A method for preparing catalytic cracking catalyst by ammonium-free method

Catalytic cracking catalysts were prepared by ammonium-free method, and the modification of rare earth-aged silicon magnesium materials and ammonia water and boric acid were used, combined with the design of downlink bed homocrystal replacement reactors, the problems of underdeveloped catalyst pore structure and ammonia nitrogen emission were solved, and the problems of underdeveloped catalyst pore structure and ammonia nitrogen emission were achieved. High performance and environmentally friendly catalyst preparation.

CN116212849BActive Publication Date: 2024-11-05PETROCHINA CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111468024.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-03
Publication Date
2024-11-05
Estimated Expiration
2041-12-03

AI Technical Summary

Technical Problem

In the existing catalytic cracking catalyst preparation methods, environmental pollution caused by underdeveloped catalyst pore structure and ammonia nitrogen emissions.

Method used

The method of preparing catalytic cracking catalysts by using ammonium-free method is used to mix the magnesium source solution with the silicon source solution and add rare earth compounds to form silicon magnesium material, and mix it with kaolin, dispersant and deionized water to beat and spray it into microspheres. After calcination and crystallization, the homocrystalline substitution reaction is carried out in a downlink bed homocrystalline substitution reactor in a countercurrent contact with silicon tetrachloride, combining the exchange modification of ammonia water and boric acid.

Benefits of technology

The pore volume and molecular sieve content of the catalyst are significantly improved, the pore structure distribution is improved, the sodium oxide content is reduced, ammonia nitrogen emissions are avoided, and the heavy oil conversion and heavy metal resistance of the catalyst are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116212849B_ABST
    Figure CN116212849B_ABST
Patent Text Reader

Abstract

The present invention relates to a method for preparing a catalytic cracking catalyst by an ammonium-free method, comprising the following steps: (1) mixing a magnesium source solution with a silicon source solution to obtain a silicon-magnesium material, then adding a rare earth compound, aging, and obtaining a silicon-magnesium material containing a rare earth; (2) mixing the silicon-magnesium material containing a rare earth with kaolin, a dispersant and / or a reinforcing agent, and deionized water, beating, spraying into microspheres, and then roasting, and then mixing with sodium silicate, a directing agent, an alkaline solution, and water, crystallizing, and obtaining a crystallized product; (3) exchanging and modifying the crystallized product with ammonia water and boric acid, and then roasting to obtain a primary roasted material; (4) contacting the primary roasted material with silicon tetrachloride in a downward bed isomorphous substitution reactor in countercurrent to perform an isomorphous substitution reaction to obtain a catalyst. The present invention utilizes the rare earth aged silicon-magnesium material and the modification of ammonia water and boric acid, and combines the isomorphous substitution process to prepare an in-situ crystallization catalyst with excellent performance and simple process flow.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of catalysts, and in particular relates to a method for producing an ammonium-free catalytic cracking catalyst. Background Art

[0002] Low cost and high performance have always been one of the important directions for the preparation and development of catalytic cracking catalysts. For heavy oil catalytic cracking catalysts, with the increasingly heavy and inferior raw oil of FCC units and the stringent environmental protection regulations, catalytic cracking catalysts are required to have more excellent reaction performance and efficient preparation process.

[0003] In order to make the catalytic cracking catalyst have unobstructed pores, good acidity, and very low sodium oxide, ammonium salts, rare earths and other substances are used for post-modification treatment and exchange during the post-modification process. While obtaining good performance, it also brings serious ammonia nitrogen pollution problems. This seriously restricts the sustainable development of catalysts. Therefore, the development of low-cost, high-performance catalyst post-modification processes is the current focus of improving quality and efficiency.

[0004] For a long time, people have done a lot of work on converting and removing nitrogen from sewage, but they all remove and convert ammonia nitrogen in water after sewage is generated. These methods often have disadvantages such as large investment, complex operation, and high operating costs. Some processes even bring secondary pollution while removing ammonia nitrogen, which significantly increases the production cost of catalysts. At the same time, ammonia nitrogen exchanged or adsorbed on molecular sieves and catalysts will enter the atmosphere during subsequent treatment, thereby polluting the air. The best idea should be to reduce the amount of ammonium salt used in the catalyst preparation process, alleviate ammonia nitrogen pollution from the source, and develop a new exchange technology and catalyst preparation process to improve the utilization rate of modified ions to ensure the sustainable development of catalytic cracking catalysts.

[0005] CN202010059891.3 discloses a method for preparing mesoporous molecular sieves without ammonia, in which the molecular sieve raw material is contacted with a dealuminizing pore-forming agent in water for chemical dealuminizing pore-forming treatment without ammonium exchange to obtain a secondary mesoporous molecular sieve product. Although this method can prepare a certain amount of mesopores, it is relatively difficult to implement in industry; CN201711117556.9 introduces in detail a method for preparing a pollution-free and highly stable catalytic cracking catalyst, which specifically comprises contacting a NaY molecular sieve raw powder with a chlorine-containing gas for a gas-phase ion exchange reaction, completing the sodium reduction and ultra-stabilization of the NaY molecular sieve raw powder in one step to obtain a low-sodium, high-silicon-aluminum ratio molecular sieve. The method also compounds different types of clay ores and treats them with high-concentration acid to obtain an acid-activated composite clay, and then mixes the low-sodium, high-silicon-aluminum ratio molecular sieve, the acid-activated composite clay, a binder, rare earths, and decationized water for pulping and spray granulation, and then calcines and solidifies them without washing or drying to obtain a finished catalytic cracking catalyst. The catalytic cracking catalyst can significantly reduce the olefin content in gasoline and increase the light oil yield. The catalyst preparation process is short and there is no ammonia nitrogen emission. The patent has made improvements in two aspects: the implementation of the gas phase ultra-stable process of NaY molecular sieve and the modification of the matrix. CN201711074372.9 and CN201611117946.1 use the gas phase ultra-stable method to achieve ammonium-free exchange; CN201611116722.9 invented a device and preparation method for preparing a low-sodium, high-silicon-aluminum ratio Y-type molecular sieve. When the device is used to prepare molecular sieves, the operation process is short, there is no ammonia nitrogen pollution, the amount of sewage is small, the production cost is low, the reaction controllability is good, the reaction degree is high, the product sodium content is low, the silicon-aluminum ratio is high, the silicon-aluminum ratio can be adjusted, the product properties are uniform, and large-scale continuous automatic operation can be carried out.

[0006] Patent CN101850239A manufactures molecular sieve into molecular sieve paper, and then heat presses the molecular sieve paper into a corrugated shape and alternately stacks or rolls it with molecular sieve paper to form a honeycomb, which is placed in a closed container and reacts with a mixed gas of nitrogen and silicon tetrachloride gas. After the reaction is completed, the molecular sieve honeycomb is repeatedly cleaned and then acid-washed. The product obtained by this method has uniform properties and avoids the problem of molecular sieves sticking together into blocks, but to manufacture molecular sieve paper and honeycomb, if a powder product is to be obtained, the honeycomb needs to be broken, which increases the manufacturing cost and labor intensity. Patent CN1286721C discloses a gas phase aluminum extraction and silicon replenishment method for molecular sieves, and the gas phase dealuminization and silicon replenishment reaction is carried out in a stirred reactor. This method makes the contact reaction of silicon tetrachloride gas and molecular sieve solid particles more uniform, avoids the phenomenon of molecular sieve solid particles agglomerating into dense blocks, can reduce labor intensity, can reduce environmental pollution, and significantly reduce production costs. However, stirring will also bring about the undesirable effect that the molecular sieve is lifted up and carried away by the airflow, and there are also shortcomings such as long production cycle, the stirred tank reactor cannot be infinitely enlarged, and it is difficult to carry out large-scale continuous production. In patents CN102049315A, CN102049316A, CN102050459A, CN102050460A, CN102451655A, CN102451656A, CN102451657A, CN102451658A, CN102451729A, and CN102451730A, the gas phase dealumination and silicon replenishment reaction is carried out in a plug flow type heated horizontal tubular reactor with a length of 50 to 95 m and a diameter of 0.1 to 1.4 m, and also includes a gas mixer, a raw material mixing unit, a gas-solid separator, an absorption tower, and a beater. The molecular sieve and gaseous silicon tetrachloride flow with the inert carrier gas in a tubular reactor and contact and react for a contact time of 10s-100min. The molecular sieve after gas-phase dealuminization and siliconization is mixed with a binder, clay and water for slurrying and granulation to obtain a catalytic cracking catalyst. This method avoids the sticking of molecular sieve particles and can achieve continuous contact reaction between molecular sieve and silicon tetrachloride. In addition, by controlling different reaction temperatures, different reaction conditions and reaction degrees can be controlled, thereby obtaining molecular sieve products with different dealuminization depths; by controlling the flow rate of the carrier gas and the length of the tubular reactor, the contact time between the molecular sieve and silicon tetrachloride can be controlled. However, in order to achieve the purpose of gas carrying molecular sieve particles and avoiding molecular sieve particles blocking the pipeline, this method is bound to increase the carrier gas flow rate, resulting in the difficulty of improving the reaction depth and the low silicon-aluminum ratio of the product; in addition, in order to achieve the reaction depth, the amount of silicon tetrachloride introduced needs to be increased, which will inevitably increase the load of the tail gas treatment system; and by controlling the length of the tubular reactor to control the contact time, the device floor space is increased, which has many inconveniences in actual production.In patents CN103769193A, CN103785436A, CN103785437A, CN103785438A, CN103787352A and CN104549445A, the above-mentioned gas phase dealumination and siliconizing reactor is optimized.

[0007] CN103240113A discloses a method for preparing an in-situ crystallization catalyst that reduces ammonia nitrogen pollution, including adding polydimethyldiallyl ammonium chloride that can adjust the stacking mode between kaolin during spraying, and after obtaining the in-situ crystallization product, first using an acidic solution to clean the exchange environment of the exchange ions, and then through other steps of exchange and roasting to obtain a catalytic cracking catalyst. This method can reduce the use of ammonium salt by more than 15%, effectively alleviate the ammonia nitrogen pollution problem in the preparation process of the in-situ crystallization catalyst, and reduce production costs and improve the reaction performance of the catalyst. CN100404432C discloses a method for reducing ammonia nitrogen pollution in the zeolite modification process, including exchanging sodium in the zeolite with a potassium compound during the zeolite modification process, and then further exchanging and modifying the zeolite with an ammonium salt. This method does not increase the cost of zeolite modification, and the use of ammonium salt is reduced by about 50%.

[0008] CN103028431A discloses a clean production process of a molecular sieve catalytic cracking catalyst, which adopts a conventional in-situ crystallization method to prepare a modified molecular sieve or a molecular sieve catalytic cracking catalyst, and mixes the molecular sieve crystallization filtration mother liquor and / or the crystallization material washing water with the ammonia nitrogen wastewater generated in the molecular sieve exchange process as the spray washing liquid of the spray washing tower of the catalyst spray granulation tail gas, and adds the acidified aluminum salt or acid solution to the above-mentioned spray recovery liquid, gelling, filtering, filtrate discharge, and the filter residue as the synthetic molecular sieve raw material. This method reduces the cost while preparing qualified catalytic cracking catalyst products. After CN102553630A obtains NaY molecular sieve microspheres, it is contacted with silicon tetrachloride gas according to a weight ratio of 0.1-0.9:1, reacts at 150-500°C for 10 minutes to 6 hours, and obtains a catalytic cracking catalyst containing a high silicon-aluminum ratio small-grain Y-type molecular sieve by washing. The in-situ crystallization catalyst prepared by this method has a long reaction time, and its pore structure and performance are inferior to those of traditional hydrothermal ultra-stable catalysts.

[0009] Through the analysis of the above patents, although many catalysts have significantly reduced the amount of ammonium salt used in the preparation process and reduced the generation of ammonia nitrogen wastewater, ammonium ions are still introduced to a greater or lesser extent, and completely ammonia-free production cannot be achieved.

[0010] There are also some patents that achieve ammonium-free exchange through gas-phase ultrastabilization technology. However, since gas-phase ultrastabilization is an isomorphous substitution process, after gas-phase ultrastabilization, the catalyst or molecular sieve lacks a rich pore structure, resulting in poor catalyst selectivity and reaction performance. Summary of the invention

[0011] The purpose of the present invention is to provide a method for preparing a catalytic cracking catalyst without ammonium, so as to solve the environmental pollution problems caused by the underdeveloped pore structure of the catalyst and the emission of ammonia nitrogen during the exchange process in the existing preparation method.

[0012] To achieve the above object, the present invention provides a method for preparing a catalytic cracking catalyst by an ammonium-free process, comprising the following steps:

[0013] (1) mixing a magnesium source solution with a silicon source solution to obtain a silicon-magnesium material, and then adding a rare earth compound and aging to obtain a rare earth-containing silicon-magnesium material;

[0014] (2) mixing the rare earth-containing silicon-magnesium material with kaolin, a dispersant and / or a reinforcing agent and deionized water, beating the mixture, spraying the mixture into microspheres, calcining the mixture, and then mixing the mixture with sodium silicate, a directing agent, an alkaline solution and water, and crystallizing the mixture to obtain a crystallized product;

[0015] (3) exchanging and modifying the crystallized product with ammonia water and boric acid, and then calcining to obtain a primary calcined material;

[0016] (4) The primary calcined material is contacted with silicon tetrachloride in a downward bed type isomorphous substitution reactor in countercurrent to carry out isomorphous substitution reaction to obtain a catalyst.

[0017] The method for preparing catalytic cracking catalyst by the ammonium-free method of the present invention comprises the following steps: in step (1), a magnesium source solution and a silicon source solution are mixed, the pH value is adjusted to 8 to 12, and then a rare earth compound is added.

[0018] The method for preparing a catalytic cracking catalyst by an ammonium-free method of the present invention, wherein the aging condition in step (1) is aging treatment at 80-120° C. for 5-300 minutes, the aging temperature is preferably 80-100° C., and the aging treatment time is preferably 30-200 minutes.

[0019] The method for preparing catalytic cracking catalyst by the ammonium-free method of the present invention, wherein the rare earth compound in step (1) is calculated as rare earth oxide RE2O3, the mass ratio of RE2O3 to silicon-magnesium material is 1-10%, and the molar ratio of Si:Mg in the silicon-magnesium material is 0.1-15:1.

[0020] The method for preparing a catalytic cracking catalyst by an ammonium-free process of the present invention comprises the following steps: in step (1), the silicon source is one or more of water glass, silica sol and white carbon black; and the magnesium source is one or more of magnesium chloride, magnesium nitrate and magnesium sulfate.

[0021] The method for preparing a catalytic cracking catalyst by an ammonium-free process of the present invention, wherein in step (2), the mass ratio of the rare earth-containing silicon-magnesium material to kaolin is 0.1-20:100, the mass ratio of the dispersant to kaolin is 1-20:100, preferably 1-15:100, the mass ratio of the reinforcing agent to kaolin is 1-20:100, preferably 2-8:100, and the solid content of the slurry after mixed slurrying is 30-50%.

[0022] In the method for preparing catalytic cracking catalyst by the ammonium-free method of the present invention, the particle size of the microspheres obtained by spraying in step (2) is 20 to 110 μm.

[0023] The method for preparing catalytic cracking catalyst by the ammonium-free method of the present invention, wherein the calcination temperature in step (2) is 600-1000° C., the calcination time is 1-3 hours, and the crystallization conditions are 85-95° C. for 16-36 hours.

[0024] Specifically, when the microspheres are calcined in step (2), low-temperature calcined microspheres can be obtained by calcining at 600-1000°C for 1-3 hours, or high-temperature calcined microspheres can be obtained by calcining at 600-850°C for 1-3 hours, or a mixture of low-temperature calcined microspheres and high-temperature calcined microspheres. After crystallization, the mother liquor is filtered out, and the filter cake is washed with deionized water until the pH is below 10.5, and dried to obtain a crystallized product with good pore structure and anti-wear performance and containing 20-60% NaY molecular sieve.

[0025] The method for preparing catalytic cracking catalyst by the ammonium-free method of the present invention comprises the following steps: the dispersant is sodium silicate and / or sodium pyrophosphate, the reinforcing agent is silica sol and / or aluminum sol, and the order of adding the dispersant and the reinforcing agent is not limited, and they can be added simultaneously or in batches.

[0026] The method for preparing a catalytic cracking catalyst by an ammonium-free process of the present invention, wherein the kaolin in step (2) is one or more of soft kaolin, hard kaolinite and coal gangue, the median diameter is 1.5 to 3.0 μm, the crystal kaolinite content is higher than 80%, the iron oxide content is lower than 1.7%, and the sum of sodium oxide and potassium oxide is lower than 0.5%.

[0027] In the method for preparing catalytic cracking catalyst by the ammonium-free method of the present invention, the concentration of aqueous ammonia in step (3) is 1-25%.

[0028] In the method for preparing a catalytic cracking catalyst by an ammonium-free process described in the present invention, the mass ratio of the boron element to the crystallized product in step (3) is 0.01 to 0.50:1.

[0029] Specifically, the process of step (3) is that the crystallized product is first treated with ammonia water at 20-60° C. for 30-120 min, and the product exchanged with ammonia water is then exchanged with boric acid, and the process conditions of the exchange are: pH 3-6, temperature 90-110° C. The exchange modification of ammonia water and boric acid can change the exchange order, that is, boric acid can be placed first and ammonia water can be placed later, or ammonia water can be placed first and boric acid can be placed later, without special limitation.

[0030] The method for preparing catalytic cracking catalyst by the ammonium-free method of the present invention comprises the following steps: after calcination in step (3), the ignition reduction is within 3%, and a microspherical primary calcined material containing 5-60% of Y-type molecular sieve is obtained.

[0031] The method for preparing a catalytic cracking catalyst without ammonium according to the present invention, wherein the catalyst has a specific surface area of ​​200 to 500 m 2 / g, pore volume 0.40~0.55mL / g.

[0032] There is no particular restriction on the composition of the directing agent in the present invention. A common directing agent can be used. For example, the directing agent composition in Example 1 of CN1232862A is prepared. The molar ratio of the directing agent recommended by the present invention is: (14-16)SiO2: (0.7-1.3)Al2O3: (14-16)Na2O: (300-330)H2O.

[0033] The method for preparing catalytic cracking catalyst by the ammonium-free method of the present invention, wherein the pretreatment furnace comprises a feeding section, a roasting section and a discharging section, the total length of the pretreatment furnace is 0.5 to 5 meters, the inner diameter is 0.01 to 1 meter, and the roasting temperature is 100 to 1000°C.

[0034] The method for preparing catalytic cracking catalyst by the ammonium-free method described in the present invention, wherein the pretreatment furnace includes a heating system and a ventilation system, the heating system is arranged on the outer layer of the pretreatment furnace in the form of a furnace tile jacket, and the ventilation system is arranged on the inner wall of the pretreatment furnace, and the ventilation system can input dry gas, nitrogen or water vapor into the interior of the pretreatment furnace.

[0035] The method for preparing catalytic cracking catalyst by the ammonium-free method described in the present invention, wherein the angle α between the pretreatment furnace feed section and the pretreatment furnace body is greater than 10° and less than 90°, and the angle β between the pretreatment furnace body and the horizontal position is greater than 10° and less than 90°.

[0036] In the method for preparing catalytic cracking catalyst by the ammonium-free method of the present invention, a shaft rotating device is provided on the top of the pretreatment furnace to control the rotation of the furnace body of the pretreatment furnace, and the rotation frequency is 10 to 80 Hz / min.

[0037] The method for preparing catalytic cracking catalyst by the ammonium-free method of the present invention, wherein the down-going bed isomorphous substitution reactor is divided into a buffer zone and a reaction zone from top to bottom, a catalyst inlet is provided at the top of the buffer zone, an atomizer connected to the catalyst inlet is provided at the upper part of the buffer zone, a nitrogen inlet carrying silicon tetrachloride is provided at the bottom of the reaction zone, a discharge port is provided at the upper part of the reaction zone, the inner diameter ratio of the buffer zone to the reaction zone is 1:1 to 4:1, preferably 1:1 to 3:1, and the heights of the buffer zone and the reaction zone are independently 0.2 to 1 meter.

[0038] The method for preparing catalytic cracking catalyst by the ammonium-free method of the present invention, wherein the inner diameter ratio of the buffer zone to the reaction zone is 1:1 to 3:1; preferably, a heating jacket or a heating belt is provided on the outer wall of the down-going bed isomorphous substitution reactor; preferably, the cavity diameter of the reaction zone is 0.05 to 0.5 meters.

[0039] The method for preparing catalytic cracking catalyst by the ammonium-free method of the present invention, wherein the atomizer is made of stainless steel, contains a plurality of symmetrically distributed air holes, the diameter of the air holes is 80-200um, and the gas pressure inside the atomizer is 0.1-6MPa.

[0040] The method for preparing a catalytic cracking catalyst by an ammonium-free process of the present invention comprises the following steps: in step (4), the isomorphous substitution reaction temperature is 200-900° C., preferably, the temperature is 300-600° C., the time for the primary calcined material to contact with silicon tetrachloride gas is 0.1-60 min, nitrogen is used as a carrier gas to carry silicon tetrachloride into the reactor, and the proportion of silicon tetrachloride to the total carrier gas is 0.1-100%.

[0041] The characteristic of this invention is that rare earth-modified silicon-magnesium materials are added during the construction of the catalyst precursor pore structure. Depending on the preparation conditions, it can have a rich pore structure and a high specific surface area, form a cross-linked structure inside the microsphere precursor, change the interwoven structure of the microspheres, increase the molecular sieve growth points, and thus obtain a higher molecular sieve content. In addition, in the post-modification stage, through the exchange modification of ammonia water and boric acid, the polymers such as silicon aluminum adhering to the surface of the intermediate product are effectively cleaned up, and the pores are further connected; the introduction of boron, combined with rare earth modification, can further enhance the catalyst's heavy oil conversion and heavy metal resistance capabilities.

[0042] In addition to the above-mentioned technology, the present invention adopts a down-flowing bed isomorphous substitution reactor in the post-modification stage to carry out isomorphous substitution reaction in countercurrent contact with silicon tetrachloride. In the reactor design, the flow rate of the catalyst can be changed and the efficiency of contact with silicon tetrachloride can be improved through the design of the zoned variable diameter reaction and the feed atomizer, thereby ensuring the uniformity of the reaction between the material and silicon tetrachloride and improving the reaction efficiency.

[0043] In summary, the present invention utilizes rare earth aged silicon magnesium material and modification of ammonia water and boric acid to make up for the shortcomings of underdeveloped mesopores and unsatisfactory pore structure distribution brought about by the traditional isomorphous substitution process, and then combines the isomorphous substitution process to prepare an in-situ crystallization catalyst with excellent performance and simple process flow.

[0044] The beneficial effects of the present invention are:

[0045] 1. The pore volume of the catalyst is developed and the molecular sieve content is increased. The introduced magnesium silicon material forms a cross-linked structure inside the microsphere precursor, improves the pore structure and specific surface area of ​​the microsphere precursor, changes the synthetic microenvironment, and combines the seed crystal and crystallization synthesis conditions, thereby effectively increasing the number of molecular sieve growth points and significantly increasing the molecular sieve content.

[0046] 2. Improved the efficiency of isomorphous substitution reaction. In the design of the reactor, the flow rate of the catalyst can be changed and the efficiency of contact with silicon tetrachloride can be improved through the design of the zoned variable diameter reaction and the feed atomizer, thereby ensuring the uniformity of the reaction between the material and silicon tetrachloride and improving the reaction efficiency.

[0047] 3. The material is in more complete contact and the reaction efficiency is high. According to the characteristics of the catalytic cracking catalyst microsphere particles, the gas-solid phase reaction principle of the descending bed mode is adopted. The material descends along the gravity field, and SiCl4 contacts the material from bottom to top under the action of the carrier gas. This contact mode can not only effectively overcome the problems of catalyst back mixing and uneven radial distribution of catalyst particles caused by the reverse gravity operation of the ascending riser, but also realize ultra-short contact operation between the material and the reactant due to the increase in the gas-solid two-phase flow rate, and the reaction is uniform, so the excellent reaction effect is very outstanding, which is very suitable for the rapid processing reaction process of gas and solid phases.

[0048] 4. No ammonia nitrogen is generated during the modification process. The isomorphous substitution reaction greatly improves the efficiency of reducing sodium oxide without the need for ammonium salt exchange. BRIEF DESCRIPTION OF THE DRAWINGS

[0049] Figure 1 This is a schematic diagram of the structure of a down-bed isomorphous substitution reactor.

[0050] Figure 2 The present invention is a schematic diagram of the structure of an apparatus for preparing catalytic cracking catalyst by an ammonium-free method.

[0051] Figure 3 It is the angle between the pretreatment section and the pretreatment furnace.

[0052] Figure 4 This is a schematic diagram of the structure of the pretreatment furnace.

[0053] Figure 5 The catalyst adsorption curves of the catalysts obtained in Example 1 and Comparative Example 2 of the present invention tested with naphthalene as the probe molecule;

[0054] Figure 6 The catalyst adsorption curves of the catalysts obtained in Example 1 and Comparative Example 2 of the present invention were tested using quinoline as a probe molecule.

[0055] in:

[0056] 1. Pretreatment furnace, 2. Downward bed isomorphous substitution reactor, 3. Absorption tower, 4. Exchange, filter and flash drying equipment;

[0057] 11. Feeding section, 12. Roasting section, 13. Discharging section, 14. Shaft rotating device, 15. Heating system, 16. Ventilation system,

[0058] 21. Buffer zone, 22. Reaction zone, 23. Catalyst inlet, 24. Atomizer, 25. Nitrogen inlet carrying silicon tetrachloride, 26. Discharge port, 27. Heating jacket. DETAILED DESCRIPTION

[0059] The present invention is described in detail below by way of examples. It is necessary to point out that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Those skilled in the art in this field can make some non-essential improvements and adjustments to the present invention based on the above content of the present invention.

[0060] See also Figure 1 As shown, the down-bed isomorphous substitution reactor 2 provided by the present invention is divided into a buffer zone 21 and a reaction zone 22 from top to bottom, a catalyst inlet 23 is provided at the top of the buffer zone 21, an atomizer 24 connected to the catalyst inlet 23 is provided at the upper part of the buffer zone 21, a nitrogen inlet 25 carrying silicon tetrachloride is provided at the bottom of the reaction zone 22, a discharge port 26 is provided at the upper part of the reaction zone 22, an inner diameter ratio of the buffer zone 21 to the reaction zone 22 is 1:1-4:1, the heights of the buffer zone 21 and the reaction zone 22 are independently 0.2-1 meter, and the weight ratio of silicon tetrachloride to the catalyst when reacting in the reaction zone 22 is 0.01-0.5:1.

[0061] Also, see Figure 1 As shown, a heating jacket 27 is provided on the outer wall of the down-bed isomorphous substitution reactor 2. Of course, in other embodiments, the heating jacket 27 can be replaced by other heating structures, such as a heating belt.

[0062] In some embodiments, the cavity diameter of the reaction zone 22 is preferably 0.05 to 0.5 meters, and the height is preferably 0.2 to 1 meter.

[0063] In some embodiments, the inner diameter ratio of the buffer zone 21 to the reaction zone 22 is preferably 1:1 to 3:1.

[0064] In some embodiments, the atomizer 24 is made of stainless steel, and contains a plurality of symmetrically distributed air holes, the diameter of the air holes is 80-200 um, and the gas pressure inside the atomizer 24 is 0.1-6 MPa.

[0065] See also Figure 2 As shown, the device for preparing catalytic cracking catalyst by the ammonium-free method provided by the present invention comprises:

[0066] Pretreatment furnace 1, used for calcination or hydrothermal treatment of catalyst to obtain pretreated catalyst;

[0067] The above-mentioned down-bed isomorphous substitution reactor 2 is used to carry out isomorphous substitution reaction on the pretreated catalyst to obtain the reacted catalyst;

[0068] Absorption tower 3, used to purge the reacted catalyst from the feed port into the absorption tower, and then the tail gas neutralization reaction occurs to obtain a catalyst intermediate;

[0069] The exchange, filter and flash drying equipment 4 includes an exchange filter for exchanging and filtering the catalyst intermediates; and a flash drying device for flashing and drying the catalyst intermediates.

[0070] Also, see Figure 3 As shown, the pretreatment furnace 1 comprises a feeding section 11, a roasting section 12 and a discharging section 13. The total length of the pretreatment furnace 1 is 0.5 to 5 meters, the inner diameter is 0.01 to 1 meter, and the roasting temperature is 100 to 1000°C.

[0071] Also, see Figure 4 As shown, the pretreatment furnace 1 includes a heating system 15 and a ventilation system 16. The heating system 15 is arranged on the outer layer of the pretreatment furnace 1 in the form of a furnace tile jacket, and the ventilation system 16 is arranged on the inner wall of the pretreatment furnace 1. The ventilation system 16 can input dry gas, nitrogen or water vapor into the interior of the pretreatment furnace 1.

[0072] Also, see Figure 3 As shown, the angle α between the feed section 11 of the pretreatment furnace 1 and the main body of the pretreatment furnace 1 is greater than 10° and less than 90°; Figure 4 As shown, the angle β between the main body of the pretreatment furnace 1 and the horizontal position is greater than 10° and less than 90°. The top of the pretreatment furnace 1 is provided with an axis rotating device 14, and the furnace body can rotate to achieve the turning of the material, and the rotation frequency is 10-80Hz / min.

[0073] Source of raw materials:

[0074] 1) Kaolin: industrial product, sourced from the catalyst plant of Lanzhou Petrochemical Company

[0075] 2) Magnesium chloride, chemically pure, Sinopharm Chemical Reagent Co., Ltd.

[0076] 3) Sodium silicate solution: industrial product, collected from Lanzhou Petrochemical Company Catalyst Plant, (SiO2: 19.75%, Na2O: 6.95%, H2O: 73.30%)

[0077] 4) Alkaline silica sol: industrial product, Yantai Hengxin Chemical Technology Co., Ltd., (SiO2: 30%)

[0078] 5) Directing agent: industrial agent, collected from Lanzhou Petrochemical Company Catalyst Plant, ratio: 16SiO2:0.8Al2O3:15.7Na2O:312H2O

[0079] 6) NaOH solution: industrial product, collected from the catalyst plant of Lanzhou Petrochemical Company (NaOH: 24%)

[0080] 7) Sodium pyrophosphate: analytical grade, Tianjin Komiou Chemical Reagent Co., Ltd.

[0081] 8) Alumina sol: industrial product, sourced from Lanzhou Petrochemical Company Catalyst Plant (Al2O3: 21.22%)

[0082] 9) Hydrochloric acid: chemically pure

[0083] 10) Ammonium nitrate: chemically pure

[0084] 11) Ammonium chloride: chemically pure

[0085] 12) Ammonium sulfate, chemically pure

[0086] 13) Ammonia: Chemically pure

[0087] 14) Boric acid: chemically pure

[0088] Specific analysis method:

[0089] The crystallinity of NaY molecular sieve was tested on a D / max-3C X-ray powder diffractometer manufactured by Rigaku, Japan, using X-ray diffraction to determine the crystallinity of the sample. The method standard is Q / SYLS0596~2002. The silicon-aluminum ratio of NaY molecular sieve was tested using X-ray powder diffraction, and the method standard is Q / SYLS0573~2002. The sample wear index was measured using the air lift method. A certain amount of sample was placed in a fixed device and blown for 5 hours under a constant airflow. Except for the first hour, the average wear percentage in the last four hours is called the catalyst wear index, in % per hour. The method and standard are: air lift method Q / SYLS0518-2002. The sample pore distribution test was performed using the Autosorb~3B specific surface measuring instrument of Quantachrome, USA, and the specific surface area, pore size distribution and pore volume of the sample were determined by the N2 low temperature (77.3K) adsorption-desorption experimental method. Microreaction activity (MA) evaluation: ASTM-D3907 method was used, the catalyst was pre-treated at 800℃, 100% water vapor for 17h, Dagang light diesel was used as the reaction raw oil, the reaction temperature was 460℃, the oil injection time was 70s, the catalyst loading was 2.5-5g, and the gasoline yield after the reaction was analyzed by GC7890.

[0090] A dynamic adsorption rate curve test system and a supporting data acquisition and analysis system workstation are used to detect the adsorption process of model probes and heavy oil macromolecules on porous catalyst materials. Based on adsorption models such as Fick's law, Maxwell-Stefan equation and Dobbins empirical formula, a set of supporting data analysis software is preliminarily developed. The diffusion coefficient diagram of probe molecules in the catalyst material during the adsorption process is obtained through a reasonable algorithm.

[0091] Example 1

[0092] 84 grams of alkaline silica sol were measured, 20g of magnesium chloride was dissolved in 100mL of distilled water, and the alkaline silica sol was slowly injected into the dissolved magnesium chloride solution and mixed for 30 minutes to obtain a silicon-magnesium material with a final pH value of 8.2. Lanthanum nitrate rare earth was added, lanthanum nitrate (calculated as cerium oxide) / silicon-magnesium material = 20% (mass ratio), and the material after adding rare earth was aged at 80°C for 5min. 100g of the aged material, 800g of kaolin (calcined base), 40g of sodium silicate solution, 160g of alkaline silica sol, and deionized water were prepared into a mixed slurry with a solid content of 46%, and spray dried to obtain 600g of spray microspheres P1 with a particle size of 20 to 110μm. A part of the P1 spray soil ball was calcined at 980°C for 2.7 h to obtain the calcined microsphere G1, and the other part was calcined at 650°C for 2.5 h to obtain the calcined microsphere B1. Then, 100g G1 and 300g B1 were mixed, and sodium silicate solution, directing agent, sodium hydroxide solution, and deionized water were added. The mixture was hydrothermally crystallized at 95°C for 30 h, the mother liquor was filtered out, and the product was washed with water and dried to obtain the product J1.

[0093] 200 g of the product J1 prepared in Example 1 was added to a stainless steel kettle under stirring. A 25% ammonia solution was added and treated for 100 min at room temperature. The washed material was filtered and exchanged with boric acid. The exchange process conditions were: pH 3.5, temperature 90°C, B: exchange material (dry basis) = 0.50 (mass ratio). After 100 min, dry gas was introduced into the material in a pretreatment furnace and roasted at 500°C and 100% water vapor for 2 hours to obtain a roasted material. 200 grams of a roasted material with a burning reduction of 2.8% is slowly added to the top of the descending bed reactor through a feeder. The top of the reactor is an atomizer with a gas eye diameter of 200μm and a pressure of 6MPa. After the spraying of the atomizer, the catalyst particles are dispersed in the reactor, run downward, and meet silicon tetrachloride gas. The proportion of silicon tetrachloride to the carrier gas is 100%. The reaction temperature is: 900℃, and the contact time with the gas is 0.1min. The gas flow rate is controlled to ensure that the ratio of silicon tetrachloride to a roasted material is 0.5:1. The inner diameter of the buffer zone and the reaction zone are both: 0.05 meters, and the heights are: 0.2 and 0.3 meters respectively. After the reacted material enters the absorption tower for 30 minutes of purging, the reacted gas is discharged through the gas outlet pipe by pumping and enters the recovery system. The recovery system is a 10% sodium hydroxide solution, and the reacted gas is acid-base neutralized and collected. The catalyst was collected by the collector at the bottom of the absorption tower, washed with 19 times water at 85°C for 0.5h, and dried to obtain catalyst C-1 with a Na2O content of 0.43%.

[0094] Example 2

[0095] 120g of magnesium nitrate was dissolved in 320mL of distilled water, and the dissolved solution was slowly injected into 2092g of water glass solution containing 20% ​​SiO2, mixed for 50 minutes, and silicon magnesium material was obtained, and the final pH value was 13.1, and then cerium chloride rare earth was added, cerium chloride (calculated as cerium oxide) / silicon magnesium material = 2.3% (mass ratio), and the material after adding rare earth was aged at 120°C for 300min, and 10g of the aged material, 1000g of kaolin (calcined base), 70g of sodium pyrophosphate, 10g of aluminum sol, and deionized water were prepared into a mixed slurry with a solid content of 32%, spray dried, and 600g of spray microspheres P2 with a particle size of 20-110μm were obtained. The P2 spray soil ball was roasted at 990°C for 1.5h to obtain the roasted microsphere G2. 100 g of G2 was added into sodium silicate solution, directing agent, sodium hydroxide solution and deionized water, and hydrothermally crystallized at 85° C. for 26 h. The mother liquor was filtered out, and the product J2 was obtained by washing with water and drying.

[0096] 80 g of the product J2 prepared in Example 2 was added to a stainless steel kettle under stirring, and boric acid was used for exchange. The exchange process conditions were: pH 4.5, temperature 95 ℃, B: exchange material (dry basis) = 0.15 (mass ratio), filtered and washed after 40min, then added 10% ammonia solution at 20 ℃, liquid-to-solid ratio of 8, treated for 100min, then the material was roasted in a pretreatment furnace at 700 ℃, 80% water vapor for 0.5 hour to obtain a roasted material with a loss on ignition of 1.8%; 80 grams of roasted material was slowly added to the top of the descending bed reactor through a feeder, the top of the reactor was an atomizer with an air eye diameter of 50 μm and a pressure of 0.1 MPa, and the catalyst particles were dispersed in the reactor through the spraying of the atomizer, and the downward operation met with silicon tetrachloride gas, the proportion of silicon tetrachloride to carrier gas was 10%, the gas-solid phase reaction temperature was 200 ℃, the contact time with the gas was 3min, and the flow of the gas was controlled to ensure that the ratio of silicon tetrachloride to the in-situ crystallization catalyst was 0.01:1. The inner diameters of the buffer zone and the reaction zone are 0.5 meters and 0.125 meters respectively, and the heights are both 1 meter. The reacted material is purged in the absorption tower for 15 minutes. The gas is pumped out through the gas outlet pipe and enters the recovery system. The recovery system is a 20% sodium carbonate solution, which neutralizes and collects the reacted gas. After the catalyst is collected by the collector at the bottom of the absorption tower, it is washed with 5 times water at 95°C for 1 hour and dried to obtain catalyst C-2 with a Na2O content of 0.34%.

[0097] Example 3

[0098] 80g of magnesium sulfate was dissolved in 300mL of distilled water, and 139g of white carbon black was dissolved in 300ml of distilled water to form a turbid solution. The magnesium sulfate solution was slowly injected into the white carbon black solution and mixed for 80 minutes to obtain a silicon-magnesium material with a final pH value of 8.5. Yttrium carbonate was then added, and yttrium carbonate (in terms of yttrium oxide) / silicon-magnesium material = 9.7% (mass ratio). The material after adding rare earth was aged at 115°C for 200min. 100g of the aged material, 1250g of kaolin (calcined base), 187.5g of sodium silicate solution, 187.5g of aluminum sol, and deionized water were prepared into a mixed slurry with a solid content of 40%, and spray dried to obtain 1200g of spray microspheres P3 with a particle size of 20 to 110μm. The P3 spray soil ball was roasted at 780°C for 1.5h to obtain the roasted microspheres G3. 500 g of G3 was added into sodium silicate solution, directing agent, sodium hydroxide solution and deionized water, and hydrothermally crystallized at 85° C. for 38 h. The mother liquor was filtered out, and the product J3 was obtained by washing with water and drying.

[0099] 400 g of the product J3 prepared in Example 3 was added to a stainless steel kettle under stirring, and a 5% ammonia solution was added at 40° C. with a liquid-to-solid ratio of 10. The mixture was treated for 120 min. After filtering and washing, boric acid was used for exchange. The exchange process conditions were: pH 5.8, temperature 92° C., B: exchange material (dry basis) = 0.38 (mass ratio). After 45 min, the material was calcined at 900° C. under 30% water vapor in a pretreatment furnace for 0.5 hour to obtain a calcined material with a loss on ignition of 0.8%. A roasted material is slowly added to the top of the descending bed reactor through a feeder. The top of the reactor is an atomizer with an air hole diameter of 80μm and a pressure of 4MPa. After being sprayed by the atomizer, the catalyst particles are dispersed in the reactor, run downward, and meet silicon tetrachloride gas. The proportion of silicon tetrachloride to the carrier gas is 30%. The gas-solid phase reaction temperature is 400℃, and the contact time with the gas is 60min. The gas flow rate is controlled to ensure that the ratio of silicon tetrachloride to the in-situ crystallization catalyst is 0.4:1. The inner diameters of the buffer zone and the reaction zone are 0.4m and 0.2m respectively, and the heights are 0.5m and 0.2m respectively. The reacted material is purged for 40min, and the gas is discharged through the gas outlet pipe by pumping and enters the recovery system. The recovery system is a 12% sodium hydroxide solution, and the reacted gas is acid-base neutralized and collected. After the catalyst is collected by the collector at the bottom of the absorption tower, it is washed with 15 times water at 65℃ for 1h and dried to obtain catalyst C-3 with a Na2O content of 0.25%.

[0100] Example 4

[0101] 130g of magnesium carbonate was dissolved in 500mL of distilled water, and the dissolved magnesium carbonate solution was slowly added to 4643g of alkaline silica sol and mixed for 90 minutes to obtain a silicon-magnesium material with a final pH of 7.3. Cerium nitrate was then added, cerium nitrate (calculated as cerium oxide) / silicon-magnesium material = 1.4% (mass ratio). The material after adding rare earth was aged at 100°C for 150min. 200g of the aged material, 1818g of kaolin (calcined), 345.42g of sodium silicate solution, 290.88g of aluminum sol, and deionized water were prepared into a mixed slurry with a solid content of 47%, which was spray-dried to obtain 1600g of spray microspheres P4 with a particle size of 20 to 110μm. A portion of P4 was calcined at 1000°C for 1.5 h to obtain calcined microspheres G4, and the other portion was calcined at 600°C for 2 h to obtain calcined microspheres B4. Then 1000 g of G4 and 250 g of B4 were added to sodium silicate solution, a directing agent, a sodium hydroxide solution, and deionized water, and hydrothermally crystallized at 89°C for 30 h. The mother liquor was filtered out, and the product was washed with water and dried to obtain product J4.

[0102] 600 g of the crystallized product J4 prepared in Example 4 was added to a stainless steel kettle under stirring, and an 8% ammonia solution was added at 60° C. with a liquid-to-solid ratio of 1.5. The mixture was treated for 50 min. After filtering and washing, boric acid was used for exchange. The exchange process conditions were: pH 3.9, temperature 88° C., B: exchange material (dry basis) = 0.22 (mass ratio). After 120 min, the material was calcined in a pretreatment furnace at 600° C. and 50% water vapor for 1 hour to obtain a calcined material with a loss on ignition of 1.2%. The roasting material is slowly added to the top of the descending bed reactor through a feeder. The top of the reactor is an atomizer with a gas eye diameter of 150μm and a pressure of 3MPa. After being sprayed by the atomizer, the catalyst particles are dispersed in the reactor and run downward to meet silicon tetrachloride gas. The proportion of silicon tetrachloride to the carrier gas is 50%. The gas-solid phase reaction temperature is 500℃, and the contact time with the gas is 30min. The gas flow rate is controlled to ensure that the ratio of silicon tetrachloride to the in-situ crystallization catalyst is 0.05:1. The inner diameters of the buffer zone and the reaction zone are 0.3m and 0.15m respectively, and the heights are 0.3m and 0.7m respectively. The reacted material is purged in the absorption tower for 60min, and the gas is discharged through the gas outlet pipe by pumping and enters the recovery system. The recovery system is a 15% sodium hydroxide solution, which neutralizes and collects the reacted gas. The catalyst was collected by the collector at the bottom of the absorption tower, washed with twice the amount of water at 35°C for 2 hours, and dried to obtain catalyst C-4 with a Na2O content of 0.49%.

[0103] Example 5

[0104] 50g of magnesium nitrate was dissolved in 200ml of distilled water, and 132g of white carbon black was gradually dissolved in 300ml of distilled water to form a turbid solution. The dissolved magnesium nitrate solution was slowly added to the white carbon black turbid solution and mixed for 30 minutes to obtain a silicon-magnesium material with a final pH value of 9.3. Lanthanum chloride was then added, and lanthanum chloride (calculated as lanthanum oxide) / silicon-magnesium material = 13.7% (mass ratio). The material after adding rare earth was aged at 95°C for 250min. 200g of the aged material, 1053g of kaolin (calcined), 136.89g of sodium silicate solution, 136.89g of alkaline silica sol, and deionized water were prepared into a mixed slurry with a solid content of 43%, which was spray-dried to obtain 900g of spray microspheres P5 with a particle size of 20 to 110μm. A portion of P5 was calcined at 970°C for 2.3 h to obtain calcined microspheres G5, and the other portion was calcined at 830°C for 1.9 h to obtain calcined microspheres B5. Then 400 g of G5 and 400 g of B5 were added to sodium silicate solution, a directing agent, a sodium hydroxide solution, and deionized water, and hydrothermally crystallized at 87°C for 16 h. The mother liquor was filtered out, and the product was washed with water and dried to obtain product J5.

[0105] 600 g of the crystallized product prepared in Example 5 was added to a stainless steel kettle under stirring, and boric acid was used for exchange. The exchange process conditions were: pH 3.6, temperature 85°C, B: exchange material (dry basis) = 0.01 (mass ratio). After 15 minutes, it was filtered and washed, and then a 15% ammonia solution was added at 40°C with a liquid-to-solid ratio of 4 for 80 minutes. Then, the material was calcined in a pretreatment furnace at 800°C with 100% water vapor for 1.5 hours to obtain a calcined material with a loss on ignition of 1.9%. 400 grams of roasted material is slowly added to the top of the descending bed reactor through a feeder. The top of the reactor is an atomizer with a gas eye diameter of 180μm and a pressure of 5MPa. After being sprayed by the atomizer, the catalyst particles are dispersed in the reactor and run downward to meet silicon tetrachloride gas. The proportion of silicon tetrachloride to the carrier gas is 80%. The gas-solid phase reaction temperature is 600℃, and the contact time with the gas is 50min. The gas flow rate is controlled to ensure that the ratio of silicon tetrachloride to the in-situ crystallization catalyst is 0.45:1. The inner diameters of the buffer zone and the reaction zone are 0.45 meters and 0.3 meters respectively, and the heights are 0.7 meters and 0.5 meters respectively. The reacted gas is discharged through the gas outlet pipe by pumping and enters the recovery system. The recovery system is a 10% sodium hydroxide solution. After the reacted material is purged in the absorption tower for 25 minutes, the gas is acid-base neutralized and collected. The catalyst was collected by the collector at the bottom of the absorption tower, washed with 8 times water at 75°C for 1.5h, and dried to obtain catalyst C-5 with a Na2O content of 0.42%.

[0106] Example 6

[0107] 80g of magnesium sulfate was dissolved in 300mL of distilled water, and the dissolved solution was slowly added to 1860g of sodium silicate solution and mixed for 40 minutes to obtain a silicon-magnesium material with a final pH value of 12.3. Lanthanum carbonate was then added, lanthanum carbonate (calculated as lanthanum oxide) / silicon-magnesium material = 4.8% (mass ratio). The material after adding rare earth was aged at 90°C for 50min. 300g of the aged material, 5000g of kaolin (calcined base), 450g of sodium pyrophosphate, 450g of silica sol, and deionized water were prepared into a mixed slurry with a solid content of 38%, which was spray-dried to obtain 4500g of spray microspheres P6 with a particle size of 20 to 110μm. A portion of P6 was calcined at 960°C for 1.4 h to obtain calcined microspheres G6, and the other portion was calcined at 880°C for 2 h to obtain calcined microspheres B6. Then 600 g of G6 and 400 g of B6 were added to sodium silicate solution, a directing agent, a sodium hydroxide solution, and deionized water, and hydrothermally crystallized at 92°C for 34 h. The mother liquor was filtered out, and the product was washed with water and dried to obtain product J6.

[0108] 820 g of the crystallized product J6 prepared in Example 6 was added to a stainless steel kettle under stirring, and boric acid was used for exchange. The exchange process conditions were: pH 4.0, temperature 93°C, B: exchange material (dry basis) = 0.45 (mass ratio). After 60 minutes, it was filtered and washed, and then a 20% ammonia solution was added at 60°C with a liquid-to-solid ratio of 7. The treatment lasted for 90 minutes. Then, the material was calcined in a pretreatment furnace at 650°C and 10% water vapor for 1.5 hours to obtain a calcined material with a loss on ignition of 1.1%. 750 grams of roasting material is slowly added to the top of the descending bed reactor through a feeder. The top of the reactor is an atomizer with a gas eye diameter of 130μm and a pressure of 2.2MPa. After being sprayed by the atomizer, the catalyst particles are dispersed in the reactor and run downward to meet silicon tetrachloride gas. The proportion of silicon tetrachloride to the carrier gas is 90%. The gas-solid phase reaction temperature is 300℃, and the contact time with the gas is 20min. The gas flow rate is controlled to ensure that the ratio of silicon tetrachloride to the in-situ crystallization catalyst is 0.36:1. The inner diameters of the buffer zone and the reaction zone are 0.2m and 0.1m respectively, and the heights are 0.4m and 0.6m respectively. The reacted material is purged in the absorption tower for 30min, and the gas is discharged by pumping through the gas outlet pipe and enters the recovery system. The recovery system is a 5% sodium carbonate solution, and the reacted gas is acid-base neutralized and collected. The catalyst was collected by the collector at the bottom of the absorption tower, washed with 5 times water at 85°C for 0.6h, and dried to obtain catalyst C-6 with a Na2O content of 0.38%.

[0109] Example 7

[0110] 242g of alkaline silica sol solution was slowly added to 70g of magnesium chloride solution dissolved in 300mL of distilled water, and mixed for 55 minutes to obtain a silicon-magnesium material with a final pH value of 11.5. Cerium nitrate was then added, cerium nitrate (calculated as cerium oxide) / silicon-magnesium material = 8.2% (mass ratio). The material after adding rare earth was aged at 98°C for 90min. 100g of the aged material, 2500g of kaolin (calcined base), 50g of sodium silicate solution, 75g of aluminum sol, and deionized water were prepared into a mixed slurry with a solid content of 36%, which was spray-dried to obtain 1500g of spray microspheres P7 with a particle size of 20 to 110μm. Part of P7 was calcined at 850°C for 2.3h to obtain calcined microspheres G7, and the other part was calcined at 680°C for 2.6h to obtain calcined microspheres B7. Then 750g of G7 and 250g of B7 were added to sodium silicate solution, directing agent, sodium hydroxide solution, and deionized water, and hydrothermally crystallized at 92°C for 32h. The mother liquor was filtered out, and the product was washed with water and dried to obtain product J7.

[0111] 550 g of the crystallized product J7 prepared in Example 7 was added to a stainless steel kettle under stirring, and a 23% ammonia solution was added at 20° C. with a liquid-to-solid ratio of 3. The mixture was treated for 40 min. After filtering and washing, boric acid was used for exchange. The exchange process conditions were: pH 4.2, temperature 95° C., B: exchange material (dry basis) = 0.09 (mass ratio). After 90 min, the material was calcined in a pretreatment furnace at 750° C. and 60% water vapor for 0.5 hour to obtain a calcined material with a loss on ignition of 2.4%. 500 grams of roasted material is slowly added to the top of the descending bed reactor through a feeder. The top of the reactor is an atomizer with a gas eye diameter of 70μm and a pressure of 3.5MPa. After being sprayed by the atomizer, the catalyst particles are dispersed in the reactor and run downward to meet silicon tetrachloride gas. The proportion of silicon tetrachloride in the carrier gas is 60%. The gas-solid phase reaction temperature is 800℃, and the contact time with the gas is 10min. The gas flow rate is controlled to ensure that the ratio of silicon tetrachloride to the in-situ crystallization catalyst is 0.25:1. The inner diameter of the buffer zone and the reaction zone are both 0.25 meters, and the heights are 0.6 meters and 0.9 meters respectively. After the reacted material is purged through the absorption tower for 20 minutes, the gas is discharged through the gas outlet pipe by pumping and enters the recovery system. The recovery system is a 13% sodium hydroxide solution, and the reacted gas is acid-base neutralized and collected. The catalyst was collected by the collector at the bottom of the absorption tower, washed with 13 times water at 85°C for 2h, and dried to obtain catalyst C-7 with a Na2O content of 0.43%.

[0112] Example 8

[0113] 90g of magnesium nitrate was dissolved in 300mL of distilled water, and the dissolved solution was slowly added to 948g of sodium silicate solution and mixed for 25 minutes to obtain a silicon-magnesium material with a final pH value of 10.5. Cerium chloride was then added, cerium chloride (calculated as cerium oxide) / silicon-magnesium material = 11% (mass ratio). The material after adding rare earth was aged at 93°C for 120min. 120g of the aged material, 750g of kaolin (calcined base), 60g of sodium silicate solution, 52.5g of aluminum sol, and deionized water were prepared into a mixed slurry with a solid content of 42%, which was spray-dried to obtain 750g of spray microspheres P8 with a particle size of 20 to 110μm. P8 was calcined at 630°C for 2.1 h to obtain calcined microspheres B8, and then 700 g of B8 was added to sodium silicate solution, directing agent, sodium hydroxide solution, and deionized water, and hydrothermally crystallized at 94°C for 36 h. The mother liquor was filtered out, and the product J8 was obtained by washing with water and drying.

[0114] 450g of the crystallized product J8 prepared in Example 8 was added to a stainless steel kettle under stirring, and exchanged with boric acid. The exchange process conditions were: pH 3.7, temperature 90°C, B: exchange material (dry basis) = 0.32 (mass ratio), filtered and washed after 30 minutes. 18% ammonia solution was added at 30°C, with a liquid-to-solid ratio of 5, and treated for 60 minutes. Then the material was roasted in a pretreatment furnace at 750°C and a water vapor amount of 60% for 0.5 hour to obtain a roasted material with a loss on ignition of 2.2%. The calcined material is slowly added to the top of the descending bed reactor through a feeder. The top of the reactor is an atomizer with an air hole diameter of 85μm and a pressure of 4.7MPa. After being sprayed by the atomizer, the catalyst particles are dispersed in the reactor and run downward to meet silicon tetrachloride gas. The proportion of silicon tetrachloride to the carrier gas is 20%. The gas-solid phase reaction temperature is 700℃, and the contact time with the gas is 2min. The gas flow rate is controlled to ensure that the ratio of silicon tetrachloride to the in-situ crystallization catalyst is 0.14:1. The inner diameters of the buffer zone and the reaction zone are 0.3m and 0.15m, respectively, and the heights are 0.8m and 1m, respectively. After the reacted material is purged in the absorption tower for 50min, the gas is discharged through the gas outlet pipe by pumping and enters the recovery system. The recovery system is a 10% sodium carbonate solution, which neutralizes and collects the reacted gas. After the catalyst is collected by the collector at the bottom of the absorption tower, it is washed with 8 times water at 95℃ for 2h and dried to obtain catalyst C-8 with a Na2O content of 0.38%.

[0115] Example 9

[0116] 170g of magnesium nitrate was dissolved in 600mL of distilled water, and 933g of white carbon was gradually dissolved in 1000ml of distilled water to form a turbid solution. The dissolved magnesium nitrate solution was slowly added to the white carbon turbid solution and mixed for 90 minutes to obtain a silicon-magnesium material with a final pH value of 7.3. Yttrium carbonate was then added, and yttrium carbonate (in terms of yttrium oxide) / silicon-magnesium material = 15.6% (mass ratio). The material after adding rare earth was aged at 83°C for 30min. 120g of the aged material, 4000g of kaolin (calcined base), 600g of sodium pyrophosphate, 720g of alkaline silica sol, and deionized water were prepared into a mixed slurry with a solid content of 42%, which was spray-dried to obtain 750g of spray microspheres P9 with a particle size of 20 to 110μm. A portion of P9 was calcined at 890°C for 1.5 h to obtain calcined microspheres G9, and the other portion was calcined at 770°C for 1.8 h to obtain calcined microspheres B9. Then 200 g of G9 and 400 g of B9 were added to sodium silicate solution, a directing agent, a sodium hydroxide solution, and deionized water, and hydrothermally crystallized at 88°C for 28 h. The mother liquor was filtered out, and the product was washed with water and dried to obtain product J9.

[0117] 550 g of the crystallized product J9 prepared in Example 9 was added to a stainless steel kettle under stirring, and a 6% ammonia solution was added at 50° C. with a liquid-to-solid ratio of 9. The mixture was treated for 50 min. After filtering and washing, boric acid was used for exchange. The exchange process conditions were: pH 3.9, temperature 89° C., B: exchange material (dry basis) = 0.28 (mass ratio). After 15 min, the material was calcined in a pretreatment furnace at 880° C. and 20% water vapor for 0.5 hour to obtain a calcined material with a loss on ignition of 0.8%. The calcined material is slowly added to the top of the descending bed reactor through a feeder. The top of the reactor is an atomizer with an air hole diameter of 160μm and a pressure of 5.5MPa. After being sprayed by the atomizer, the catalyst particles are dispersed in the reactor, run downward, and meet silicon tetrachloride gas. The proportion of silicon tetrachloride to the carrier gas is 40%. The gas-solid phase reaction temperature is 450℃, and the contact time with the gas is 1min. The gas flow rate is controlled to ensure that the ratio of silicon tetrachloride to the in-situ crystallization catalyst is 0.30:1. The inner diameter of the buffer zone and the reaction zone are both 0.5 meters, and the heights are 0.9 meters and 0.4 meters respectively. After the reacted material is purged by the absorption tower for 35 minutes, the gas is discharged by pumping through the gas outlet pipe and enters the recovery system. The recovery system is an 8% sodium carbonate solution, and the reacted gas is acid-base neutralized and collected. After the catalyst is collected by the collector at the bottom of the absorption tower, it is washed with 10 times water at 95℃ for 1h and dried to obtain catalyst C-9 with a Na2O content of 0.36%.

[0118] Example 10

[0119] 60g of magnesium chloride was dissolved in 200mL of distilled water, and the dissolved solution was slowly added to 191g of alkaline silica sol solution and mixed for 70 minutes to obtain a silicon-magnesium material with a final pH value of 8.5. Cerium nitrate was then added, cerium nitrate (calculated as cerium oxide) / silicon-magnesium material = 5.7% (mass ratio). The material after adding rare earth was aged at 89°C for 280min. 300g of the aged material, 6000g of kaolin (calcined base), 660g of sodium pyrophosphate, 900g of alkaline silica sol, and deionized water were prepared into a mixed slurry with a solid content of 36%, which was spray-dried to obtain 2100g of spray microspheres P10 with a particle size of 20 to 110μm. A portion of P10 was calcined at 830°C for 2.8 hours to obtain calcined microspheres G10, and the other portion was calcined at 670°C for 3.6 hours to obtain calcined microspheres B10. Then, 900g of G10 and 300g of B10 were added to sodium silicate solution, a directing agent, a sodium hydroxide solution, and deionized water, and hydrothermally crystallized at 92°C for 32 hours. The mother liquor was filtered out, and the product was washed with water and dried to obtain product J10.

[0120] 550 g of the crystallized product J10 prepared in Example 10 was added to a stainless steel kettle under stirring, and boric acid was used for exchange. The exchange process conditions were: pH 3.5, temperature 86°C, B: exchange material (dry basis) = 0.40 (mass ratio). After 120 minutes, 13% ammonia solution was added at 50°C, the liquid-to-solid ratio was 5.5, and the treatment was carried out for 70 minutes. After filtering and washing, the material was calcined in a pretreatment furnace at 600°C and 70% water vapor for 2 hours to obtain a calcined material with a loss on ignition of 1.5%. The calcined material is slowly added to the top of the downward bed reactor through a feeder. The top of the reactor is an atomizer with an air hole diameter of 140μm and a pressure of 3MPa. After being sprayed by the atomizer, the catalyst particles are dispersed in the reactor and run downward to meet silicon tetrachloride gas. The proportion of silicon tetrachloride in the carrier gas is 50%. The gas-solid phase reaction temperature is 500℃, and the contact time with the gas is 30min. The gas flow rate is controlled to ensure that the ratio of silicon tetrachloride to the in-situ crystallization catalyst is 0.23:1. The inner diameters of the buffer zone and the reaction zone are 0.3m and 0.15m, respectively, and the heights are 0.3m and 0.7m, respectively. The reacted material is purged in the absorption tower for 60min, and the gas is pumped out through the gas outlet pipe and enters the recovery system. The recovery system is a 15% sodium hydroxide solution, which neutralizes and collects the reacted gas. After the catalyst is collected by the collector at the bottom of the absorption tower,

[0121] The catalyst was then washed with 16 times the amount of water at 75°C for 1 hour and dried to obtain catalyst C-10 with a Na2O content of 0.46%.

[0122] Comparative Example 1

[0123] Compared with Example 3, 139g of white carbon black was dissolved in 300ml of distilled water to form a turbid solution, which was aged at 115°C for 200min. 100g of the aged material, 1250g of kaolin (calcined base), 187.5g of sodium silicate solution, 187.5g of aluminum sol, and deionized water were prepared into a mixed slurry with a solid content of 40%, and spray-dried to obtain 1200g of spray microspheres P11 with a particle size of 20 to 110μm. The P11 spray soil ball was calcined at 780°C for 1.5h to obtain calcined microspheres G11. 500g of G11 was added to sodium silicate solution, directing agent, sodium hydroxide solution, and deionized water, and hydrothermally crystallized at 85°C for 38h, and the mother liquor was filtered out, washed with water, and dried to obtain product J11.

[0124] The product J11 prepared in comparative example 1 was first roasted at 900°C for 0.5 hours under 30% water vapor in a roasting furnace to obtain a roasting material with a burning loss of 0.8%. The roasting material was slowly added to the top of the reactor through a feeder. There was another silicon tetrachloride gas inlet at the top of the reactor. The proportion of silicon tetrachloride to the carrier gas was 30%. The roasting material and silicon tetrachloride reacted in the reactor in the same direction. The gas-solid phase reaction temperature was 400°C, the contact time with the gas was 60min, and the ratio of silicon tetrachloride to the roasting material was 0.4:1. The reacted gas was discharged through the gas outlet pipe by pumping and entered the recovery system. The recovery system was a 12% sodium hydroxide solution for acid-base neutralization. After the catalyst was collected by the collector at the bottom of the absorption tower, it was washed with 15 times water at 65°C for 1h and dried to obtain the catalyst C-11 with a Na2O content of 0.46%.

[0125] Comparative Example 2

[0126] Compared with Example 1, 20g of magnesium chloride was dissolved in 100mL of distilled water and aged at 80°C for 5min. 100g of the aged material, 800g of kaolin (calcined), 40g of sodium silicate solution, 160g of alkaline silica sol and deionized water were prepared into a mixed slurry with a solid content of 46%, and spray dried to obtain 600g of spray microspheres P12 with a particle size of 20 to 110μm. A part of the P12 spray soil ball was calcined at 980°C for 2.7h to obtain calcined microspheres G12, and another part was calcined at 650°C for 2.5h to obtain calcined microspheres B12, then 100g of G12 and 300g of B12 were mixed, sodium silicate, a directing agent, a sodium hydroxide solution and deionized water were added, and hydrothermal crystallization was carried out at 95°C for 30h, the mother liquor was filtered out, and the product J12 was obtained by washing and drying.

[0127] The product J12 prepared in comparative example 2 was roasted in a roasting furnace at 500°C and 100% water vapor for 2 hours to obtain a roasted material. The roasted material was reacted in the same direction with silicon tetrachloride gas in an inclined tubular furnace, the proportion of silicon tetrachloride to carrier gas was 100%, the reaction temperature was: 900°C, the contact time with gas was 0.1min, and the ratio of silicon tetrachloride to roasted material was 0.5:1. The gas after the reaction entered the recovery system, which was a 10% sodium hydroxide solution for acid-base neutralization. The catalyst was discharged from the other end of the reaction tube, and then washed with 19 times water at 85°C for 0.5h, and dried to obtain catalyst C-12 with a Na2O content of 0.45%.

[0128] Comparative Example 3

[0129] Compared with Example 7, 242g of alkaline silica sol solution was slowly added to 70g of magnesium chloride solution dissolved in 300mL of distilled water, mixed for 55 minutes, and a silicon-magnesium material was obtained. The final pH value was 11.5. The material was aged at 100°C for 90min, and then cerium nitrate was added, cerium nitrate (as cerium oxide) / silicon-magnesium material = 8.2% (mass ratio). 100g of the material after rare earth, 2500g of kaolin (calcined base), 50g of sodium silicate solution, 75g of aluminum sol, and deionized water were added to prepare a mixed slurry with a solid content of 36%, spray dried to obtain 1500g of spray microspheres P13 with a particle size of 20 to 110μm. A portion of P13 was calcined at 850°C for 2.3 h to obtain calcined microspheres G13, and the other portion was calcined at 680°C for 2.6 h to obtain calcined microspheres B13. Then, 750 g of G13 and 250 g of B13 were added to sodium silicate solution, a directing agent, a sodium hydroxide solution, and deionized water, and hydrothermally crystallized at 92°C for 32 h. The mother liquor was filtered out, and the product was washed with water and dried to obtain product J13.

[0130] The product J13 prepared in comparative example 3 was first roasted in a roasting furnace at 750°C and 60% water vapor for 0.5 hours, and then entered the reactor in the same direction with silicon tetrachloride, the proportion of silicon tetrachloride in the carrier gas was 30%, the roasting material and silicon tetrachloride reacted in the reactor in the same direction, the gas-solid phase reaction temperature was 400°C, the contact time with the gas was 60 minutes, and the ratio of silicon tetrachloride to the roasting material was 0.4:1. The gas after the reaction entered the recovery system, which was a 12% sodium hydroxide solution for acid-base neutralization. After the catalyst was collected, it was washed with 13 times water at 85°C for 2 hours and dried to obtain the catalyst C-13 with a Na2O content of 0.45%.

[0131] Comparative Example 4

[0132] Compared with Example 8, 90g of magnesium nitrate was dissolved in 300mL of distilled water, and the dissolved solution was slowly added to 948g of sodium silicate solution, mixed for 25 minutes, and a silicon-magnesium material was obtained, and the final pH value was 10.5. The material was aged at 93°C for 120min, and the aged material 120g, kaolin 750g (calcined base), sodium silicate solution 60g, aluminum sol 52.5g, and deionized water were prepared into a mixed slurry with a solid content of 42%, spray-dried, and 750g of spray microspheres P14 with a particle size of 20 to 110μm were obtained. P14 was calcined at 630°C for 2.1h to obtain calcined microspheres B14, and then 700g of B14 was added to sodium silicate solution, a directing agent, a sodium hydroxide solution, and deionized water, and hydrothermally crystallized at 94°C for 36h, and the mother liquor was filtered to remove, and the product J14 was obtained by washing and drying.

[0133] 450 g of the crystallized product J14 prepared in Comparative Example 4 was added to a stainless steel kettle under stirring, and ammonium chloride and deionized water were added, ammonium chloride / crystallized product=0.20, ammonium sulfate / crystallized product=0.30, and the mixture was exchanged at pH=3.0-3.5 and 90°C for 1.5 hours. The filtrate was filtered out, and the filter cake was washed with deionized water and dried to obtain an exchange material; the exchange material was roasted at 560°C and a water vapor introduction rate of 95% for 2 hours to obtain a roasted material; the roasted material was exchanged once with lanthanum chloride, and the exchange conditions were: lanthanum chloride / a roasted material=0.034, pH=3.5-4.2, temperature of 90°C, and time of 1 hour. The exchanged material was then roasted at 700°C for 1.5 hours to obtain a second roasted material. After acid exchange, the second roasted material was filtered, washed, and dried to obtain a catalyst C-14 with a Na2O content of 0.39%.

[0134] The crystallization conditions and results of Examples 1 to 10 and Comparative Examples 1 to 4 are shown in Table 1, and the test results of the pore structure of the crystallized product are shown in Table 2. The pore structure results in Table 2 show that the patented synthesis method can be used to prepare a crystallized product with a more developed pore structure. The addition of silicon-magnesium structural materials brings about changes in the structure of the microsphere precursor in the synthesis system, thereby improving the pore structure of the crystallized product. The pore structure and specific surface area of ​​the crystallized product prepared by directly aging after adding silicon and magnesium without aging with rare earth are not as good as those of the corresponding embodiments, indicating that aging rare earth with silicon and magnesium can form a better cross-linked structure, which is more conducive to the growth of in-situ molecular sieves and brings about a significant increase in specific surface area and pore volume. Compared with materials using only silicon or magnesium, the crystallized product prepared by this scheme has a richer pore structure. Figure 1 , Figure 2The results show that compared with Comparative Example 2, Example 1 uses the exchange of ammonia water and boric acid, so the catalyst has a richer medium and macroporous structure. There is no difference in the adsorption curve tested using naphthalene as the probe molecule; but when quinoline is used as the probe molecule, the adsorption curves of the two agents are significantly different because quinoline contains basic groups, indicating that the patented technology can bring more excellent acid distribution and activity accessibility to the catalyst, providing a guarantee for achieving efficient conversion of heavy oil and improving gasoline yield.

[0135] The results of sodium oxide and 17h micro-reaction activity of the catalyst in Table 3 show that the catalyst prepared by pore expansion material and isomorphous substitution process has a simpler process flow, lower sodium oxide content and better 17h micro-reaction activity.

[0136] Table 1 In-situ crystallization process conditions and preparation results

[0137]

[0138] Table 2 Pore structure characteristics of crystallized products

[0139]

[0140] Table 3 Catalyst sodium oxide content and micro-reaction activity

[0141]

[0142] Of course, the present invention may have many other embodiments. Without departing from the spirit and essence of the present invention, technicians familiar with the field may make various corresponding changes and deformations based on the present invention, but these corresponding changes and deformations should all fall within the scope of protection of the claims of the present invention.

Claims

1. A method for preparing a catalytic cracking catalyst without ammonium, characterized in that: The following steps are involved: (1) Mixing a magnesium source solution with a silicon source solution to obtain a silicon-magnesium material, and then adding a rare earth compound and aging to obtain a rare earth-containing silicon-magnesium material; (2) mixing the rare earth-containing silicon-magnesium material with kaolin, a dispersant and / or a reinforcing agent and deionized water, beating the mixture, spraying the mixture into microspheres, calcining the mixture, and then mixing the mixture with sodium silicate, a directing agent, an alkaline solution and water, and crystallizing the mixture to obtain a crystallized product; (3) exchanging and modifying the crystallized product with ammonia water and boric acid, and then calcining the product to obtain a primary calcined material; (4) The primary calcined material is contacted with silicon tetrachloride in a down-flowing bed isomorphous substitution reactor in a countercurrent manner to carry out an isomorphous substitution reaction to obtain a catalyst.

2. The method for preparing a catalytic cracking catalyst without ammonium according to claim 1, characterized in that: In step (1), the magnesium source solution and the silicon source solution are mixed, the pH is adjusted to 8-12, and then the rare earth compound is added.

3. The method for preparing a catalytic cracking catalyst without ammonium according to claim 1, characterized in that: The aging condition in step (1) is aging treatment at 80-120° C. for 5-300 minutes.

4. The method for preparing a catalytic cracking catalyst without ammonium according to claim 3, characterized in that: The aging conditions are aging treatment at 80~100°C for 30~200 minutes.

5. The method for preparing a catalytic cracking catalyst without ammonium according to claim 1, characterized in that: In step (1), the rare earth compound is calculated as rare earth oxide RE2O3, the mass ratio of RE2O3 to silicon-magnesium material is 1-10%, and the molar ratio of Si:Mg in the silicon-magnesium material is 0.1-15:

1.

6. The method for preparing a catalytic cracking catalyst without ammonium according to claim 1, characterized in that: In step (1), the silicon source is one or more of water glass, silica sol and white carbon black; the magnesium source is one or more of magnesium chloride, magnesium nitrate and magnesium sulfate.

7. The method for preparing a catalytic cracking catalyst without ammonium according to claim 1, characterized in that: In step (2), the mass ratio of the rare earth-containing silicon-magnesium material to kaolin is 0.1-20:100, the mass ratio of the dispersant to kaolin is 1-20:100, the mass ratio of the reinforcing agent to kaolin is 1-20:100, and the solid content of the slurry after mixing and beating is 30-50%.

8. The method for preparing a catalytic cracking catalyst without ammonium according to claim 7, characterized in that: In step (2), the mass ratio of the dispersant to kaolin is 1-15:100, and the mass ratio of the reinforcing agent to kaolin is 2-8:

100.

9. The method for preparing a catalytic cracking catalyst without ammonium according to claim 1, characterized in that: The particle size of the microspheres obtained by spraying in step (2) is 20-110 μm.

10. The method for preparing catalytic cracking catalyst by the ammonium-free method according to claim 1, characterized in that: In step (2), the calcination temperature is 600-1000° C., the calcination time is 1-3 h, and the crystallization conditions are 85-95° C. for 16-36 h.

11. The method for preparing a catalytic cracking catalyst without ammonium according to claim 1, characterized in that: The dispersant is sodium silicate and / or sodium pyrophosphate; the reinforcing agent is silica sol and / or aluminum sol.

12. The method for preparing catalytic cracking catalyst by the ammonium-free method according to claim 1, characterized in that: The kaolin in step (2) is soft kaolin and / or hard kaolin, with a median diameter of 1.5-3.0 μm, a crystal kaolinite content higher than 80%, iron oxide lower than 1.7%, and a sum of sodium oxide and potassium oxide lower than 0.5%.

13. The method for preparing catalytic cracking catalyst by the ammonium-free method according to claim 1, characterized in that: The concentration of ammonia water in step (3) is 1-25%.

14. The method for preparing catalytic cracking catalyst by the ammonium-free method according to claim 1, characterized in that: In step (3), the mass ratio of boron element to crystallized product is 0.01-0.50:

1.

15. The method for preparing catalytic cracking catalyst by the ammonium-free method according to claim 1, characterized in that: The process of step (3) is that the crystallized product is first treated with ammonia water at 20-60°C for 30-120 minutes, and the product exchanged with ammonia water is then exchanged with boric acid. The process conditions of the exchange are: pH 3-6, temperature 90-110°C.

16. The method for preparing catalytic cracking catalyst by the ammonium-free method according to claim 1, characterized in that: After calcination in step (3), the ignition reduction is within 3%, and a microspherical primary calcined material containing 5-60% of Y-type molecular sieve is obtained.

17. The method for preparing catalytic cracking catalyst by the ammonium-free method according to claim 1, characterized in that: In step (4), the mass ratio of silicon tetrachloride to the primary calcined material is 0.01-0.5:

1.

18. The method for preparing catalytic cracking catalyst by the ammonium-free method according to claim 1, characterized in that: Catalyst specific surface area 200 ~500 m 2 / g, pore volume 0.40~0.55mL / g.

19. The method for preparing catalytic cracking catalyst by the ammonium-free method according to claim 1, characterized in that: The roasting step in step (3) is carried out in a pretreatment furnace, which comprises a feeding section, a roasting section and a discharging section. The total length of the pretreatment furnace is 0.5 to 5 meters, the inner diameter is 0.01 to 1 meter, and the roasting temperature is 100 to 1000°C.

20. The method for preparing catalytic cracking catalyst by the ammonium-free process according to claim 19, characterized in that: The pretreatment furnace includes a heating system and a ventilation system. The heating system is arranged on the outer layer of the pretreatment furnace in the form of a furnace tile jacket, and the ventilation system is arranged on the inner wall of the pretreatment furnace. The ventilation system can input dry gas, nitrogen or water vapor into the pretreatment furnace.

21. The method for preparing catalytic cracking catalyst by the ammonium-free method according to claim 19, characterized in that: The angle α between the pretreatment furnace feeding section and the pretreatment furnace body is greater than 10° and less than 90°, and the angle β between the pretreatment furnace body and the horizontal position is greater than 10° and less than 90°.

22. The method for preparing catalytic cracking catalyst by the ammonium-free process according to claim 19, characterized in that: A shaft rotating device is provided on the top of the pretreatment furnace to control the rotation of the furnace body of the pretreatment furnace, and the rotation frequency is 10-80 Hz / min.

23. The method for preparing catalytic cracking catalyst by the ammonium-free method according to claim 1, characterized in that: The down-going bed isomorphous substitution reactor is divided into a buffer zone and a reaction zone from top to bottom, a catalyst inlet is provided at the top of the buffer zone, an atomizer connected to the catalyst inlet is provided at the upper part of the buffer zone, a nitrogen inlet carrying silicon tetrachloride is provided at the bottom of the reaction zone, a discharge port is provided at the upper part of the reaction zone, an inner diameter ratio of the buffer zone to the reaction zone is 1:1-4:1, and the heights of the buffer zone and the reaction zone are independently 0.2-1 meters.

24. The method for preparing a catalytic cracking catalyst by an ammonium-free process according to claim 23, characterized in that: The inner diameter ratio of the buffer zone to the reaction zone is 1:1 to 3:

1.

25. The method for preparing catalytic cracking catalyst by the ammonium-free process according to claim 23, characterized in that: The inner diameter ratio of the buffer zone to the reaction zone is 1:1-3:1; a heating jacket or a heating belt is arranged on the outer wall of the down-going bed isomorphous substitution reactor; and the cavity diameter of the reaction zone is 0.05-0.5 meters.

26. The method for preparing catalytic cracking catalyst by the ammonium-free process according to claim 23, characterized in that: The atomizer is made of stainless steel and contains a plurality of symmetrically distributed air holes. The diameter of the air holes is 80-200 μm. The gas pressure inside the atomizer is 0.1-6 MPa.

27. The method for preparing catalytic cracking catalyst by the ammonium-free process according to claim 1, characterized in that: In step (4), the isomorphous substitution reaction temperature is 200-900°C, the time for which the primary calcined material is in contact with silicon tetrachloride gas is 0.1-60 min, and nitrogen is used as a carrier gas to carry silicon tetrachloride into the reactor, with the proportion of silicon tetrachloride in the total carrier gas being 0.1-100%.

28. The method for preparing catalytic cracking catalyst by the ammonium-free method according to claim 1, characterized in that: In step (4), the isomorphous substitution reaction temperature is 300-600°C.