A bioactive glass composite hydrogel scaffold material and its preparation method and application

The composite hydrogel scaffold is formed through the dynamic bond reaction of bioactive glass with dextran and gelatin, which solves the problem of easy collapse of hydrogel scaffolds in the human body environment in the existing technology, and achieves self-healing and cell compatibility. It provides an effective bone repair solution with good biocompatibility and low cost.

CN116099041BActive Publication Date: 2024-10-15SOUTH CHINA UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310055932.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-17
Publication Date
2024-10-15
Estimated Expiration
2043-01-17

AI Technical Summary

Technical Problem

The existing technology is difficult to provide a hydrogel scaffold with environmental adaptability, high mechanical properties and biological activity in the human environment for the regeneration and repair of aging bone tissue, and simple powder materials are easy to collapse.

Method used

Bioactive glass is used to react with materials such as dextran and gelatin to form a composite hydrogel scaffold through dynamic bond reactions. The dynamic bonds between amino groups and aldehyde groups are used to achieve gel formation. A porous structure scaffold is prepared using freeze-drying technology to ensure self-sufficiency. Healing and cytocompatibility.

Benefits of technology

The hydrogel scaffold achieves self-healing, stable structure, and promotes cell osteogenesis, avoiding the loss of hydrogel function and providing a simple and easy-to-operate bone repair solution with good biocompatibility and low cost. cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116099041B_ABST
    Figure CN116099041B_ABST
Patent Text Reader

Abstract

The present invention discloses a bioactive glass composite hydrogel scaffold material and a preparation method and application thereof; the present invention comprises dissolving a sodium periodate-modified polymer material and a strontium-doped bioactive glass powder material in a PBS solution; heating and stirring to obtain a suspension solution; adding gelatin to the suspension solution to obtain a mixed solution, stirring to form a gel, and obtaining the bioactive glass composite hydrogel scaffold material. The bioactive glass composite hydrogel scaffold of the present invention enhances the osteogenesis ability by changing the aging level of oxidatively induced bone marrow mesenchymal stem cells, and because the addition of strontium-doped bioactive glass improves the mechanical strength of the hydrogel, reduces the degradation rate and swelling rate of the hydrogel, and better meets the requirements of bone defects. The bioactive glass composite hydrogel scaffold of the present invention has no obvious toxicity, has porosity, self-healing properties and cell compatibility, and exhibits a good tissue regeneration and repair effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical fields of biomedical materials, tissue engineering and regenerative medicine, and specifically relates to a bioactive glass composite hydrogel scaffold material and a preparation method and application thereof. Background Art

[0002] As we age, age-related changes are inevitable, so the oral problems of the elderly show different characteristics from those of young people in many aspects. Due to the influence of systemic and local factors, degenerative changes will occur in the jaws, and then the teeth will become loose and fall off, and the chewing function will be lost. This change is inseparable from the alveolar bone. For the elderly, the functions of various organs in the body gradually degenerate. For example, alveolar bone defects are a manifestation of human functional degeneration and are considered an important factor affecting the health of the elderly. There is an old Chinese saying that the tongue is still there even if the teeth are gone. This can be explained by the fact that soft and flexible things last longer than hard things. It also accurately reflects the general situation of alveolar bone absorption in the elderly. There are usually two different ways to solve this problem, one is direct repair and the other is to wear dentures. When the denture is suspended on the elderly's own teeth, the retention and stability of the denture are significantly improved. But whether it is direct repair or the use of dentures, one thing is the same: it is necessary to improve the condition of the alveolar bone. And improving the condition of the alveolar bone is inseparable from improving the osteogenic ability of aging bone marrow mesenchymal stem cells.

[0003] Polymer hydrogel is a soft material with a three-dimensional network structure that can absorb and retain a large amount of water. Polymer hydrogel has good biocompatibility and mechanical properties and has important application value in the fields of biomedicine and bioengineering. Hydrogel is a material that can better fit irregular defect sites, and the Schiff base reaction is a dynamic reaction. Non-dynamic chemical bond assembly scaffolds are very stable, have low environmental adaptability, and are easily broken; physical bond or dynamic chemical bond assembly scaffold microgels have weak interaction forces and poor mechanical properties, but have strong environmental adaptability ([1] Li Jin, Zhao Zinian, Li Zhengzheng, Xue Song, Zheng Zelin. Synthesis mechanism and biomedical application of self-healing hydrogels [J]. Materials Guide, 2019, 33(19): 3328-3335+3346.).

[0004] Bioactive glass itself has a good ability to promote osteogenesis, so it is necessary to choose bioactive glass as the main starting point for designing materials. Bioactive glass itself has good biocompatibility and is degradable. The structure of bioactive glass is different from the traditional glass with -Si-O-Si-bridge oxygen bond as the network structure. Instead, it is formed by introducing a covalent bond network after the alkali metal and alkaline earth metal are interrupted, which is a non-bridge oxygen bond. It is an inorganic non-metallic material with good bioactivity and biocompatibility. Through the preparation method of the sol-gel method, its composition can be regulated at the molecular level. Among the many properties of bioactive glass, the interaction between the bone defect and the bioactive glass is inseparable from its ion release mechanism. This process includes five steps, namely, ion dissolution and exchange with body fluids, network structure destruction, Si-O bond interruption, formation of a colloidal layer on the surface of bioglass, formation of an amorphous Ca-P layer, and formation of a carbonated hydroxyapatite crystal layer. This series of inorganic chemical reactions at the interface of bioactive glass and body fluids is the premise for inducing osteoblast proliferation, activating osteoblast-related genes, promoting osteoblast differentiation and calcification, and ultimately achieving good bone repair effects. However, pure powder materials are prone to disintegration in the human body environment and "travel around the world" with body fluids.

[0005] Therefore, it is of great significance to develop a hydrogel scaffold with strong environmental adaptability, high mechanical properties and biological activity. Summary of the invention

[0006] The purpose of the present invention is to provide a bioactive glass composite hydrogel scaffold material for regeneration and repair of aged bone tissue, and a preparation method and application thereof. The scaffold material utilizes dynamic bonds generated between amino groups and aldehyde groups to achieve gelation, and has porosity, self-healing properties and cell compatibility.

[0007] The main application subject of the hydrogel of the present invention is aging individuals, which require a certain mechanical strength but cannot cause secondary damage to the original tissue, so the hydrogel formed by the dynamic bond reaction is selected. From the perspective of actual production, the bone repair body components are required to be simple and easy to obtain, and excessive use of cross-linking agents is avoided. The use of a simple and convenient self-healing reaction is for this purpose. This is to expand the application of bioactive glass, and further strengthen the understanding of bioactive glass, constantly expand new horizons, and make new generalizations.

[0008] The hydrogel used as a carrier of the present invention has one of its assembly raw materials as a polymer material such as dextran, which is mainly extracted from the cell wall of baker's yeast, widely used in the food industry, widely available, has no obvious toxic side effects on the human body, has a large number of hydroxyl groups, and is easily oxidized to produce aldehyde groups; another component material is gelatin, which has good biocompatibility and is also low-priced and easy to obtain. The preparation method of this hydrogel material is simple, the reaction conditions are mild, and it meets practical needs.

[0009] The bioactive glass of the invention is prepared by calcining ethyl orthosilicate, triethyl phosphate, calcium nitrate and strontium nitrate as main components.

[0010] The purpose of the present invention is achieved by one of the following technical solutions.

[0011] A method for preparing a bioactive glass composite hydrogel scaffold material comprises the following steps:

[0012] (1) dissolving a sodium periodate-modified polymer material and a strontium-doped bioactive glass powder material in a PBS solution; heating and stirring to obtain a suspension solution;

[0013] (2) adding gelatin to the suspension solution obtained in step (1) to obtain a mixed solution, stirring to form a gel, and obtaining the bioactive glass composite hydrogel scaffold material.

[0014] Preferably, the polymer material in step (1) is one of chondroitin sulfate, dextran, carboxymethyl chitosan, collagen and sodium alginate.

[0015] Preferably, in step (2), the concentrations of the sodium periodate-modified polymer material, gelatin and strontium-doped bioactive glass powder material in the mixed solution are 5-30wt%, 5-40wt% and 1-5wt%, respectively.

[0016] Preferably, the preparation of the sodium periodate-modified polymer material in step (1) comprises the following steps: adding the polymer material to an aqueous solution of 2-(N-morpholine)ethanesulfonic acid, adding sodium periodate to react for 3-5 hours after the polymer material is dissolved, and then adding ethylene glycol and stirring to terminate the reaction, dialyzing the reaction solution and freeze-drying it to obtain a sodium periodate-modified polymer material.

[0017] Further preferably, the concentration of the 2-(N-morpholine)ethanesulfonic acid aqueous solution is 1-3wt%; the pH of the 2-(N-morpholine)ethanesulfonic acid aqueous solution is 5-6;

[0018] Further preferably, the amount of the polymer material is 20-30 w / v% of the 2-(N-morpholino)ethanesulfonic acid aqueous solution;

[0019] Further preferably, the amount of sodium periodate used is 1-10 w / v% of the 2-(N-morpholino)ethanesulfonic acid aqueous solution;

[0020] Further preferably, the reaction of adding sodium periodate is carried out at 30-50° C. in the dark with stirring;

[0021] More preferably, the stirring time for adding ethylene glycol is 20-40 minutes.

[0022] Preferably, the preparation of the strontium-doped bioactive glass powder material in step (1) comprises the following steps:

[0023] A. Add anhydrous ethanol and dodecylamine into water and stir evenly to obtain a clear mixture;

[0024] B. Adding ethyl orthosilicate to the clarified mixture in step A, then dropping triethyl phosphate, performing a first stirring reaction at 30-50° C. to obtain a reaction solution, adding calcium nitrate tetrahydrate and strontium nitrate dihydrate to the reaction solution, continuing to perform a second stirring reaction at 30-50° C., and aging at room temperature to obtain an aged reaction solution;

[0025] C. Centrifuge the aged reaction solution in step B, take the precipitate, wash, dry, and heat-treat it to obtain the strontium-doped bioactive glass powder material.

[0026] Further preferably, the volume ratio of anhydrous ethanol and water in step A is (3-5):1; the mass volume ratio of dodecylamine and water in step A is 1:(5-10) g / mL;

[0027] Further preferably, the volume ratio of the tetraethyl orthosilicate in step B to the anhydrous ethanol in step A is 1:(3-6); the volume ratio of triethyl phosphate to tetraethyl orthosilicate in step B is (15-10):1; the time of the first reaction in step B is 20-60 min;

[0028] Further preferably, the mass ratio of calcium nitrate tetrahydrate to strontium nitrate dihydrate in step B is (1-2):1; the mass ratio of calcium nitrate tetrahydrate to dodecylamine in step B is 1:(2-4); the time of the second reaction in step B is 2.5-4.5h; the time of the aging treatment in step B is 18-24h;

[0029] Further preferably, the heat treatment temperature in step C is 600-650° C., and the heat treatment time is 2-4 hours.

[0030] The above preparation method obtains a bioactive glass composite hydrogel scaffold material.

[0031] The use of the above-mentioned bioactive glass composite hydrogel scaffold material in the preparation of a hydrogel scaffold for regeneration and repair of aged bone tissue.

[0032] The composite hydrogel scaffold based on chemical dynamic bonds developed by the present invention can effectively solve the problem of mesenchymal stem cell osteogenesis after oxidative aging, and can self-heal to form a stable scaffold. The composite hydrogel scaffold has the following advantages: (1) self-healing, maintaining the integrity of the hydrogel structure and avoiding loss of hydrogel function; (2) the scaffold has moderate mechanical properties and can maintain a certain structural stability at the defect site; (3) changing the level of oxidative induced cell senescence and promoting the level of cell osteogenesis after induction; (4) the preparation method is simple and easy to operate. In summary, this composite self-healing hydrogel scaffold provides a new solution for tissue regeneration and repair.

[0033] Compared with the prior art, the present invention has the following advantages:

[0034] (1) The preparation method provided by the present invention selects three materials, strontium-doped bioactive glass, gelatin and oxidized dextran, for compounding. The obtained composite hydrogel has good biocompatibility and performance in promoting the repair of aged bone tissue. The synthetic materials are widely available and low in cost. The synthetic method is simple and convenient. The hydrogel scaffold is prepared by freeze drying, which is simple and has stable quality.

[0035] (2) The preparation method provided by the present invention is to select a high molecular organic substance with good biocompatibility - gelatin, blend it with oxidized dextran and use freeze-drying technology to prepare a multi-level porous structure, which is conducive to cell growth and adhesion;

[0036] (3) The present invention assembles the hydrogel scaffold through the dynamic bond generated between the amino group and the aldehyde group, and the reaction conditions are relatively mild, which is suitable for tissue engineering. The dynamic assembly of the hydrogel by the amino group and the aldehyde group makes the scaffold have self-healing properties, and the self-healing properties of the hydrogel can better maintain the three-dimensional structure, which is also conducive to cell growth. In addition, the aldehyde group can further form hydrogen bonds and Schiff bases with the protein amino groups on the surrounding tissues, which can adhere the hydrogel scaffold to the surrounding tissues, thereby effectively avoiding the displacement of the hydrogel scaffold. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 Schematic diagram of the mechanism of assembly of the bioactive glass composite hydrogel of the present invention;

[0038] Figure 2a and Figure 2b This is a diagram showing the cell compatibility evaluation of the composite hydrogel scaffold of Example 2;

[0039] Figure 3 This is a scanning electron microscopy image of the cross section of the composite gel assembly scaffold obtained in Example 3 after freeze-drying;

[0040] Figure 4 The compression modulus graph and the compression stress-strain curve graph of the hydrogel scaffold in Example 4;

[0041] Figure 5 This is a degradation curve diagram of the hydrogel scaffold in Example 5;

[0042] Figure 6 is a swelling curve diagram of the hydrogel scaffold of Example 6;

[0043] Figure 7 This is the curve of the change in the aging degree of the aged bone marrow mesenchymal stem cells by the hydrogel scaffold in Example 7;

[0044] Figure 8 This is the curve of the effect of the hydrogel scaffold in Example 8 on the osteogenic ability of aged bone marrow mesenchymal stem cells. DETAILED DESCRIPTION

[0045] The present invention is further described in detail below in conjunction with embodiments and drawings, but the embodiments of the present invention are not limited thereto.

[0046] The preparation of the sodium periodate-modified dextran used below comprises the following steps:

[0047] (1) 22 g of 2-(N-morpholino)ethanesulfonic acid solid was dissolved in 1 L of deionized water and the pH value was adjusted to 5.5 with 1 M hydrochloric acid solution to obtain MES buffer;

[0048] (2) Weigh 20 g of dextran and dissolve it in 100 ml of MES buffer at 50°C with magnetic stirring. After dissolution, add 6 g of sodium periodate in batches. After reacting at 40°C in the dark for 4 hours, add 15 ml of ethylene glycol and stir for 30 minutes to terminate the reaction. Use a dialysis bag with a molecular weight of 8000-14000 to dialyze the solution with deionized water for 3 days and freeze-dry to obtain sodium periodate-modified dextran.

[0049] The preparation of the bioactive glass used below includes the following steps:

[0050] A. Add anhydrous ethanol and dodecylamine into water (the volume ratio of anhydrous ethanol to water is 4:1; the mass volume ratio of dodecylamine to water is 1:5 g / mL), stir evenly to obtain a clear mixture;

[0051] B. Adding tetraethyl orthosilicate to the clarified mixture described in step A (the volume ratio of the tetraethyl orthosilicate to the anhydrous ethanol described in step A is 1:5), then dripping triethyl phosphate (the volume ratio of the triethyl phosphate to the tetraethyl orthosilicate is 14.035:1), carrying out a first stirring reaction at 40° C. for 30 min to obtain a reaction solution, adding calcium nitrate tetrahydrate and strontium nitrate dihydrate to the reaction solution (the mass ratio of the calcium nitrate tetrahydrate to the strontium nitrate dihydrate is 1.148:1; the mass ratio of the calcium nitrate tetrahydrate to dodecylamine is 1:2.424), continuing to stir for a second time at 40° C. for 3 h; aging at room temperature for 24 h to obtain an aged reaction solution;

[0052] C. Centrifuge the aged reaction solution in step B, take the precipitate, wash, dry, heat-treat at 650° C. for 3 h, and obtain the strontium-doped bioactive glass powder material.

[0053] Example 1

[0054] (1) 200 mg of sodium periodate-modified dextran was added to 2 ml of PBS solution, heated to 40°C and stirred to dissolve, and then 80 mg of strontium-doped bioactive glass was added and stirred to obtain a suspension;

[0055] (2) Add 200 mg of gelatin to the suspension in step (1) while it is still hot, and stir until the mixture undergoes obvious gelation, thereby obtaining a hydrogel scaffold (the concentration of strontium-doped bioactive glass is 4% w / v, g / ml).

[0056] The assembly method of the hydrogel scaffold of this embodiment is as follows Figure 1 As shown, assembly is achieved through dynamic binding bonds between amino and aldehyde groups.

[0057] The preparation method of the "hydrogel without bioactive glass doping" described in the following examples is the same as the above-mentioned hydrogel scaffold doped with strontium bioactive glass, except that no strontium-doped bioactive glass is added in step (1);

[0058] The preparation method of the "Strontium-free bioactive glass hydrogel" described in the following examples is the same as the above-mentioned Strontium-doped bioactive glass hydrogel scaffold, except that step (1) adds Strontium-free bioactive glass.

[0059] Example 2

[0060] The cell compatibility of the hydrogel scaffold of Example 1 is as follows Figure 2a , Figure 2bAs shown, cells were cultured in a high-glucose medium containing 10 v / v% fetal bovine serum. By comparing the cell activity at 1 day, 3 days, and 7 days, and through the CCK-8 cytotoxicity assay and cell live-dead staining results, it was found that both strontium-doped and non-strontium-doped bioactive glass composite hydrogels had good cell compatibility, and had no obvious toxicity compared to hydrogels without bioactive glass.

[0061] Example 3

[0062] The freeze-dried cross-sectional view of the composite scaffold of this embodiment is as follows Figure 3 As shown, after preparing the composite hydrogel of strontium-doped bioactive glass in Example 1, it was frozen at minus 20 degrees Celsius for 48 hours, and sent to a freeze dryer for freeze drying for 24 hours to obtain a scaffold. The scaffold was soaked in liquid nitrogen at minus 80 degrees for 5 minutes, and cut with a scalpel to obtain a cross section. Finally, it was sprayed with gold and observed with a high-power scanning electron microscope. It can be seen that after freeze drying, the morphology of the hydrogel is porous, and the bioglass particles added in the last two groups can be clearly seen.

[0063] Example 4

[0064] In this example, under the test condition of controlling the strain rate, the compressive stress-strain curves of the hydrogel scaffolds prepared from the bioactive glass without bioactive glass, the bioactive glass without strontium and the bioactive glass with strontium in Example 1 were obtained by testing, and the compression modulus of the assembly was calculated by selecting the straight line segment of the curve, as shown in FIG. Figure 4 In the absence of strontium-doped bioglass, the modulus of the microgel assembly scaffold was limited and at a relatively low level; after adding bioactive glass, the modulus of both groups increased.

[0065] Example 5

[0066] In this example, degradation curves of the hydrogel scaffolds prepared from the bioactive glass without strontium, the bioactive glass without strontium and the bioactive glass with strontium were obtained. Different hydrogels were immersed in PBS and placed in a shaker at the same time, and the remaining mass was weighed, such as Figure 5 In the absence of bioactive glass, the degradation rate of the microgel assembly scaffold is fast; after adding bioactive glass, the degradation rate decreases.

[0067] Example 6

[0068] In this example, the swelling curves of the hydrogel scaffolds prepared from the bioactive glass without bioactive glass, the bioactive glass without strontium doping and the bioactive glass doped with strontium in Example 1 were obtained by testing. The three different hydrogels were immersed in PBS and the weight after water absorption was weighed until the swelling equilibrium was reached. Figure 6 In the absence of bioactive glass, the swelling rate of the microgel assembly scaffold is relatively large; after adding bioactive glass, the swelling rate decreases.

[0069] Example 7

[0070] The changes in the cell senescence level in this example are after H2O2 oxidation induction, and the expression levels of senescence markers after 5 days of exposure to the hydrogel extract of Example 1 are tested. Figure 7 As shown, by comparing the expression levels of P21 and P53, it can be found that the composite hydrogel has the ability to reduce the level of aging, and the strontium-doped experimental group has a better effect.

[0071] Example 8

[0072] The changes in the cell senescence level in this example are the expression levels of osteogenic genes tested after 14 days of exposure to the hydrogel extract of Example 1 after H2O2 oxidation induction. Figure 8 As shown, by comparing the expression levels of related osteogenic genes, it can be found that the composite hydrogel has the ability to promote H2O2 oxidation-induced osteogenesis of aged bone marrow mesenchymal stem cells, and the strontium-doped experimental group has a better effect.

[0073] The embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the implementation methods of the present invention. For professionals in the relevant field, other different forms of changes or modifications can be made based on the above embodiments, and it is not necessary and impossible to list all implementation methods here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.

Claims

1. A method for preparing a bioactive glass composite hydrogel scaffold material, characterized in that: The following steps are involved: (1) Dissolving the sodium periodate-modified polymer material and the strontium-doped bioactive glass powder material in a PBS solution; The suspension solution is obtained by heating and stirring uniformly; the strontium-doped bioactive glass is obtained by calcining ethyl orthosilicate, triethyl phosphate, calcium nitrate and strontium nitrate as main components; the polymer material is dextran; (2) adding gelatin to the suspension solution obtained in step (1) to obtain a mixed solution, stirring to form a gel, and obtaining the bioactive glass composite hydrogel scaffold material; the concentrations of the sodium periodate-modified polymer material, gelatin, and strontium-doped bioactive glass powder material in the mixed solution are 5-30wt%, 5-40wt%, and 1-5wt%, respectively; The preparation of the sodium periodate-modified polymer material in step (1) comprises the following steps: adding the polymer material to an aqueous solution of 2-(N-morpholine)ethanesulfonic acid, adding sodium periodate to react for 3-5 hours after the polymer material is dissolved, and then adding ethylene glycol to stir and terminate the reaction, dialyzing the reaction solution and then freeze-drying to obtain a sodium periodate-modified polymer material; The preparation of the strontium-doped bioactive glass powder material in step (1) comprises the following steps: A. Add anhydrous ethanol and dodecylamine into water and stir evenly to obtain a clear mixture; B. Adding ethyl orthosilicate to the clarified mixture in step A, then dropping triethyl phosphate, performing a first stirring reaction at 30-50° C. to obtain a reaction solution, adding calcium nitrate tetrahydrate and strontium nitrate dihydrate to the reaction solution, continuing to perform a second stirring reaction at 30-50° C., and aging at room temperature to obtain an aged reaction solution; C. Centrifuge the aged reaction solution in step B, take the precipitate, wash, dry, and heat-treat it to obtain the strontium-doped bioactive glass powder material.

2. The preparation method according to claim 1, characterized in that: The concentration of the 2-(N-morpholine)ethanesulfonic acid aqueous solution is 1-3wt%; the pH of the 2-(N-morpholine)ethanesulfonic acid aqueous solution is 5-6; The amount of the polymer material is 20-30w / v of the 2-(N-morpholine)ethanesulfonic acid aqueous solution; The amount of sodium periodate used is 1-10w / v of the 2-(N-morpholino)ethanesulfonic acid aqueous solution; The sodium periodate reaction is carried out at 30-50° C. in the dark with stirring; The stirring time for adding ethylene glycol is 20-40 minutes.

3. The preparation method according to claim 1, characterized in that: The volume ratio of anhydrous ethanol and water in step A is (3-5): 1; the mass volume ratio of dodecylamine and water in step A is 1: (5-10) g / mL.

4. The preparation method according to claim 1, characterized in that: The volume ratio of the tetraethyl orthosilicate in step B to the anhydrous ethanol in step A is 1: (3-6); the volume ratio of triethyl phosphate to tetraethyl orthosilicate in step B is (15-10): 1; the time of the first stirring reaction in step B is 20-60min; the mass ratio of calcium nitrate tetrahydrate to strontium nitrate dihydrate in step B is (1-2): 1; the mass ratio of calcium nitrate tetrahydrate to dodecylamine in step B is 1: (2-4); the time of the second stirring reaction in step B is 2.5-4.5h; the time of the aging treatment in step B is 18-24h; the temperature of the heat treatment in step C is 600-650°C, and the time of the heat treatment is 2-4h.

5. A bioactive glass composite hydrogel scaffold material prepared by the preparation method according to any one of claims 1 to 4.

6. Use of the bioactive glass composite hydrogel scaffold material according to claim 5 in the preparation of a hydrogel scaffold for regeneration and repair of aged bone tissue.