Molybdenum target and method for producing same
The molybdenum target with controlled microstructure and low impurity content addresses the issue of high particle generation in existing targets, resulting in improved yield and quality of molybdenum films through precise manufacturing processes.
Patent Information
- Application Number
- PCT/JP2024/017842
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-15
- Filing Date
- 2024-05-14
- Publication Date
- 2024-11-21
AI Technical Summary
The existing molybdenum sputtering targets suffer from high particle generation during film formation, leading to reduced yield and quality, due to insufficient control over pore generation and distribution, which is exacerbated by the miniaturization of interconnects.
A molybdenum target with a relative density of 99% or more, oxygen content of 25 ppm or less, and tungsten content of 10-100 ppm, featuring precise control over pore size and distribution, is manufactured using a process involving hot pressing and hot isostatic pressing at specific temperature ranges to achieve a high-purity sputtering target with controlled crystal grain size and Vickers hardness.
The solution significantly reduces particle generation, enabling the formation of high-quality molybdenum films with low specific resistance and stable production, by minimizing pores and ensuring uniformity in the target's microstructure.
Smart Images

Figure JP2024017842_21112024_PF_FP_ABST
Abstract
Description
Molybdenum target and method for producing the same
[0001] The present invention relates to a molybdenum target formed of a sintered body of molybdenum powder and a method for producing the same.
[0002] In recent years, tungsten, which has heat resistance and low resistance properties, has been widely used as a wiring material or electrode material in the field of semiconductor device manufacturing. Tungsten films are generally formed by sputtering. Tungsten film sputtering involves bombarding a tungsten target with argon ions generated by plasma discharge, knocking tungsten atoms from the target surface and depositing them on a substrate placed opposite the target. A major problem in this process is that particles generated from the target surface adhere to the substrate, reducing yield. For this reason, tungsten targets with extremely low particle generation, fine and uniform crystal grains, and high relative density are essential.
[0003] However, even if high-purity tungsten films can be formed, there is a concern that they will not be able to meet the future demand for even lower resistivity. Therefore, it is necessary to find a promising material to replace tungsten. In this regard, molybdenum films have attracted attention as they may be able to achieve sufficiently low electrical resistivity values, but they are also known to have a problem of high particle generation during sputtering, which reduces material yield.
[0004] Therefore, a molybdenum sputtering target capable of effectively reducing particles during sputtering has been proposed, which has a molybdenum content of 99.99% by mass or more, a relative density of 98% or more, and an average crystal grain size of 400 μm or less. A method for manufacturing a sputtering target has also been proposed, which includes the steps of preparing a molybdenum powder, hot-pressing the molybdenum powder under a load at a temperature of 1350°C to 1500°C, and hot-isostatically pressing the compact obtained by the hot pressing at a temperature of 1300°C to 1850°C (see Patent Document 1).
[0005] Japanese Patent Application Laid-Open No. 2022-125041
[0006] However, it has been found that the generation of particles from the molybdenum target cannot be sufficiently reduced even by the method of Patent Document 1. In particular, as miniaturization of wiring and the like using molybdenum progresses, particles generated from the molybdenum target have a significant impact on yield, and therefore, there is a demand for further suppression of particle generation.
[0007] Therefore, as a result of studying the causes of particles when forming a film by sputtering a molybdenum target, it was found that although the target manufactured by the above-mentioned manufacturing method has a relative density of the sintered body that reaches just under 100%, pores are inevitably present and the size and distribution of these pores are not controlled, so particle generation cannot be suppressed and this causes a decrease in yield.
[0008] Therefore, in order to improve the yield, a molybdenum target that generates as few particles as possible is required, and a manufacturing method that can obtain such a molybdenum target is required.
[0009] In view of the above circumstances, an object of the present invention is to provide a molybdenum target in which the generation of pores, which are the cause of particle generation, is suppressed and the size and distribution of the pores are controlled with high precision, and a method for manufacturing the same.
[0010] In order to achieve the above object, a first aspect of the present invention is a molybdenum target formed of a sintered body of molybdenum powder, the molybdenum target having a relative density of 99% or more, an oxygen content of 25 ppm or less, a carbon content of 30 ppm or less, a tungsten content of 10 ppm to 100 ppm, a molybdenum content excluding the oxygen content, the carbon content, and the tungsten content of 99.999 mass% or more, and a thickness of 0.15 mm 2 In the observation area of 0.01 μm 2 0.2 μm or more 2 There are 20 or less pores with a size of less than 0.2 μm 2 More than 1.8 μm 2There are five or fewer pores with a size of less than 1.8 μm 2 The molybdenum target has one or less pores of the above size.
[0011] The second aspect of the present invention is an average particle diameter d calculated as a circle equivalent diameter. Ave is 20 μm or more and 100 μm or less, and the standard deviation 3σ of the particle diameter calculated using the circle equivalent diameter and the average particle diameter d Ave The ratio (3σ / d Ave ) is 1.2 or less.
[0012] A third aspect of the present invention is the molybdenum target according to the second aspect, wherein the average aspect ratio of the grain size is less than 1.2.
[0013] In a fourth aspect of the present invention, the average value of the Vickers hardness is 180 or less, and the standard deviation 3σ of the Vickers hardness and the average value H Ave The ratio (3σ / H Ave ) is 0.07 or less.
[0014] The fifth aspect of the present invention is a method for producing a powder having an average particle size D obtained by a laser diffraction / scattering method. Ave The median diameter D50 is 2.0 to 3.5, and the median diameter D90 and the average particle diameter D Ave The ratio of D90 to D Ave ) is 1.7 or less, and the median diameter D95 and the average particle diameter D Ave The ratio of D95 / D Ave The molybdenum target is produced by hot pressing molybdenum powder having a sintering ratio (Sr) of 0.01 to 0.15 (mol / L) at a temperature of 1400°C or higher and 1500°C or lower, followed by sintering at a temperature of 1500°C or higher and 1600°C or lower by hot isostatic pressing.
[0015] A sixth aspect of the present invention is the method for producing a molybdenum target according to the fifth aspect, wherein the molybdenum powder has a tungsten content of 10 ppm to 100 ppm, and a molybdenum content excluding the oxygen content, the carbon content, and the tungsten content of 99.999 mass% or more.
[0016] A seventh aspect of the present invention is the method for producing a molybdenum target according to the fifth or sixth aspect, wherein the hot pressing is carried out under high vacuum conditions at a holding temperature of 1400 to 1500° C. for a holding time of 360 to 600 minutes.
[0017] According to the present invention, it is possible to realize a molybdenum target and a method for manufacturing the same in which the generation of pores, which are the cause of particle generation, is suppressed and the size and distribution of the pores are controlled with high precision.
[0018] 0.01 to 0.2 μm in the examples and comparative examples of the present invention 2 1 is a graph showing the relationship between the number of pores and the number of particles in the examples of the present invention and the comparative examples. 2 1 is a graph showing the relationship between the number of pores and the number of particles in the examples of the present invention and the comparative example. 2 FIG. 10 is a diagram showing the relationship between the number of pores and the number of particles.
[0019] The molybdenum target of the present invention has a molybdenum purity (content) of 5N (99.999 mass%) or more, a relative density of 99% or more, an oxygen content of 25 ppm or less, a carbon content of 30 ppm or less, a tungsten content of 10 ppm to 100 ppm, and a thickness of 0.15 mm 2 In the observation area of 0.01 μm 2 0.2 μm or more 2 There are 20 or less pores with a size of less than 0.2 μm 2 More than 1.8 μm 2 There are five or fewer pores with a size of less than 1.8 μm 2 The molybdenum purity of 5N means that the molybdenum content excluding the oxygen content, carbon content, and tungsten content is 99.999 mass% or more.
[0020] (Purity) To form a molybdenum film with low resistivity, it is necessary to suppress impurities contained in the molybdenum film, and therefore it is essential to highly purify the molybdenum target. Specifically, it is necessary for the molybdenum target to have a purity of 99.999 mass % (5N) or more.
[0021] (Gas Components) Gas components such as carbon and oxygen contained in a molybdenum target adversely affect the resistivity of the molybdenum film. These gas components are incorporated into the molybdenum film during film formation, and as their content increases, the resistivity of the molybdenum film tends to increase. Therefore, the carbon content of the molybdenum target is preferably 30 mass ppm or less, and the oxygen content is preferably 25 mass ppm or less.
[0022] (Tungsten Content) The molybdenum target of the present invention has a tungsten content of 10 ppm to 100 ppm, preferably 20 ppm to 50 ppm.
[0023] The reason for setting the tungsten content within this range is as follows: Normally, the tungsten content is reduced to an unavoidable level, but in the present invention, the tungsten content is set within a predetermined range. If the tungsten content is too low, grain growth is likely to occur during sintering, the crystal grain size becomes large, and large pores are likely to form. On the other hand, if the tungsten content is too high, sinterability tends to deteriorate, making it difficult to achieve high density.
[0024] (Crystal Grain Size) The molybdenum target of the present invention has an average crystal grain size d calculated based on a circle equivalent diameter. Ave is 20 μm or more and 100 μm or less.
[0025] The reason for using such an average value of the crystal grain size (average grain size) is as follows: As the average grain size of the molybdenum target becomes smaller, the difference in the amount of erosion caused by the difference in orientation of each crystal grain present on the target surface can be reduced, thereby reducing the number of abnormal discharges caused by unevenness and suppressing the generation of particles during film formation.
[0026] On the other hand, if the average particle size is too small, the film formation rate becomes too slow, resulting in a decrease in productivity.
[0027] In addition, the standard deviation 3σ of the particle diameter calculated using the circle equivalent diameter and the average particle diameter d Ave The ratio (3σ / d Ave) is 1.2 or less. This ratio is found by dividing the standard deviation 3σ by the average particle size. The aspect ratio of the length to width of the particle size is less than 1.2. This aspect ratio is the value obtained by dividing the major axis of the particle image by the minor axis to determine the "particle size calculated using the equivalent circle diameter," and was found using the image analysis software "Image-j."
[0028] Standard deviation 3σ of particle size and average particle size d Ave The ratio (3σ / d Ave The reason why the aspect ratio of the length to the width of the grain size is preferably 1.2 or less is as follows: There is a correlation between the variation in crystal grain size and the number and size of pores, and the smaller the variation in crystal grain size, the fewer the number of pores in the target and the smaller their size, so that within the above range, particle generation during film formation can be suppressed. In addition, the reason why the aspect ratio of the length to the width of the grain size is preferably less than 1.2 is that a stable film formation rate can be obtained that does not adversely affect production, and the film formation rate is unlikely to change even when the target is replaced.
[0029] (Relative Density) The relative density of the molybdenum target is preferably 99% or more. If the relative density of the target is 99% or more, the amount of gas components contained in the target is small, so that when a film is formed, an increase in the resistivity of the film can be suppressed. Furthermore, the higher the relative density of the target, the fewer the number of pores, so that the number of abnormal discharges caused by unevenness on the target surface is reduced, and the generation of particles during film formation can be suppressed.
[0030] (Vickers Hardness) The average Vickers hardness of the molybdenum target is preferably 160 or more and 180 or less, and more preferably 165 to 175.
[0031] The reason why the average value of the Vickers hardness is preferably in the above range is as follows: There is a correlation between the average value of the Vickers hardness and the number and size of pores in the target, and the higher the average value of the Vickers hardness, the fewer the number and size of pores in the target, which makes it possible to suppress particle generation during film formation.
[0032] On the other hand, if the average Vickers hardness is very high, it is highly likely that the heat treatment conditions were not appropriate and that internal strain in the molybdenum has not been removed. This internal strain can become the starting point for cracking due to thermal stress during target processing or film formation by sputtering.
[0033] In addition, the standard deviation 3σ of Vickers hardness and the average value H Ave The ratio (3σ / H Ave The calculation method was to divide the standard deviation 3σ by the average value of the Vickers hardness.
[0034] The reason why the ratio of three times the standard deviation (3σ) of the Vickers hardness to the average value of the Vickers hardness is preferably in the above-mentioned range is as follows.
[0035] There is a correlation between the variation in Vickers hardness and the number and size of pores. The smaller the variation in Vickers hardness, the fewer the number and size of pores in the target, which makes it possible to suppress particle generation during film formation.
[0036] (Pore) The molybdenum target of the present invention has a pore size of 0.15 mm. 2 In the observation area of 0.01 μm 2 0.2 μm or more 2 There are 20 or less pores with a size of less than 0.2 μm 2 More than 1.8 μm 2 There are five or fewer pores with a size of less than 1.8 μm 2 There is one or less pore of this size.
[0037] The reasons for setting the size and number of pores within the above-mentioned ranges in the present invention are as follows: By controlling the size and number of pores, an electric field is concentrated in the pores, which can suppress particles generated by localized dissolution and scattering, thereby improving yield. Furthermore, the number of particles generated remains low until the end of the target's life, allowing for stable production.
[0038] Although a molybdenum target having extremely few coarse pores and suppressed pore localization in the surface and thickness directions of the molybdenum target has not been realized until now, it can be realized by having the above-mentioned relative density, hardness, and crystal grain size characteristics. Furthermore, the molybdenum target of the present invention having extremely few coarse pores and suppressed pore localization in the surface and thickness directions of the molybdenum target can be realized by the manufacturing method described below.
[0039] As described above, the molybdenum target of the present invention has small and few pores. Therefore, by using this molybdenum target, the amount of particles generated can be significantly reduced, and a high-quality molybdenum film can be stably formed.
[0040] A method for manufacturing a molybdenum target according to one embodiment of the present invention will be described.
[0041] The molybdenum target of the present invention has an average particle diameter D obtained by a laser diffraction / scattering method. Ave The molybdenum powder can be manufactured by hot pressing at a temperature of 1400°C or higher and 1500°C or lower (HP process) using molybdenum powder having a surface roughness of 2.5 to 4.0 μm and a median diameter D50 of 2.0 to 3.5, and then sintering the molybdenum powder by hot isostatic pressing at a temperature of 1500°C or higher and 1600°C or lower (HIP process).
[0042] The method for producing a sputtering target of the present invention is to use a laser diffraction / scattering method to obtain an average particle diameter D Ave The first point is to use molybdenum powder having a particle size of 2.5 to 4.0 μm, preferably 2.8 to 3.7 μm, and a median diameter D50 of 2.0 to 3.5, preferably 2.2 to 3.3 μm.
[0043] In addition, the method for producing a sputtering target of the present invention is also advantageous in that the median diameter D90 and the average particle diameter D Ave The ratio of D90 to D Ave The second point is to use molybdenum powder having a ρ of 1.7 or less, preferably 1.5 or less.
[0044] In addition, the method for producing a sputtering target of the present invention is also advantageous in that the median diameter D95 and the average particle diameter D Ave and the ratio (D95 / D Ave The third point is to use tungsten powder having a refractive index of 2.0 or less, preferably 1.8 or less.
[0045] In this way, in the present invention, by using a molybdenum powder having a particle size within a predetermined range and an extremely narrow particle size distribution range, i.e., a small variation in particle size from the average particle size, a molybdenum target having extremely small and few pores can be realized. In the present invention, the feature of such a narrow particle size distribution is realized by comparing the median diameter D90 with the average particle size D obtained by the laser diffraction / scattering method. Ave The value divided by the median diameter D95 and the average particle diameter D obtained by the laser diffraction / scattering method Ave The value obtained by dividing the particle size by the particle diameter is defined as being equal to or less than a predetermined value. Note that powders having a wide particle size distribution outside this range cannot achieve the effects of the present invention.
[0046] Furthermore, if the average particle size of the powder is too large, a sintered body with the desired density cannot be obtained, whereas if it is too small, the density rises sharply during hot pressing (HP) and oxides are trapped, so it is necessary to keep the average particle size within a specified range.
[0047] The molybdenum powder used in the present invention has a tungsten content of 10 ppm to 100 ppm, and a molybdenum content excluding the oxygen content, carbon content, and tungsten content of 99.999 mass % or more.
[0048] Since the oxygen content affects the oxygen content of the molybdenum target, the oxygen content of the raw material powder is preferably set to, for example, 3000 mass ppm or less, as this increases the amount of oxide sublimation, which may damage the hot press apparatus.
[0049] The sputtering target of the present invention can be produced by hot pressing the above-mentioned molybdenum powder at a temperature of 1400°C or higher and 1500°C or lower, and then sintering it by hot isostatic pressing at a temperature of 1500°C or higher and 1600°C or lower.
[0050] Vacuum hot pressing in a high vacuum region promotes degassing and sintering, reducing the amount of oxygen contained in the molybdenum target and allowing for the production of high-density sintered compacts. If the oxygen content of the molybdenum powder is high, the number of oxides in the molybdenum target increases, resulting in increased particle generation. Furthermore, a thick surface oxide film inhibits sintering, making it impossible to obtain high-density sintered compacts.
[0051] Here, high vacuum is 1×10 -2 Pa or less, preferably 1×10 -3 Pa or less, more preferably 1 × 10 -4 Pa or less.
[0052] As described above, gas components such as carbon and oxygen contained in the molybdenum target adversely affect the resistivity of the molybdenum film, so the carbon content in the molybdenum target is preferably 30 ppm by mass or less, and the oxygen content is preferably 25 ppm by mass or less.
[0053] The oxygen concentration can be achieved by vacuum hot pressing as described above.
[0054] On the other hand, regarding the carbon concentration, during hot pressing, carbon diffuses from the graphite members constituting the hot pressing apparatus into the molybdenum sintered compact, causing an increase in the carbon content. Therefore, the lower the hot pressing temperature, the better, and a carbon concentration of 30 ppm by mass or less, preferably 20 ppm by mass or less, can be stably achieved at 1500°C or less.
[0055] In the HP process, a sintered body having a relative density of 95% or more is produced. The HP temperature for producing a sintered body with such properties is preferably 1400°C or higher and 1500°C or lower. If the HP temperature is too low, the density will not rise to a level at which HIP treatment is possible, and if it is too high, rapid grain growth will cause localized formation of coarse pores, which is undesirable. If the HP pressure is too low, the density will not rise to a level at which HIP treatment is possible. If it is too high, the HP equipment will be severely worn out. For example, the pressure during HP treatment is 39.2 MPa (400 kg / cm 2 ) or more 44.1MPa (450kg / cm 2) or less. The HP holding time in this process is 360 minutes or more and 600 minutes or less. If the HP holding time is too short, the density will not increase to a level at which HIP treatment is possible, and if it is too long, productivity will decrease. In the present invention, it is important to control the powder particle size and particle size distribution, and to set the HP temperature to 1400°C or more and 1500°C or less, and the HP holding time to 360 minutes or more and 600 minutes or less. This makes it possible to prevent the pores in the sintered body from becoming coarse and to uniformly distribute fine pores throughout the sintered body.
[0056] After the HP treatment, the sintered body is subjected to hot isostatic pressing (HIP) to reduce pores in the sintered body and to increase density.
[0057] The HIP temperature is 1500°C or higher and 1600°C or lower. If the HIP temperature is lower than 1500°C, the processing temperature is low, making it difficult to obtain a high relative density of 99% or higher within a processing time suitable for mass production. In particular, in the present invention, since a molybdenum powder with a tungsten content within a predetermined range is used, a sintered body with a relative density of 99% or higher cannot be obtained at temperatures lower than 1500°C. Furthermore, if the HIP temperature exceeds 1600°C, the high processing temperature leads to rapid coarsening of the crystal grains, resulting in the local formation of coarse pores, which is undesirable. The pressure is not particularly limited and may be, for example, 100 to 200 MPa, and in this embodiment, it is 176.4 MPa (1800 kg / cm). 2 )
[0058] According to the above manufacturing method, a molybdenum target having the characteristics of the present invention can be obtained. In particular, the number of pores in the molybdenum target can be reduced, the size of the pores can be reduced, and localization of the pores can be suppressed. Therefore, by using the sputtering target of this embodiment, it is possible to reduce particle generation during film formation, and it is possible to stably form a high-quality molybdenum film.
[0059] The presence of pores in a sputtering target is strongly correlated with the size and particle size distribution of the raw material powder, the relative density of the sintered body, the size and distribution of the target's crystal grain size, and the size and distribution of its hardness. The finer the size of the raw material powder and the narrower the range of its particle size distribution, the higher the relative density of the sintered body, and the smaller the variation in crystal grain size and hardness, the more significantly the occurrence of pores is reduced and the size of the pores becomes extremely small.
[0060] On the other hand, even if the crystal grain size is fine, if the variation is large, the formation of coarse pores cannot be suppressed. The present inventors have found that by optimizing the size and particle size distribution of the raw material powder, the hot pressing conditions, and the hot isostatic pressing conditions, the relative density of the sintered body is increased and the variation in crystal grain size and hardness is suppressed, making it possible to produce a molybdenum target of the present invention with very few coarse pores and almost no localized pores.
[0061] That is, in the method for producing a molybdenum target of this embodiment, the raw material powder is hot pressed at a temperature of 1400°C to 1500°C, and then sintered by hot isostatic pressing at a temperature of 1500°C to 1600°C.
[0062] According to the above-described method for producing a molybdenum target, it is possible to obtain a sputtering target having small and few pores. 2 In the observation area of 0.01 μm 2 0.2 μm or more 2 There are 20 or less pores with a size of less than 0.2 μm 2 More than 1.8 μm 2 There are five or fewer pores with a size of less than 1.8 μm 2 It is possible to stably produce a molybdenum target having one or less pores of the above size.
[0063] In the method for producing a molybdenum target of the present invention, the relative density is 99% or more, the Vickers hardness is 180 or less, and the standard deviation 3σ of the Vickers hardness and the average value H Ave The ratio (3σ / H Ave) is 0.07 or less, the average particle size is 20 μm or more and 100 μm or less, the standard deviation 3σ of the average particle size and the average particle size H Ave The ratio (3σ / H Ave ) of 1.2 or less can be efficiently and stably produced.
[0064] This makes it possible to manufacture a molybdenum target with small and few pores, and by using this molybdenum target, the amount of particles generated can be significantly reduced, making it possible to stably form a high-quality molybdenum film.
[0065] The sintered body produced as described above is processed into a predetermined target shape in a processing step. Although the processing method is not particularly limited, mechanical processing methods such as grinding and cutting are typically applied. The processed size and shape are determined according to the target specifications, and are processed into, for example, a circular or rectangular shape. The processed sintered body is bonded to a backing plate to form a sputtering cathode.
[0066] The present invention will be described below with reference to Examples and Comparative Examples. The average particle size and particle size distribution of the molybdenum powder were determined using a particle size distribution measuring device "LS13320" manufactured by Microtrackbell Corporation.
[0067] (Examples 1-4) As shown in Table 1, the tungsten content is 10 ppm to 100 ppm, the molybdenum content excluding the tungsten and gas content is 99.999 mass% or more (purity 5N), and the average particle size D obtained by the laser diffraction / scattering method is Ave The median diameter D50 is 2.0 to 3.5, and the median diameter D90 and the average particle diameter D Ave The ratio of D90 to D Ave ) is 1.7 or less, and the median diameter D95 and the average particle diameter D Ave The ratio of D95 / D AveA molybdenum powder having a ρ of 2.0 or less was used, and the powder was hot pressed at a temperature of 1400°C or higher and 1500°C or lower, both inclusive, as shown in Table 1, and then subjected to HIP at a temperature of 1500°C or higher and 1600°C or lower, both inclusive, as shown in Table 1, to obtain a molybdenum sintered body. The obtained molybdenum sintered body was ground using a lathe to form a predetermined target shape (diameter 440 mm, thickness 6 mm).
[0068] (Comparative Example 1) As shown in Table 1, the average particle diameter D obtained by the laser diffraction / scattering method Ave is smaller than 2.5 μm, the median diameter D50 is smaller than 2.0 μm, and the median diameter D90 and the average particle diameter D Ave The ratio of D90 to D Ave ) is 1.7 or less, and the median diameter D95 and the average particle diameter D Ave The ratio of D95 / D Ave Molybdenum powder having a porosity of 2.0 or less was used and hot pressed at the temperatures shown in Table 1 to obtain molybdenum sintered bodies. The particle size of the molybdenum powder was too small, which resulted in a rapid increase in density and the trapping of a large amount of oxide.
[0069] (Comparative Example 2) As shown in Table 1, the average particle diameter D obtained by the laser diffraction / scattering method Ave The median diameter D50 is 2.0 to 3.5, and the median diameter D90 and the average particle diameter D Ave The ratio of D90 to D Ave ) is 1.7 or less, and the median diameter D95 and the average particle diameter D Ave The ratio of D95 / D Ave A molybdenum powder having a porosity of 2.0 or less was used, and a molybdenum sintered body was obtained by hot pressing the molybdenum powder at the temperature shown in Table 1. Since HIP was not performed, a sintered body with sufficient density could not be obtained.
[0070] (Comparative Example 3-8) As shown in Table 1, the average particle diameter D obtained by the laser diffraction / scattering method Ave is smaller than 2.5 μm, the median diameter D50 is smaller than 2.0 μm, and the median diameter D90 and the average particle diameter D Ave The ratio of D90 to D Ave ) is 1.7 or less, and the median diameter D95 and the average particle diameter DAve The ratio of D95 / D Ave A molybdenum powder having a porosity of 2.0 or less was used, and the molybdenum powder was hot pressed at the temperatures shown in Table 1, followed by HIP to obtain a molybdenum sintered body. The obtained molybdenum sintered body was ground using a lathe to have a predetermined target shape (diameter 440 mm, thickness 6 mm).
[0071] (Comparative Example 9) As shown in Table 1, the average particle diameter D obtained by the laser diffraction / scattering method Ave The median diameter D50 is 2.5 to 4.0 μm, the median diameter D90 is 2.0 to 3.5 μm, and the median diameter D90 and the average particle diameter D Ave The ratio of D90 to D Ave ) is 1.7 or more, and the median diameter D95 and the average particle diameter D Ave The ratio of D95 / D Ave A molybdenum powder having a porosity of 2.0 or more was used, and the molybdenum powder was hot pressed at the temperatures shown in Table 1, followed by HIP to obtain a molybdenum sintered body. The obtained molybdenum sintered body was ground using a lathe to have a predetermined target shape (diameter 440 mm, thickness 6 mm).
[0072] (Comparative Example 10) As shown in Table 1, the average particle diameter D obtained by the laser diffraction / scattering method Ave is greater than 4.0 μm, the median diameter D50 is 2.0 to 3.5 μm, and the median diameter D90 and the average particle diameter D Ave The ratio of D90 to D Ave ) is 1.7 or less, and the median diameter D95 and the average particle diameter D Ave The ratio of D95 / D Ave A molybdenum powder having a porosity of 2.0 or more was used, and the molybdenum powder was hot pressed at the temperatures shown in Table 1, followed by HIP to obtain a molybdenum sintered body. The obtained molybdenum sintered body was ground using a lathe to have a predetermined target shape (diameter 440 mm, thickness 6 mm).
[0073] (Comparative Examples 11 to 13) As shown in Table 1, the average particle diameter D obtained by the laser diffraction / scattering method Ave is larger than 4.0 μm, the median diameter D50 is larger than 3.5 μm, and the median diameter D90 and the average particle diameter D Ave The ratio of D90 to DAve ) is 1.7 or more, and the median diameter D95 and the average particle diameter D Ave The ratio of D95 / D Ave A molybdenum powder having a porosity of 2.0 or more was used, and the molybdenum powder was hot pressed at the temperatures shown in Table 1, followed by HIP to obtain a molybdenum sintered body. The obtained molybdenum sintered body was ground using a lathe to have a predetermined target shape (diameter 440 mm, thickness 6 mm).
[0074] The results are shown in Tables 2 and 3. (Examples and Comparative Examples) The relative density, Vickers hardness, grain size, tungsten content, oxygen content, carbon content, and pores of the obtained targets were measured according to the following procedures.
[0075] (Relative Density) Samples of 10 × 10 × 6 mm were taken from the center, edge, and halfway along the line connecting the center and edge of the obtained molybdenum target. The cross section of each sample was polished and etched, and then the specific gravity was calculated using Archimedes' method to determine the theoretical density of molybdenum (10.23 g / cm). 3 The relative density of each sample was added up and divided by the number of samples to obtain a value, which was taken as the relative density of the molybdenum target according to the present invention.
[0076] (Vickers Hardness) Samples measuring 10 × 10 × 6 mm were taken from the center, edge, and halfway along the line connecting the center and edge of the obtained molybdenum target. After polishing the cross section of each sample, hardness measurements were performed three times at 1 mm intervals in the depth direction of the target using a Mitutoyo Vickers hardness tester "HM-200" under a load of 1 kg for a loading time of 15 seconds. The average value of the obtained values was calculated. The average values calculated for each sample were added together and divided by the number of samples to obtain the hardness of the molybdenum target according to the present invention. Furthermore, the standard deviation of the molybdenum target according to the present invention was determined by adding the standard deviations calculated for each sample and dividing the sum by the number of samples.
[0077] (Crystal Grain Size) Samples measuring 10 × 10 × 6 mm were taken from the center, edge, and halfway along the line connecting the center and edge of the obtained molybdenum target. The cross section of each sample was polished and etched, and images were taken at 1 mm intervals in the depth direction of the target using a Keyence Corporation optical microscope "Digital Microscope VHX-6000." The equivalent circle diameters were then determined using image analysis software "Image-j," and the average value was calculated. The average values calculated for each test piece were added together and divided by the number of samples, resulting in the average grain size of the molybdenum target according to the present invention. Furthermore, the standard deviation of the molybdenum target according to the present invention was determined by adding the standard deviations determined for each sample and dividing the sum by the number of samples.
[0078] (Oxygen Content) When the molybdenum sintered body was processed into a target shape, an analysis sample was taken and the oxygen content of the compact was measured. The oxygen content was analyzed using an analyzer "TC-600" manufactured by LECO Corporation.
[0079] (Carbon Content) When the molybdenum sintered body was processed into a target shape, an analytical sample was taken and the carbon content of the compact was measured. The carbon content was analyzed using an analyzer "EMIA-320V" manufactured by Horiba, Ltd.
[0080] (Pore) Samples measuring 10 × 10 × 6 mm were taken from the center, edge, and halfway along the line connecting the center and edge of the resulting sputtering target. After polishing the cross section of each sample, two SEM images were taken at 1 mm intervals in the depth direction of the target using a Hitachi High-Technologies Corporation electron microscope "TM4000Plus." The pore area of the taken SEM images was determined using image analysis software "Image-j," and the size and number of pores in each sample were calculated. The size and number of pores determined for each sample were added together and divided by the number of samples to determine the size and number of pores in the molybdenum target according to the present invention.
[0081] Furthermore, using the obtained targets of the examples and comparative examples, films were formed as follows, and the resistivity of the films was measured as follows, and particles were evaluated as follows.
[0082] The results of Examples 1 to 4 and Comparative Examples 1 to 13 are shown in Table 3, and the relationship between the number of pores of a predetermined size and the number of particles is shown in Figures 1 to 3. Resistivity of 11 μΩ cm or less was marked as ○, and that exceeding 11 μΩ cm was marked as ×. If the resistivity is 11 μΩ cm or less, low-resistance LSI wiring can be formed, making it possible to realize devices with low power consumption. Film thickness distribution of 2% or less was marked as ○, and that exceeding 2% was marked as ×. Film thickness distribution of 2% or less allows for the stable production of devices with little variation in performance and quality.
[0083] (Specific Resistivity Measurement) The obtained molybdenum target was bonded to an aluminum alloy backing plate with an In-based brazing material to form a sputtering cathode. The sputtering cathode was assembled into an ENTRON (registered trademark) sputtering device manufactured by ULVAC, Inc., and a molybdenum thin film with a thickness of 10 nm was formed on a semiconductor wafer with a diameter of 300 mm. The sputtering conditions were as follows: ultimate pressure: 1 × 10 -5 Pa, discharge method: DC, power: 4 kW, gas source: Ar, gas flow rate: 150 sccm, film formation temperature: 200° C., sputtering time: 5 seconds, distance between target and wafer: 60 mm.
[0084] The film thickness of nine points on the molybdenum thin film on the wafer was measured using an "S-MAT2300" manufactured by TECHNORAYS, and the sheet resistance was measured using an "OmniMap RS100" manufactured by KLATencor, to calculate the resistivity (μΩ cm) of the thin film, and the average value was taken as the resistivity of the molybdenum thin film.
[0085] (Measurement of Particles) The surface of the molybdenum thin film on a semiconductor wafer with a diameter of 300 mm was inspected using a surface inspection device "WM-10" manufactured by TOPCON Corporation, which was used for resistivity measurement, and the number of particles with a size of 0.065 μm or more was counted. 2This is the number of winning balls, and 20 or less is considered to be preferable, and 15 or less is considered to be more preferable.
[0086] (Measurement of Film Thickness Distribution) The film thickness of the molybdenum thin film on the wafer was measured at 49 points using an S-MAT2300 manufactured by TECHNORAYS, and calculated using the following formula: Film Thickness Distribution (%) = (Maximum Value - Minimum Value) / (Maximum Value + Minimum Value) x 100
[0087]
[0088]
[0089]
[0090] As shown in Examples 1 to 4, the tungsten content is 10 ppm to 100 ppm, the molybdenum content excluding the tungsten and gas content is 99.999 mass% or more (purity 5N), and the average particle size D obtained by the laser diffraction / scattering method is Ave The median diameter D50 is 2.0 to 3.5, and the median diameter D90 and the average particle diameter D Ave The ratio of D90 to D Ave ) is 1.7 or less, and the median diameter D95 and the average particle diameter D Ave The ratio of D95 / D Ave A molybdenum powder having a porosity of 2.0 or less was used, and the powder was hot pressed at a temperature of 1400°C to 1500°C, and then subjected to HIP at a temperature of 1500°C to 1600°C, thereby obtaining a molybdenum sintered body. The obtained molybdenum sintered body had a relative density of 99% or more and a surface roughness of 0.15 mm 2 In the observation area of 0.01 μm 2 0.2 μm or more 2 There are 20 or less pores with a size of less than 0.2 μm 2 More than 1.8 μm 2 There are five or fewer pores with a size of less than 1.8 μm 2 It is possible to obtain a molybdenum target having one or less pores of the above size. By using such a molybdenum target, it is possible to suppress particle generation and stably form a high-quality molybdenum thin film.
[0091] In addition, in Examples 1 to 4, the hot pressing temperature is low at 1500° C. or less, so the carbon content of the target is sufficiently low, and a thin film having a sufficiently low resistivity of 11 μΩ·cm or less can be formed.
[0092] In Comparative Example 1, the powder was too fine and had a high oxygen content, resulting in a rapid increase in density during HP, leading to oxide trapping. In Comparative Example 2, HIP was not performed, resulting in insufficient density. In Comparative Examples 3 and 4, the tungsten and oxygen contents were high, resulting in high resistivity. Furthermore, the raw material powder was too fine, resulting in a rapid increase in density during HP, and the HP temperature was low, resulting in oxides not sublimating but remaining. In Comparative Example 3, the HIP temperature was high, resulting in abnormal grain growth, and in Comparative Example 4, the HIP temperature was low, resulting in low density. In Comparative Examples 5 and 6, the tungsten and oxygen contents were high, resulting in high resistivity. Furthermore, the powder was too fine and had a high oxygen content, resulting in a rapid increase in density during HP, leading to oxide trapping. Furthermore, the HIP temperature was low, resulting in low density. In Comparative Example 7, the oxygen content was high, resulting in high resistivity, and the raw material powder was too fine, resulting in a rapid increase in density during HP, resulting in some oxides remaining. In Comparative Example 8, the high oxygen content resulted in high resistivity, and the raw material powder was too fine, causing a sudden increase in density during HP, resulting in some residual oxides. Furthermore, the high HIP temperature caused abnormal grain growth, resulting in a large aspect ratio. In Comparative Examples 9 to 11, the raw material powder was too coarse, resulting in insufficient density. Furthermore, in Comparative Example 11, insufficient particle size adjustment resulted in uneven grain size and a large aspect ratio, resulting in insufficient density. In Comparative Example 12, the high HIP temperature caused abnormal grain growth, resulting in a large aspect ratio. Furthermore, the coarse raw material powder also resulted in insufficient density. In Comparative Example 13, the high HP temperature resulted in a large amount of carbon diffusion. Furthermore, insufficient adjustment of the raw material particle size distribution resulted in uneven grain size and a large aspect ratio, resulting in insufficient density due to the coarse powder.
Claims
1. A molybdenum target formed of a sintered body of molybdenum powder, having a relative density of 99% or more, an oxygen content of 25 ppm or less, a carbon content of 30 ppm or less, a tungsten content of 10 ppm to 100 ppm, a molybdenum content excluding the oxygen content, the carbon content, and the tungsten content of 99.999 mass% or more, and a diameter of 0.15 mm 2 In the observation area of 0.01 μm 2 0.2 μm or more 2 There are 20 or less pores with a size of less than 0.2 μm 2 More than 1.8 μm 2 There are 5 or less pores with a size of less than 1.8 μm 2 A molybdenum target having one or less pores of this size or larger.
2. Average particle size d calculated using the equivalent circle diameter Ave is 20 μm or more and 100 μm or less, and the standard deviation 3σ of the particle size calculated using the circle equivalent diameter and the average particle size d Ave Ratio to (3σ / d Ave 2. The molybdenum target according to claim 1, wherein the molybdenum content is 1.2 or less.
3. The molybdenum target according to claim 2, wherein the aspect ratio of the grain size d is less than 1.
2.
4. The average value of Vickers hardness is 180 or less, and the standard deviation of Vickers hardness 3σ and the average value of Vickers hardness H Ave Ratio to (3σ / H Ave 4. The molybdenum target according to claim 1, wherein the molybdenum content is 0.07 or less.
5. Average particle size D obtained by laser diffraction / scattering method Ave The median diameter D50 is 2.0 to 3.5, and the median diameter D90 and the average particle diameter D Ave The ratio of D90 to D Ave ) is 1.7 or less, and the median diameter D95 and the average particle diameter D Ave The ratio of D95 / D Ave ) is 2.0 or less, hot-pressed at a temperature of 1400° C. or more and 1500° C. or less, and then sintered by hot isostatic pressing at a temperature of 1500° C. or more and 1600° C. or less.
6. The method for producing a molybdenum target according to claim 5, wherein the molybdenum powder has a tungsten content of 10 ppm to 100 ppm, and a molybdenum content excluding the oxygen content, the carbon content and the tungsten content is 99.999 mass % or more.
7. The method for producing a molybdenum target according to claim 5 or 6, wherein the hot pressing is carried out under high vacuum at a holding temperature of 1400 to 1500° C. for a holding time of 360 to 600 minutes.
Citation Information
Patent Citations
Dense sintered compact of ferroelectric oxide and its production
JP1999240720A
Molybdenum sputtering target material and its production
JP2000234167A
Sputtering target material
JP2000319774A
Method of producing molybdenum target for sputtering and molybdenum target
JP2003342720A
METHOD FOR PRODUCING INTEGRALLY SINTERED Mo BASED TARGET MATERIAL, AND INTEGRALLY SINTERED Mo BASED TARGET MATERIAL
JP2005344136A