed end in the length direction of the test piece, causing the test piece to deform along the curvature of the bending block. In this way, cracks are generated in the test piece. It should be noted that the welding conditions are a welding current of 200 A, a welding voltage of 12 V, a welding speed of 15 cm / min, and a load strain of 2%.

[0302] After wet polishing and finishing of the cracked area in the test piece, it was observed with an optical microscope to determine whether it was a liquefaction crack or a plastic loss crack. In the case where the specific crack was a liquefaction crack, it was determined that the alloy plate of the test number had confirmed liquefaction cracks ("NA" (Not Acceptable) in the "Liquidation Crack" column in Table 3). In the case where the specific crack was a plastic loss crack, it was determined that the alloy plate of the test number had not confirmed liquefaction cracks ("E" (Excellent) in the "Liquidation Crack" column in Table 3).

[0303] For the test pieces where no liquefaction cracks were confirmed, the total length of the plastic loss cracks was calculated. The total length of the plastic loss cracks was calculated by measuring the plastic loss crack length with a ruler based on the photographs generated by optical microscope observation and comparing it with the ruler. The obtained plastic loss crack lengths (mm) are shown in Table 3.

[0304] [Evaluation results]

[0305] Referring to Tables 1 to 3, the chemical compositions of the alloy plates of Test Nos. 1 to 15 are appropriate, and D exceeds 0.0 and is less than 6.5. As a result, these alloy plates have excellent corrosion resistance, no liquefaction cracks are confirmed, and the total length of the loss cracks is less than 4.0 mm. That is, these alloy plates have excellent corrosion resistance and excellent weldability.

[0306] On the other hand, the alloy plates of test numbers 16 to 19 had D of 0.0 or less. As a result, the total length of the loss-of-plasticity cracks was 4.0 mm or more. That is, these alloy plates did not have excellent weldability.

[0307] The alloy plates of test numbers 20 to 23 had D of 6.5 or more. As a result, the total length of the plastic loss cracks of these alloy plates was 4.0 mm or more. That is, these alloy plates did not have excellent weldability.

[0308] The alloy plates of test numbers 24 and 25 do not contain Ca and B, and D is 6.5 or more. As a result, the total length of the plastic loss cracks of these alloy plates is 4.0 mm or more. That is, these alloy plates do not have excellent weldability.

[0309] The alloy plate of Test No. 26 had an excessively low N content. As a result, the alloy plate did not have excellent corrosion resistance.

[0310] The alloy plate of test number 27 had an excessively high N content. As a result, the total length of the loss-of-plasticity cracks of the alloy plate was 4.0 mm or more. That is, the alloy plate did not have excellent weldability.

[0311] The Ca content of the alloy plate of Test No. 28 was too low. As a result, the total length of the loss-of-plasticity cracks of the alloy plate was 4.0 mm or more. That is, the alloy plate did not have excellent weldability.

[0312] The Ca content of the alloy plates of test numbers 29 and 30 was too high. As a result, the total length of the loss-of-plasticity cracks of these alloy plates was 4.0 mm or more. That is, these alloy plates did not have excellent weldability.

[0313] The alloy plate of test number 31 had an excessively low B content, and D was 6.5 or more. As a result, liquid cracking was observed in the alloy plate. That is, the alloy plate did not have excellent weldability.

[0314] The alloy plates of test numbers 32 and 33 had too high B contents, and D was 6.5 or more. As a result, liquefaction cracks were observed in these alloy plates. That is, these alloy plates did not have excellent weldability.

[0315] The alloy plate of Test No. 34 had an excessively low Ni content, and D was 0.0 or less. As a result, the alloy plate did not have excellent corrosion resistance.

[0316] The alloy plate of test number 35 had an excessively high Ni content. As a result, the total length of the loss-of-plasticity cracks of the alloy plate was 4.0 mm or more. That is, the alloy plate did not have excellent weldability.

[0317] The Cr content of the alloy plate of test number 36 was too low. As a result, the total length of the loss-of-plasticity cracks of the alloy plate was 4.0 mm or more. That is, the alloy plate did not have excellent weldability.

[0318] The Cr content of the alloy plate of test number 37 was too high. As a result, the total length of the loss-of-plasticity cracks of the alloy plate was 4.0 mm or more. That is, the alloy plate did not have excellent weldability.

[0319] The Mo content of the alloy plate of Test No. 38 was too low. As a result, the alloy plate did not have excellent corrosion resistance.

[0320] The alloy plate of test number 39 has an excessively high Mo content and an excessively low N content. As a result, the total length of the loss-of-plasticity cracks of the alloy plate is 4.0 mm or more. That is, the alloy plate does not have excellent weldability.

[0321] The alloy plate of Test No. 40 had an excessively high V content. As a result, the alloy plate did not have excellent corrosion resistance.

[0322] The P content of the alloy plate of test number 41 was too high. As a result, liquid cracking was observed in the alloy plate. That is, the alloy plate did not have excellent weldability.

[0323] The embodiments of the present disclosure are described above. However, the above embodiments are merely examples for implementing the present disclosure. Therefore, the present disclosure is not limited to the above embodiments, and the above embodiments can be appropriately modified and implemented within the scope of the present disclosure.

Claims

1. A NiCrFe alloy material having the following chemical composition: Contains by mass% C: 0.002~0.030%, Si: 0.05-0.50%, Mn: 0.10~1.50%, P: 0.050% or less, S: 0.0200% or less, Ni: 29.0-40.0%, Cr: 24.00~30.00%, Mo: 5.0~7.5%, N: 0.20~0.40%, Al: 0.50% or less, Ca: 0.0002-0.0040%, and B: 0.0001~0.0050%, Balance: Fe and impurities, And satisfying formula (1), 0.0<8.5×Mn+19.5×Ni-12.43×Cr-42.4×Mo-10250×Ca+1250×B-74.3776<6.5(1) in, In the formula (1), the content of the corresponding element is substituted in mass % at the element symbol.

2. A NiCrFe alloy material having the following chemical composition: Contains by mass% C: 0.002~0.030%, Si: 0.05-0.50%, Mn: 0.10~1.50%, P: 0.050% or less, S: 0.0200% or less, Ni: 29.0-40.0%, Cr: 24.00~30.00%, Mo: 5.0~7.5%, N: 0.20~0.40%, Al: 0.50% or less, Ca: 0.0002-0.0040%, and B: 0.0001~0.0050%, Also contains the freedom to choose Cu: 0.40% or less, W: 1.00% or less, Sn: 0.50% or less, Co: 0.50% or less, V: 0.50% or less, Nb: 0.50% or less, Ti: 0.50% or less, Zr: 0.200% or less, Hf: 0.200% or less, Ta: 0.50% or less, and Rare earth elements: 0.0030% or less of one or more elements in the group consisting of Balance: Fe and impurities, And satisfying formula (1), 0.0<8.5×Mn+19.5×Ni-12.43×Cr-42.4×Mo-10250×Ca+1250×B-74.3776<6.5(1) in, In the formula (1), the content of the corresponding element is substituted in mass % at the element symbol.

3. The NiCrFe alloy material according to claim 2, wherein: The chemical composition contains a Cu: 0.40% or less, W: 1.00% or less, Sn: 0.50% or less, and Co: One or more elements selected from the group consisting of 0.50% or less.

4. The NiCrFe alloy material according to claim 2, wherein: The chemical composition contains a V: 0.50% or less, Nb: 0.50% or less, Ti: 0.50% or less, Zr: 0.200% or less, Hf: 0.200% or less, and Ta: One or more elements selected from the group consisting of 0.50% or less.

5. The NiCrFe alloy material according to claim 2, wherein: The chemical composition contains rare earth elements: less than 0.0030%.