A friction nano-electricity generating composite yarn and its preparation method and application

By adopting a three-layer structure design in the friction nanoelectric generator yarn, using the combination of conductive yarn, nanofiber yarn and hydrophobic polyester microfiber, the problems of low output performance and insufficient wear resistance of traditional friction nanoelectric generator yarns are solved, and the problem of low output performance and insufficient wear resistance is achieved. High strength, high wear resistance and high electrical performance output.

CN115323552BActive Publication Date: 2024-11-22XI'AN POLYTECHNIC UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211057617.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-08-31
Publication Date
2024-11-22
Estimated Expiration
2042-08-31

AI Technical Summary

Technical Problem

Traditional friction nanogenerating yarns have low output performance and insufficient wear resistance, which cannot meet the wear needs of wearable electronic products in daily sports.

Method used

The nanofiber yarns of conductive yarns are coated by double-electrode electrospinning method, and the hydrophobic polyester microfibers are used as the outer layer to form a three-layer structure from the inside to the outside: the conductive yarns are used as the electrode layer and the nanofiber yarns are used as the outer layer. Charge storage layer and hydrophobic polyester microfibers are used as charge generation layers.

Benefits of technology

Improves triboelectric output performance, enhances the wear resistance, comfort and water washing durability of composite yarns, ensuring that mechanical energy can still be collected and high electrical output can be maintained in water drop environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115323552B_ABST
    Figure CN115323552B_ABST
Patent Text Reader

Abstract

The present invention discloses a friction nano-power generation composite yarn and a preparation method and application thereof. The method comprises preparing nanofiber coated yarn, preparing hydrophobic polyester roving and preparing friction nano-power generation composite yarn. The composite yarn prepared by the present invention has a three-layer structure. The inner layer is a light and soft conductive yarn as an electrode layer; the middle layer is a PA11 / nano zinc oxide nanofiber yarn, which has the characteristics of nanoscale diameter, high surface area, high porosity and small pore size, and as the middle layer, has the function of retaining more friction charges and reducing charge neutralization; the outer layer is a hydrophobically finished polyester yarn, which not only has high strength, good wear resistance and good water washability, but also the hydrophobic treatment enables it to still collect mechanical energy in a water drop environment and maintain performance electrical output. The composite yarn can be used as a yarn raw material for two-dimensional braided and knitted fabrics.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of friction nano power generation, and in particular to a friction nano power generation composite yarn with enhanced friction electric output and wear resistance, and a preparation method and application thereof. Background Art

[0002] Nowadays, with the development of modern industries and multidisciplinary fields such as the Internet of Things, big data, and artificial intelligence, functional wearable electronic products are developing rapidly. Multifunctional wearable electronic products are widely used in personal health management, motion detection, smart fabrics, etc. In recent years, based on the principles of friction electrification and electrostatic induction, friction nanogenerators can collect random, low-frequency environmental mechanical energy to power wearable electronic products. The human body itself is a rich source of green mechanical energy and an application of smart wearable electronics. Through the seamless combination of friction nanogenerator textiles and human movement, energy acquisition and utilization can be achieved.

[0003] At present, the output performance of traditional friction-generated yarn is low and its function is single. As an energy collector, the friction nanogenerator converts the body's mechanical energy into electrical energy, and its core lies in the output performance. In order to broaden the application field by improving the electrical output performance, researchers have proposed various methods, including material selection, process design, optimization of friction materials, design of multilayer structures, and addition of nanoparticles. The charge transfer mechanism of the friction nanogenerator is caused by the different affinity of materials for electrons. The friction materials ranked at the front of the friction sequence list are considered to be ideal choices, such as PDMS, PA, PET and PTFE. In addition, the researchers proved that materials such as PI, PP, and PA as dielectric layers can capture charges and store them in deep well layers by designing multilayer structures, thereby reducing charge dissipation and improving the surface potential.

[0004] At present, most friction nanogenerator yarns are prepared by selecting the electrospinning process and adding nanoparticles. Because electrospun nanofibers have the characteristics of large porosity and large specific surface area, they can increase the friction charge density and the yarns made are easy to combine with textiles. However, the nanostructure is easily worn due to its fragile interface. As wearable electronic textiles need to withstand the wear of the actual movement of the human body in daily life, nanofibers cannot meet the wear resistance requirements. The most critical factor in wear resistance lies in the type of material. Textile materials such as nylon and polyester are considered to be ideal wear-resistant materials. Comfort performance is another major comprehensive experience indicator of clothing. Therefore, it is necessary to develop a wear-resistant, high-strength, comfortable, hydrophobic, and high-electrical performance output friction generator yarn. Summary of the invention

[0005] In view of the deficiencies in the prior art, the technical problem to be solved by the present invention is to provide a friction nano-electricity composite yarn and a preparation method and application thereof.

[0006] The technical solution of the present invention to solve the technical problem of the method is to provide a method for preparing a friction nano-electricity composite yarn, characterized in that the method comprises the following steps:

[0007] (1) preparing nanofiber coated yarn: using PA11 / nano zinc oxide solution as the electrospinning solution for the positive and negative electrodes and the conductive yarn as the core yarn, and adopting a double-electrode electrospinning method to spin-coat the nanofiber yarn formed by the PA11 / nano zinc oxide solution on the outer surface of the conductive yarn to form the nanofiber coated yarn;

[0008] (2) preparing hydrophobic polyester roving: using polyester staple fibers as raw materials, sequentially opening, carding and drawing the polyester staple fibers to obtain polyester slivers; then subjecting the polyester slivers to hydrophobic finishing to obtain hydrophobic polyester slivers; then spinning the hydrophobic polyester slivers into roving to obtain hydrophobic polyester roving;

[0009] (3) Preparation of friction nano-electricity generation composite yarn: using nanofiber-coated yarn as core yarn and hydrophobic polyester roving as outer yarn, the hydrophobic polyester micron fiber formed by the hydrophobic polyester roving is twisted and coated on the outer surface of the nanofiber-coated yarn by a ring spinning process to obtain friction nano-electricity generation composite yarn.

[0010] The technical solution of the present invention to solve the technical problem of the composite yarn is to provide a friction nano-power generation composite yarn prepared by the preparation method, characterized in that the composite yarn has a three-layer structure from inside to outside; the inner layer is conductive yarn, which serves as an electrode layer; the middle layer is nanofiber yarn, which serves as a charge storage layer; and the outer layer is hydrophobic polyester micron fiber, which serves as a charge generation layer.

[0011] The technical solution of the present invention to solve the application technical problem is to provide an application of the friction nano-electricity generation composite yarn, characterized in that the composite yarn is used as a yarn raw material for two-dimensional woven fabrics and knitted fabrics.

[0012] Compared with the prior art, the present invention has the following beneficial effects:

[0013] (1) The composite yarn of the present invention has high strength, high wear resistance, comfort, high hydrophobicity, water washing durability and high electrical performance output, and can enhance the triboelectric output, thereby enhancing the power generation performance of the composite yarn.

[0014] (2) The composite yarn of the present invention has a three-layer structure. The inner layer is a light and soft conductive yarn as the electrode layer; the middle layer is a PA11 / nano zinc oxide nanofiber yarn, which has the characteristics of nanoscale diameter, high surface area, high porosity and small pore size. As the middle layer, it has the function of retaining more friction charges and reducing charge neutralization; the outer layer is a hydrophobic polyester yarn, which is not only high in strength, good in wear resistance and good in water washability, but also hydrophobic treatment enables it to still collect mechanical energy in a water drop environment and maintain performance electrical output. At the same time, the polyester yarn is soft and skin-friendly, and the human body feels comfortable when wearing it.

[0015] (3) The composite yarn of the present invention comprises nanometer-level nanofiber yarn and micrometer-level hydrophobic polyester micron fiber, and the various properties of the composite yarn are further enhanced through the nanometer-micrometer size gradient structure.

[0016] (4) The preparation process of the present invention combines electrospinning, impregnation-drying and ring spinning processes, the preparation method is simple to operate and the parameters are easy to control. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 It is a schematic diagram of the preparation process of the nanofiber coated yarn of the present invention;

[0018] Figure 2 It is a schematic diagram of the preparation process of twisting and coating the hydrophobic polyester micron fiber on the nanofiber coated yarn of the present invention;

[0019] Figure 3 This is a surface SEM image of the nanofiber coated yarn prepared in Example 1 of the present invention;

[0020] Figure 4 This is a surface SEM image of the hydrophobic polyester sliver prepared in Example 1 of the present invention;

[0021] Figure 5 This is a surface morphology image of the composite yarn prepared in Example 1 of the present invention;

[0022] Figure 6 This is a cross-sectional morphology diagram of the composite yarn prepared in Example 1 of the present invention;

[0023] Figure 7 The voltage output diagrams are of the composite yarn and nanofiber coated yarn prepared in Example 1 of the present invention and the ring spun core-spun yarn prepared in Comparative Example 1;

[0024] Figure 8 Current output diagrams of the composite yarn and nanofiber coated yarn prepared in Example 1 of the present invention and the ring-spun core-spun yarn prepared in Comparative Example 1;

[0025] Fig. 9The tensile performance diagram of the composite yarn and nanofiber coated yarn prepared in Example 1 of the present invention and the ring spun core-spun yarn prepared in Comparative Example 1;

[0026] Fig.10 This is a test diagram of the wear resistance of the composite yarn and nanofiber coated yarn prepared in Example 1 of the present invention and the ring-spun core-spun yarn prepared in Comparative Example 1;

[0027] Fig.11 Surface morphology of the composite yarn prepared in Example 1 of the present invention under different wear cycles;

[0028] Fig.12 This is a graph showing the washing performance of the composite yarn prepared in Example 1 of the present invention;

[0029] Fig.13 This is a diagram of the hydrophobic performance of the composite yarn prepared in Example 1 of the present invention;

[0030] Fig.14 This is a test performance diagram of the current output of the composite yarn prepared in Example 1 of the present invention after dripping 0.22g of water;

[0031] Fig.15 This is a test performance diagram of the current output of the composite yarn prepared in Example 1 of the present invention after dripping 0.44g of water

[0032] Fig.16 This is a physical picture of the electronic textile prepared in Example 1 of the present invention;

[0033] Fig.17 This is a voltage output performance diagram of the electronic textile prepared in Example 1 of the present invention;

[0034] Fig.18 This is a graph showing the current output performance of the electronic textile prepared in Example 1 of the present invention;

[0035] Fig.19 This is a graph showing the charge output performance of the electronic textile prepared in Example 1 of the present invention;

[0036] Fig. 20 This is a diagram of charging a commercial capacitor when the electronic fabric prepared in Example 1 of the present invention is tapped;

[0037] Fig.21 This is a graph showing the air permeability of the electronic fabric prepared in Example 1 of the present invention;

[0038] Fig. 22 This is a diagram of the moisture permeability performance of the electronic fabric prepared in Example 1 of the present invention;

[0039] Fig.23 This is a graph showing the performance of the composite yarn prepared in Example 1 of the present invention as a self-powered sensor for detecting finger straightening performance;

[0040] Fig.24 This is a graph showing the performance of the electronic textile prepared in Example 1 of the present invention as a self-powered sensor for detecting elbow bending;

[0041] Fig.25 A diagram showing the performance of the electronic textile prepared in Example 1 of the present invention being used as a self-powered sensor to detect knee bending. DETAILED DESCRIPTION

[0042] The specific embodiments of the present invention are given below. The specific embodiments are only used to further illustrate the present invention in detail and do not limit the protection scope of the claims of the present invention.

[0043] The present invention provides a method for preparing a friction nano-electricity composite yarn (hereinafter referred to as the method), characterized in that the method comprises the following steps:

[0044] (1) Preparation of nanofiber coated yarn:

[0045] Using PA11 / nano zinc oxide solution as the electrospinning solution of positive and negative electrodes and conductive yarn as the core yarn, a double-electrode electrospinning method is used to spin-coat the nanofiber yarn formed by the PA11 / nano zinc oxide solution on the outer surface of the conductive yarn, so that the nanofiber yarn is oriented, which is beneficial to improve the mechanical properties of the nanofiber yarn and form a nanofiber-coated yarn;

[0046] Preferably, in step (1), the diameter of the conductive yarn is 0.5 to 1.0 mm, and the conductivity is not less than 2.3×10 7 S / m; Use lightweight and soft conductive yarn, preferably copper wire, silver wire or gold-plated tungsten wire.

[0047] Preferably, in step (1), the electrospinning solution is prepared by ultrasonically dissolving nano zinc oxide in HFIP (hexafluoroisopropanol); then adding PA11 (nylon 11) particles, stirring and dissolving, to obtain a homogeneous PA11 / nano zinc oxide solution.

[0048] Preferably, in step (1), in the preparation of the electrospinning solution, the ultrasonic dissolution time is 50 to 70 minutes, the temperature is 20 to 30°C, and the ultrasonic frequency is 40kHz; the stirring dissolution time is 1.8 to 2.5 hours, the temperature is 60 to 65°C, and the rotation speed is 55 to 60 r / min.

[0049] Preferably, in step (1), in the electrospinning solution, the concentration of PA11 is 6-15wt% (preferably 9-15wt%, more preferably 9wt%), and the concentration of nano zinc oxide is 1-7wt% (preferably 2-5wt%, more preferably 3wt%).

[0050] Preferably, in step (1), the process parameters of the dual-electrode electrospinning are: the positive electrode voltage is 5 to 6 V, the negative electrode voltage is -5 to -6 V, the rotation speed of the rotating collection device is 200 to 600 r / min, preferably 300 to 500 r / min; the moving speed of the conductive yarn is 0.05 to 0.3 mm / s, preferably 0.1 mm / s; the jet flow rate of the electrospinning solution of the positive and negative electrodes is 0.01 to 0.05 mL / h (preferably 0.03 to 0.05 mL / h), preferably the jet flow rate of the electrospinning solution of the positive and negative electrodes is the same and is 0.03 mL / h.

[0051] Preferably, in step (1), the diameter of a single nanofiber of the nanofiber yarn is 685-750 nm, preferably 700-735 nm; the average diameter of the nanofiber coated yarn is 0.43-1.34 mm, preferably 0.9-1.2 mm.

[0052] (2) Preparation of hydrophobic polyester roving:

[0053] The polyester staple fibers are used as raw materials, and the polyester staple fibers are sequentially opened, carded into strips, and drawn to obtain polyester slivers; the polyester slivers are then subjected to hydrophobic finishing to form a hydrophobic film on the outer surface of the polyester slivers to obtain hydrophobic polyester slivers; the hydrophobic polyester slivers are then spun through a roving machine to obtain rovings, and micron-level hydrophobic polyester rovings are obtained as outer covering yarns;

[0054] Preferably, in step (2), when combing into slivers, the rotation speeds of the cylinder and the doffer are both selected to be low (i.e., 118-150 r / min) to ensure uniform combing of the short fibers. During drawing, the drafting multiple of the drawing frame is 5-7, preferably 6 times; the use of the drawing frame to draw and draft the fibers in order is beneficial to improving the mechanical properties of the polyester sliver.

[0055] Preferably, in step (2), the polyester sliver is immersed in a hydrophobic finishing agent at room temperature for 10 to 25 minutes (preferably 20 minutes), and then dried at a temperature of 100 to 150° C. (preferably 120° C.) for 15 to 30 minutes (preferably 20 minutes) to obtain a hydrophobic polyester sliver; the hydrophobic finishing agent is a silicone finishing agent.

[0056] Preferably, in step (2), when spinning the roving, the drafting multiple is 7 to 9 (preferably 7 times), the preparation process is strictly controlled, and the dry basis weight of the obtained hydrophobic polyester roving is 4 to 5 g / 10m.

[0057] Preferably, in step (2), the single fiber diameter of the hydrophobic polyester roving is 10 to 15 μm.

[0058] (3) Preparation of friction nano-electricity composite yarn:

[0059] The nanofiber coated yarn and the hydrophobic polyester roving are respectively wound on two yarn tubes of a ring spinning machine, with the nanofiber coated yarn as the core yarn and the hydrophobic polyester roving as the outer yarn. The hydrophobic polyester micron fiber formed by the hydrophobic polyester roving is twisted and coated on the outer surface of the nanofiber coated yarn using the ring spinning process on the ring spinning machine to obtain a three-layer friction nano power generation composite yarn (referred to as composite yarn).

[0060] Preferably, in step (3), the ring spinning process is: feeding the hydrophobic polyester roving from the rear jaw of the rear roller, passing through the rear roller, the middle roller and the front roller in sequence, and then outputting from the front jaw of the front roller to form hydrophobic polyester micron fiber; feeding the nanofiber coated yarn from the rear jaw of the front roller, and then outputting from the front jaw of the front roller; then, the nanofiber coated yarn and the hydrophobic polyester micron fiber are assembled in the front area, the hydrophobic polyester micron fiber is twisted and coated on the outer surface of the nanofiber coated yarn, and then wound on the bobbin through a steel wire ring to form a three-layer structure of friction nano power generation composite yarn.

[0061] The present invention also provides a friction nano-power generation composite yarn (referred to as composite yarn) prepared by the preparation method, characterized in that the composite yarn has a three-layer structure from inside to outside; the inner layer is conductive yarn, which serves as an electrode layer; the middle layer is electrostatically spun nanofiber yarn, which serves as a charge storage layer; and the outer layer is hydrophobic polyester micron fiber, which serves as a charge generation layer.

[0062] Preferably, the average diameter of the composite yarn is 1.4-1.8 mm.

[0063] Preferably, the mass of the hydrophobic polyester micron fiber accounts for 8-15% of the total mass of the composite yarn; the mass ratio of the hydrophobic polyester micron fiber to the conductive yarn is 0.5-1:1 (preferably 0.6-0.7:1).

[0064] The present invention also provides an application of the composite yarn, characterized in that the composite yarn is used as a yarn raw material for two-dimensional braided fabrics and knitted fabrics;

[0065] When the composite yarn is used as the raw material of a two-dimensional braided fabric, the specific two-dimensional braiding process is: the composite yarn is wound on the spindle of a two-dimensional braiding machine, the spandex fiber bundle is used as the core layer, and the composite yarn is coated on the outside of the spandex fiber bundle through a two-dimensional braiding process to obtain a two-dimensional braided fabric with extensibility. Preferably, the rotation speed of the two-dimensional braiding machine is 10 to 15 r / min. The spandex fiber bundle is composed of 1 to 5 70D spandex monofilaments.

[0066] When the composite yarn is used as the raw material of knitted fabric, the knitted fabric is made by a hand-cranked horizontal loom through a conventional knitting process.

[0067] In the following examples, PDMS is fixed to one end of the exciter, and the contact and separation frequency (2-4 Hz) between PDMS and the sample to be tested is controlled by setting the moving acceleration of the exciter. The conductive yarn is connected to the test end of the electrometer, and the voltage, charge and current of the composite yarn are tested and read using the electrometer.

[0068] Example 1

[0069] (1) Preparation of nanofiber coated yarn:

[0070] Add nano zinc oxide to HFIP, and ultrasonically treat it for 60 minutes at 25°C to obtain a nano zinc oxide solution with a mass fraction of 3%; then add PA11 particles to the nano zinc oxide solution, and stir and dissolve it at 65°C for 2 hours to obtain a PA11 / nano zinc oxide solution with a mass fraction of 6% of PA11;

[0071] Then, PA11 / nano zinc oxide solution was used as the electrospinning solution for the positive and negative electrodes, and copper wire was used as the core yarn. The double-electrode electrospinning technology was adopted to adjust the electrospinning parameters (positive electrode voltage was 5V, negative electrode voltage was -5V, the rotation speed of the rotating collection device was 300r / min, the moving speed of the conductive yarn was 0.1mm / s, and the injection flow rate was 0.03mL / h), and the copper wire was rotationally coated by a conventional nozzle-type electrospinning device to form nanofiber coated yarn;

[0072] (2) Preparation of hydrophobic polyester roving:

[0073] The polyester staple fibers are opened, carded and drawn in sequence to obtain polyester slivers; when carding, the rotation speeds of the cylinder and the doffer are both low; when drawing, the drafting multiple of the drawing frame is 6 times;

[0074] The polyester sliver is immersed in the silicone finishing agent for 20 minutes, and then dried at 120°C for 20 minutes to obtain a hydrophobic polyester sliver; the hydrophobic polyester sliver is then spun into roving by a roving machine, and then wound to obtain a hydrophobic polyester roving; when the roving is spun, the drafting multiple is 7 times, and the roving dry weight is 5g / 10m;

[0075] (3) Preparation of friction nano-electricity generation composite yarn: The nanofiber-coated yarn and the hydrophobic polyester roving are respectively wound on two yarn tubes of a ring spinning machine, with the nanofiber-coated yarn as the core yarn and the hydrophobic polyester roving as the outer yarn. The hydrophobic polyester micron fiber formed by the hydrophobic polyester roving is twisted and coated on the outer surface of the nanofiber-coated yarn through the ring spinning machine to obtain a three-layer friction nano-electricity generation composite yarn.

[0076] Depend on Figure 3 It can be seen that PA11 and nano zinc oxide have good spinnability, and the nanofibers form a large specific surface area and porosity.

[0077] Depend on Figure 4 It can be seen that after the hydrophobic finishing, a hydrophobic film is formed on the outer surface of the polyester sliver.

[0078] Depend on Figure 5 It can be seen that the hydrophobic polyester microfibers in the outermost layer of the composite yarn are tightly wrapped around the nanofibers in the middle layer.

[0079] Depend on Figure 6 It can be seen that the composite yarn has a uniform and compact three-layer coaxial coating structure.

[0080] Depend on Figure 7 It can be seen that the output voltage of the composite yarn is higher than that of the nanofiber coated yarn obtained in step (1) and the ring spun core yarn of comparative example 1, and the voltage is 2 times and 1.5 times that of the nanofiber coated yarn and the ring spun core yarn, respectively.

[0081] Depend on Figure 8 It can be seen that the output current of the composite yarn is higher than that of the nanofiber coated yarn obtained in step (1) and the ring spun core yarn of comparative example 1, and the current is 2 times and 1.5 times that of the nanofiber coated yarn and the ring spun core yarn, respectively.

[0082] Depend on Fig. 9 It can be seen that the tensile strength of the composite yarn is higher than that of the nanofiber coated yarn obtained in step (1) and the ring spun core yarn of comparative example 1.

[0083] Depend on Fig.10 It can be seen that the wear resistance of the composite yarn is higher than that of the nanofiber coated yarn obtained in step (1) and the ring-spun core-spun yarn of comparative example 1. The composite yarn can withstand 4500 wears, while the nanofiber coated yarn obtained in step (1) can only withstand 550 wears, and the ring-spun core-spun yarn of comparative example 1 can only withstand 3000 wears.

[0084] Depend on Fig.11 It can be seen that the surface morphology of the composite yarn under different abrasion times remains good and wear-free, and the middle layer still maintains a good morphological structure after 4000 friction and wear times.

[0085] Depend on Fig.12 It can be seen that the electrical output voltage of the composite yarn remains basically unchanged during and after 10 washings, and it still has stable electrical performance output, which is washable and stable.

[0086] Depend on Fig.13 It can be seen that the composite yarn has excellent hydrophobicity, with a water contact angle of 157°.

[0087] Depend on Fig.14 It can be seen that the composite yarn does not affect the current output after a 0.22g water drop is dropped. Fig.15It can be seen that the composite yarn does not affect the current output after a 0.44g water drop is dropped. The composite yarn still maintains high electrical performance output after being dropped with water.

[0088] Depend on Fig.16 It can be seen that ordinary cotton yarn is first selected for yarn feeding, the needles are cast on and 8-10 rows are woven, and then the composite yarn is introduced through the hand-cranked horizontal loom for normal weaving, the composite yarn is woven for 10 rows, and then ordinary cotton yarn is introduced to weave 8-10 rows, and finally the needles are closed to obtain the electronic fabric.

[0089] Depend on Fig.17 It can be seen that the voltage output of the electronic fabric at 2-4Hz can reach 55V.

[0090] Depend on Fig.18 It can be seen that the current output of the electronic fabric at 2-4 Hz can reach 0.67 μA.

[0091] Depend on Fig.19 It can be seen that the electronic fabric has a charge output of 2 to 4 Hz and a charge transfer amount of up to 16.5 nC.

[0092] Depend on Fig. 20 It can be seen that the electricity generated by flapping the electronic fabric can charge commercial capacitors of different capacities, and the larger the capacitor capacity, the slower the charging rate.

[0093] Depend on Fig.21 and 22 It can be seen that the air permeability and moisture permeability of electronic fabrics are between those of cotton fabrics, polyester fabrics and denim fabrics. They have excellent air permeability and moisture permeability, excellent wearable comfort, and can be used as electronic products for long-term wear.

[0094] Depend on Figure 23-25 It can be seen that the composite yarn can be used as a self-powered sensor to monitor the movement of the finger straightening, and the electronic fabric can be used as a self-powered sensor to monitor the movement of the elbow bending and knee bending, respectively. This shows that the composite yarn and the electronic fabric made of the composite yarn can be used as self-powered sensors for human motion detection.

[0095] Comparative Example 1

[0096] (1) Preparation of hydrophobic polyester roving: exactly the same as step (2) of Example 1;

[0097] (2) Preparation of ring-spun core-spun yarn: Copper wire (the same copper wire as in Example 1) and hydrophobic polyester roving are respectively wound on two yarn tubes of a ring spinning machine, with the copper wire as the core yarn and the hydrophobic polyester roving as the outer covering yarn. The hydrophobic polyester micron fiber formed by the hydrophobic polyester roving is twisted and coated on the outer surface of the copper wire by the ring spinning machine using a ring spinning process to obtain the ring-spun core-spun yarn.

[0098] Step (2) specifically comprises: feeding the hydrophobic polyester roving from the rear jaw of the rear roller, passing through the rear roller, the middle roller and the front roller in sequence, and then outputting from the front jaw of the front roller to form the hydrophobic polyester micron fiber; feeding the copper wire from the rear jaw of the front roller, and then outputting from the front jaw of the front roller; and then gathering the copper wire and the hydrophobic polyester micron fiber in the front area, twisting and coating the hydrophobic polyester micron fiber on the outer surface of the copper wire, and then winding it on the bobbin through a steel wire ring to form the ring spun core-spun yarn.

[0099] Example 2

[0100] (1) Preparation of nanofiber coated yarn:

[0101] Add nano zinc oxide to HFIP, and ultrasonically treat it for 60 minutes at 25°C to obtain a nano zinc oxide solution with a mass fraction of 3%; then add PA11 particles to the nano zinc oxide solution, and stir and dissolve it at 65°C for 2 hours to obtain a PA11 / nano zinc oxide solution with a mass fraction of 9% of PA11;

[0102] Then, PA11 / nano zinc oxide solution was used as the electrospinning solution for the positive and negative electrodes, and copper wire was used as the core yarn. The double-electrode electrospinning technology was adopted to adjust the electrospinning parameters (positive electrode voltage was 5V, negative electrode voltage was -5V, the rotation speed of the rotating collection device was 300r / min, the moving speed of the conductive yarn was 0.1mm / s, and the injection flow rate was 0.03mL / h), and the copper wire was rotationally coated by a conventional nozzle-type electrospinning device to form nanofiber coated yarn;

[0103] (2) Preparation of hydrophobic polyester roving:

[0104] The polyester staple fibers are opened, carded and drawn in sequence to obtain polyester slivers; when carding, the rotation speeds of the cylinder and the doffer are both low; when drawing, the drafting multiple of the drawing frame is 6 times;

[0105] The polyester sliver is immersed in the silicone finishing agent for 20 minutes, and then dried at 120°C for 20 minutes to obtain a hydrophobic polyester sliver; the hydrophobic polyester sliver is then spun into roving by a roving machine, and then wound to obtain a hydrophobic polyester roving; when the roving is spun, the drafting multiple is 7 times, and the roving dry weight is 5g / 10m;

[0106] (3) Preparation of friction nano-electricity generation composite yarn: The nanofiber-coated yarn and the hydrophobic polyester roving are respectively wound on two yarn tubes of a ring spinning machine, with the nanofiber-coated yarn as the core yarn and the hydrophobic polyester roving as the outer yarn. The hydrophobic polyester micron fiber formed by the hydrophobic polyester roving is twisted and coated on the outer surface of the nanofiber-coated yarn through the ring spinning machine to obtain a three-layer friction nano-electricity generation composite yarn.

[0107] Example 3

[0108] (1) Preparation of nanofiber coated yarn:

[0109] Add nano zinc oxide to HFIP, and ultrasonically treat it for 60 minutes at 25°C to obtain a nano zinc oxide solution with a mass fraction of 3%; then add PA11 particles to the nano zinc oxide solution, and stir and dissolve it at 65°C for 2 hours to obtain a PA11 / nano zinc oxide solution with a mass fraction of 12% of PA11;

[0110] Then, PA11 / nano zinc oxide solution was used as the electrospinning solution for the positive and negative electrodes, and copper wire was used as the core yarn. The double-electrode electrospinning technology was adopted to adjust the electrospinning parameters (positive electrode voltage was 5V, negative electrode voltage was -5V, the rotation speed of the rotating collection device was 300r / min, the moving speed of the conductive yarn was 0.1mm / s, and the injection flow rate was 0.03mL / h), and the copper wire was rotationally coated by a conventional nozzle-type electrospinning device to form nanofiber coated yarn;

[0111] (2) Preparation of hydrophobic polyester roving:

[0112] The polyester staple fibers are opened, carded and drawn in sequence to obtain polyester slivers; when carding, the rotation speeds of the cylinder and the doffer are both low; when drawing, the drafting multiple of the drawing frame is 6 times;

[0113] The polyester sliver is immersed in the silicone finishing agent for 20 minutes, and then dried at 120°C for 20 minutes to obtain a hydrophobic polyester sliver; the hydrophobic polyester sliver is then spun into roving by a roving machine, and then wound to obtain a hydrophobic polyester roving; when the roving is spun, the drafting multiple is 7 times, and the roving dry weight is 5g / 10m;

[0114] (3) Preparation of friction nano-electricity generation composite yarn: The nanofiber-coated yarn and the hydrophobic polyester roving are respectively wound on two yarn tubes of a ring spinning machine, with the nanofiber-coated yarn as the core yarn and the hydrophobic polyester roving as the outer yarn. The hydrophobic polyester micron fiber formed by the hydrophobic polyester roving is twisted and coated on the outer surface of the nanofiber-coated yarn through the ring spinning machine to obtain a three-layer friction nano-electricity generation composite yarn.

[0115] Example 4

[0116] (1) Preparation of nanofiber coated yarn:

[0117] Add nano zinc oxide to HFIP, and ultrasonically treat it for 60 minutes at 25°C to obtain a nano zinc oxide solution with a mass fraction of 3%; then add PA11 particles to the nano zinc oxide solution, and stir and dissolve it at 65°C for 2 hours to obtain a PA11 / nano zinc oxide solution with a mass fraction of 15% of PA11;

[0118] Then, PA11 / nano zinc oxide solution was used as the electrospinning solution for the positive and negative electrodes, and copper wire was used as the core yarn. The double-electrode electrospinning technology was adopted to adjust the electrospinning parameters (positive electrode voltage was 5V, negative electrode voltage was -5V, the rotation speed of the rotating collection device was 300r / min, the moving speed of the conductive yarn was 0.1mm / s, and the injection flow rate was 0.03mL / h), and the copper wire was rotationally coated by a conventional nozzle-type electrospinning device to form nanofiber coated yarn;

[0119] (2) Preparation of hydrophobic polyester roving:

[0120] The polyester staple fibers are opened, carded and drawn in sequence to obtain polyester slivers; when carding, the rotation speeds of the cylinder and the doffer are both low; when drawing, the drafting multiple of the drawing frame is 6 times;

[0121] The polyester sliver is immersed in the silicone finishing agent for 20 minutes, and then dried at 120°C for 20 minutes to obtain a hydrophobic polyester sliver; the hydrophobic polyester sliver is then spun into roving by a roving machine, and then wound to obtain a hydrophobic polyester roving; when the roving is spun, the drafting multiple is 7 times, and the roving dry weight is 5g / 10m;

[0122] (3) Preparation of friction nano-electricity generation composite yarn: The nanofiber-coated yarn and the hydrophobic polyester roving are respectively wound on two yarn tubes of a ring spinning machine, with the nanofiber-coated yarn as the core yarn and the hydrophobic polyester roving as the outer yarn. The hydrophobic polyester micron fiber formed by the hydrophobic polyester roving is twisted and coated on the outer surface of the nanofiber-coated yarn through the ring spinning machine to obtain a three-layer friction nano-electricity generation composite yarn.

[0123] Table 1

[0124] Example Voltage (V) Current (μA) Charge (nC) Example 1 17.00 0.19 6.10 Example 2 19.74 0.26 7.11 Example 3 19.44 0.27 7.11 Example 4 15.33 0.17 6.22

[0125] It can be seen from Table 1 that the composite yarns of the present invention all have good electrical performance output, and the electrical performance output is best when the mass fraction of PA11 is 9%.

[0126] Any matters not described in the present invention are applicable to the prior art.

Claims

1. A method for preparing a friction nano-electricity composite yarn, characterized in that: The method comprises the following steps: (1) preparing nanofiber coated yarn: using PA11 / nano zinc oxide solution as the electrospinning solution for the positive and negative electrodes and the conductive yarn as the core yarn, and adopting a double-electrode electrospinning method to spin-coat the nanofiber yarn formed by the PA11 / nano zinc oxide solution on the outer surface of the conductive yarn to form the nanofiber coated yarn; (2) preparing hydrophobic polyester roving: using polyester staple fibers as raw materials, sequentially opening, carding and drawing the polyester staple fibers to obtain polyester slivers; then subjecting the polyester slivers to hydrophobic finishing to obtain hydrophobic polyester slivers; then spinning the hydrophobic polyester slivers into roving to obtain hydrophobic polyester roving; (3) Preparation of friction nano-electricity generation composite yarn: using nanofiber-coated yarn as core yarn and hydrophobic polyester roving as outer yarn, and using ring spinning process to twist and wrap hydrophobic polyester micron fibers formed by hydrophobic polyester roving on the outer surface of nanofiber-coated yarn to obtain a three-layer friction nano-electricity generation composite yarn; the inner layer is conductive yarn, which serves as the electrode layer; the middle layer is nanofiber yarn, which serves as the charge storage layer; and the outer layer is hydrophobic polyester micron fiber, which serves as the charge generation layer.

2. The method for preparing the friction nano-electricity composite yarn according to claim 1, characterized in that: In step (1), the conductive yarn has a conductivity of not less than 2.3×10 7 Lightweight and soft conductive yarn of S / m.

3. The method for preparing the friction nano-electricity composite yarn according to claim 1, characterized in that: In step (1), the electrospinning solution is prepared by ultrasonically dissolving nano zinc oxide in HFIP; then adding PA11 particles and stirring to dissolve them to obtain a homogeneous PA11 / nano zinc oxide solution; The time of ultrasonic dissolution is 50-70 minutes, the temperature is 20-30°C, and the ultrasonic frequency is 40kHz; the time of stirring dissolution is 1.8-2.5 hours, the temperature is 60-65°C, and the rotation speed is 55-60r / min; In the electrospinning solution, the concentration of PA11 is 6-15wt%, and the concentration of nano zinc oxide is 1-7wt%.

4. The method for preparing the friction nano-electricity composite yarn according to claim 1, characterized in that: In step (1), the process parameters of dual-electrode electrospinning are: the positive electrode voltage is 5 to 6 V, the negative electrode voltage is -5 to -6 V, the rotation speed of the rotating collection device is 200 to 600 r / min; the moving speed of the conductive yarn is 0.05 to 0.3 mm / s; the injection flow rate of the electrospinning solution of the positive and negative electrodes is 0.01 to 0.05 mL / h and the injection flow rate is the same.

5. The method for preparing the friction nano-electricity composite yarn according to claim 1, characterized in that: In step (2), when the sliver is carded, the rotation speeds of the cylinder and the doffer are both low; when drawing, the drafting multiple of the drawing frame is 5 to 7; The polyester sliver is immersed in a hydrophobic finishing agent at room temperature for 10 to 25 minutes, and then dried at a temperature of 100 to 150° C. for 15 to 30 minutes to obtain a hydrophobic polyester sliver; the hydrophobic finishing agent is a silicone finishing agent; When spinning roving, the drafting multiple is 7 to 9, and the dry weight of the obtained hydrophobic polyester roving is 4 to 5 g / 10m.

6. The method for preparing the friction nano-electricity composite yarn according to claim 1, characterized in that: In step (3), the ring spinning process is: feeding the hydrophobic polyester roving from the rear jaw of the rear roller, passing through the rear roller, the middle roller and the front roller in sequence, and then outputting from the front jaw of the front roller to form hydrophobic polyester micron fiber; feeding the nanofiber coated yarn from the rear jaw of the front roller, and then outputting from the front jaw of the front roller; then the nanofiber coated yarn and the hydrophobic polyester micron fiber are assembled in the front area, the hydrophobic polyester micron fiber is twisted and coated on the outer surface of the nanofiber coated yarn, and then wound on the bobbin through a steel wire ring to form a three-layer structure of friction nano power generation composite yarn.

7. A friction nano-electricity composite yarn prepared by the preparation method according to any one of claims 1 to 6, characterized in that: The composite yarn has a three-layer structure from inside to outside; the inner layer is conductive yarn, which serves as an electrode layer; The middle layer is nanofiber yarn, which serves as a charge storage layer; the outer layer is hydrophobic polyester micron fiber, which serves as a charge generation layer.

8. The friction nanostructured composite yarn according to claim 7, characterized in that: The mass of the hydrophobic polyester micron fiber accounts for 8-15% of the total mass of the composite yarn; the mass ratio of the hydrophobic polyester micron fiber to the conductive yarn is 0.5-1:

1.

9. An application of the friction nano-electricity composite yarn according to claim 7 or 8, characterized in that: The composite yarn is used as a yarn material for two-dimensional woven and knitted fabrics.

10. The use of the friction nano power generation composite yarn according to claim 9, characterized in that: When the composite yarn is used as a raw material for a two-dimensional braided fabric, the specific two-dimensional braiding process is: winding the composite yarn on a spindle of a two-dimensional braiding machine, using a spandex fiber bundle as a core layer, and coating the composite yarn on the outside of the spandex fiber bundle through a two-dimensional braiding process to obtain a two-dimensional braided fabric; the rotation speed of the two-dimensional braiding machine is 10 to 15 r / min; When the composite yarn is used as a raw material for knitted fabric, the knitted fabric is produced by a conventional knitting process.